Preparation method and application of polyvinyl alcohol / sodium alginate / chitosan hydrogel damping package

Through the preparation of polyvinyl alcohol/sodium alginate/chitosan hydrogel, the problem of poor protection effect of existing packaging materials on soft fruits and environmental pollution is solved, and an environmentally friendly and efficient vibration-absorbing packaging material is provided, which significantly reduces Damage rates in fruit transportation.

CN118725347APending Publication Date: 2024-10-01NINGBO UNIV
View PDF 0 Cites 0 Cited by

Patent Information

Application Number
CN202410851771.5
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Filing Date
2024-06-28
Publication Date
2024-10-01

AI Technical Summary

Technical Problem

Existing food packaging has poor protection effect on soft fruits during logistics and transportation, and commonly used materials have environmental pollution problems, and there is a lack of environmentally friendly buffer packaging materials.

Method used

Adopt the preparation method of polyvinyl alcohol/sodium alginate/chitosan hydrogel, mix PVA and CS solutions by stirring, and add sodium alginate under appropriate pH conditions to form PVA/SA/CS hydrogel, and freeze it. Melt preparation to obtain vibration-damping packaging.

Benefits of technology

The prepared hydrogel has good biodegradability, moderate hardness and high gel strength, significantly reduces the vibration damage of fruits during transportation, reduces transportation losses, and shows excellent vibration reduction and protection effects during the logistics process.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN118725347A_ABST
    Figure CN118725347A_ABST
Patent Text Reader

Abstract

The invention discloses a preparation method and application of a polyvinyl alcohol / sodium alginate / chitosan hydrogel damping package, and is characterized in that the preparation method comprises the following steps: (1) mixing 5-15 wt% of PVA solution and 0.5-1.5 wt% of CS solution according to a volume ratio of (2-6): 1, and uniformly stirring and mixing at 400-800 rpm to obtain PVA / CS mixed solution; and (2) adding triethanolamine into the PVA / CS mixed solution while stirring until the pH value is adjusted to 7-7.3, adding sodium alginate powder until the concentration is 2-2.5 wt%, uniformly stirring to obtain a PVA / SA / CS hydrogel precursor stock solution, pouring the PVA / SA / CS hydrogel precursor stock solution into a mold, and freezing and thawing to obtain the PVA / SA / CS hydrogel vibration reduction package. A good vibration reduction protection effect is achieved on peach fruits, and the transportation loss of the peach fruits is reduced.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The invention belongs to the technical field of food packaging and transportation, and particularly relates to a preparation method and application of a polyvinyl alcohol / sodium alginate / chitosan hydrogel vibration-damping package. Background Art

[0002] Many fruits with soft texture, thin skin and thin wax are susceptible to mechanical damage such as impact, compression, abrasion and puncture during logistics transportation. Fruit damage will cause the wound to be exposed to fungal infection, resulting in a decline in fruit quality, threatening food safety and causing economic losses. In modern logistics, cushioning materials are often used to reduce the damage to fruits caused by vibration during transportation. At present, the more commonly used vibration-reducing packaging methods include foam packaging, corrugated paper packaging, pearl cotton packaging and inflatable bag packaging. Among them, corrugated paper packaging has the worst protection effect and the highest loss rate during logistics. The other three types of packaging are made of plastic materials and produce white pollution after use, polluting the environment and lacking certain environmental protection. Therefore, the development of a green and environmentally friendly cushioning packaging material has become a current research hotspot. Hydrogels are soft and elastic, and have a good vibration-reducing protective effect. However, due to the different materials, the plasticity and water loss of hydrogels are also different, which limits the use of hydrogels in actual transportation. Therefore, it is of great significance to find suitable materials to prepare hydrogels that meet these limitations.

[0003] Polyvinyl alcohol (PVA) is a new type of water-soluble environmentally friendly material. It has been successfully applied in composite hydrogels in recent years. It can form chemically cross-linked PVA hydrogels through multifunctional aldehyde molecules such as glutaraldehyde and glyoxal and radiation cross-linking. However, the chemical cross-linking method may leave residual initiators or cross-linkers, resulting in reduced biocompatibility of the hydrogel. There are certain risks in using it in vibration-damping packaging materials that are in direct contact with fruits and vegetables. Sodium alginate (SA) is a natural polymer material extracted from brown algae kelp. It has excellent biocompatibility, non-toxicity, biodegradability and abundant storage capacity. Chitosan (CS) is the only natural cationic polysaccharide in nature. It contains free amino groups, has a wide range of sources, and has excellent biocompatibility, biodegradability, antibacterial properties, and film-forming properties. At present, there are no relevant research reports on the preparation method of polyvinyl alcohol / sodium alginate / chitosan freeze-thaw hydrogels and their application in food transportation at home and abroad. Summary of the invention

[0004] The technical problem to be solved by the present invention is to provide a preparation method and application of a polyvinyl alcohol / sodium alginate / chitosan hydrogel which can reduce vibration damage to fruits and vegetables during transportation, and has a good vibration reduction and protection effect on peach fruits during logistics transportation, thereby reducing transportation losses.

[0005] The technical solution adopted by the present invention to solve the above technical problems is: a method for preparing a polyvinyl alcohol / sodium alginate / chitosan hydrogel vibration-damping package, comprising the following steps:

[0006] (1) Preparation of polyvinyl alcohol / chitosan (PVA / CS) hydrogel solution

[0007] Mixing 5-15 wt % PVA solution and 0.5-1.5 wt % CS solution in a volume ratio of (2-6):1, stirring and mixing at 400-800 rpm to obtain a PVA / CS mixed solution;

[0008] (2) Preparation of polyvinyl alcohol / sodium alginate / chitosan (PVA / SA / CS) hydrogel

[0009] The PVA / CS mixed solution prepared in step (1) is added with triethanolamine while stirring until the pH is adjusted to 7-7.3, and sodium alginate (SA) powder is added to make its concentration 2-2.5wt%, and stirred evenly to obtain a PVA / SA / CS hydrogel precursor solution, which is poured into a mold and freeze-thawed to obtain a PVA / SA / CS hydrogel vibration-damping package.

[0010] Preferably, the method comprises the following steps:

[0011] (1) Preparation of polyvinyl alcohol / chitosan (PVA / CS) hydrogel solution

[0012] 10 wt % PVA solution and 1 wt % CS solution were mixed at a volume ratio of 4:1, and stirred at 600 rpm for 15 min to obtain a PVA / CS mixed solution;

[0013] (2) Preparation of polyvinyl alcohol / sodium alginate / chitosan (PVA / SA / CS) hydrogel

[0014] The PVA / CS mixed solution prepared in step (1) was added with triethanolamine while stirring until the pH value was adjusted to 7-7.3, and sodium alginate (SA) powder was added to make its concentration 2.25wt%, and stirred for 30min to obtain the PVA / SA / CS hydrogel precursor solution, which was poured into a mold and frozen at -20°C for 12h. After thawing, the PVA / SA / CS hydrogel vibration-damping package was obtained.

[0015] Furthermore, the preparation method of the PVA solution is as follows: weigh polyvinyl alcohol particles and pour them into a beaker, heat and stir them at 90°C and 425rpm with a magnetic stirrer until the polyvinyl alcohol is completely dissolved, and then stir at 425rpm for 15-30min to obtain a PVA solution with a mass concentration of 10%.

[0016] Furthermore, the preparation method of the CS solution is as follows: weigh chitosan powder, pour it into a beaker filled with 1wt% glacial acetic acid aqueous solution, stir it at 800rpm with a magnetic stirrer at room temperature for 20-40min until the chitosan powder is completely dissolved to obtain a 1wt% CS solution.

[0017] The polyvinyl alcohol / sodium alginate / chitosan hydrogel vibration-damping packaging prepared by the preparation method is used in the logistics and transportation process of peach fruits.

[0018] Compared with the prior art, the advantages of the present invention are:

[0019] 1. The preparation process of the PVA / SA / CS hydrogel prepared by the present invention is simple, and the raw materials have good biodegradability.

[0020] 2. The present invention utilizes the property of polyvinyl alcohol that the gel is not deformed during molding, and prepares the PVA / SA / CS hydrogel into a vibration-damping package of a desired shape, and the water loss rate of the hydrogel is also low.

[0021] 3. Compared with PVA hydrogel, PVA / SA hydrogel and PVA / CS hydrogel, PVA / SA / CS hydrogel has a more moderate hardness and excellent gel strength.

[0022] 4. The swelling rate of PVA hydrogel is low, which makes PVA hydrogel mainly lose water at a fast rate under room temperature. The swelling rate of the PVA / SA / CS hydrogel prepared after improvement is greatly improved, and the water absorption is also increased. At a higher swelling rate, PVA / SA / CS hydrogel will not be excessively deformed due to water loss, thereby improving the defect of hydrogel water loss and deformation.

[0023] 5. The prepared PVA / SA / CS hydrogel was used in the logistics transportation of peach fruits, which proved that its hydrogel vibration-damping packaging had a good vibration-damping protection effect on the fruits during logistics transportation, reducing the logistics loss rate of the fruits. BRIEF DESCRIPTION OF THE DRAWINGS

[0024] Figure 1 Figure 2 shows the PVA / SA / CS hydrogel sample, where a is the front view and b is the top view.

[0025] Figure 2 The scanning electron micrographs of PVA / SA / CS hydrogels, a is the surface × 60 and b is the surface × 200, c is the cross section × 60 and d is the cross section × 200;

[0026] Figure 3 The water loss rate change diagram of PVA / SA / CS hydrogel, PVA hydrogel, PVA / SA hydrogel and PVA / CS hydrogel;

[0027] Figure 4 The hardness diagrams of PVA / SA / CS hydrogel, PVA hydrogel, PVA / SA hydrogel and PVA / CS hydrogel;

[0028] Figure 5 The gel strength diagrams of PVA / SA / CS hydrogel, PVA hydrogel, PVA / SA hydrogel and PVA / CS hydrogel;

[0029] Figure 6 FTIR images of PVA, SA, CS and PVA / SA / CS hydrogels;

[0030] Figure 7 This is a graph showing the ethylene release of peach fruits in different packages after simulated logistics vibration;

[0031] Figure 8 This is a graph showing the ethylene release of peach fruits in different packages after logistics transportation;

[0032] Fig. 9 These are pictures of peach fruits packed in EPE after logistics transportation. a was taken 2 days after logistics transportation, and b was taken after 2 days of logistics transportation + 2 days of storage.

[0033] Fig.10 These are pictures of peach fruit surface damage after logistics transportation in PVA / SA / CS hydrogel vibration-damping packaging. a was taken 2 days after logistics transportation, and b was taken 2 days after logistics transportation + 2 days of storage. DETAILED DESCRIPTION

[0034] The present invention is further described in detail below with reference to the accompanying drawings.

[0035] 1. Implementation

[0036] Example 1

[0037] A method for preparing a polyvinyl alcohol / sodium alginate / chitosan hydrogel vibration-damping package comprises the following steps:

[0038] 1. Preparation of polyvinyl alcohol / chitosan (PVA / CS) hydrogel solution

[0039] Weigh 50 g of polyvinyl alcohol (PVA) particles and pour them into a 500 mL beaker. Heat and stir the mixture at 90 °C and 425 rpm for 40 min with a magnetic stirrer until the polyvinyl alcohol is completely dissolved. Stir the mixture at room temperature and 425 rpm for 20 min to obtain a PVA solution with a mass concentration of 10%.

[0040] Weigh 1 g of chitosan powder and pour it into a beaker containing 100 mL of 1 wt% glacial acetic acid aqueous solution. Stir with a magnetic stirrer at 800 rpm for 30 min at room temperature until the chitosan powder is completely dissolved to obtain a 1 wt% CS solution.

[0041] The PVA solution and the CS solution were mixed at a volume ratio of 4:1 and stirred at 600 rpm for 15 min to make the two mixed evenly to obtain a PVA / CS mixed solution for subsequent experiments;

[0042] 2. Preparation of polyvinyl alcohol / sodium alginate / chitosan (PVA / SA / CS) hydrogel

[0043] The PVA / CS mixed solution prepared in step 1 was added with triethanolamine while stirring until the pH was adjusted to 7.2, and sodium alginate (SA) powder was added to make its concentration 2.25wt%, and stirred with a mechanical stirrer at room temperature and 1500rpm for 30min to obtain a PVA / SA / CS hydrogel precursor solution. The PVA / SA / CS hydrogel precursor solution was poured into a mold, frozen at -20°C for 12h, and the PVA / SA / CS hydrogel vibration-damping package was obtained after thawing. Figure 1 This is a sample picture of PVA / SA / CS hydrogel. Figure 1 a is the front view of the packaging. Figure 1 b is a top view of the packaging.

[0044] Figure 2 is the scanning electron microscopy image of PVA / SA / CS hydrogel, a is the surface, c and d are cross sections, Figure 2 As can be seen from a and b, the surface of the PVA / SA / CS hydrogel has a dense strip-shaped three-dimensional polymer network, with many tiny holes of different sizes inside; and from the cross-section of the PVA / SA / CS hydrogel Figure 2 Observations in c and d revealed that there are many complex and irregular channels inside the hydrogel, as well as many tiny holes. These tiny holes and channels ensure the high water content and swelling properties of the hydrogel, and have better anti-seismic and cushioning properties.

[0045] Example 2

[0046] The method is the same as the above-mentioned Example 1, except that: in step (1), 5 wt% PVA solution and 0.5 wt% CS solution are mixed in a volume ratio of 2:1, and the mixture is stirred at 400 rpm to obtain a PVA / CS mixed solution; in step (2), triethanolamine is added to the PVA / CS mixed solution while stirring until the pH is adjusted to 7, and then sodium alginate powder is added to make its concentration 2 wt%.

[0047] Example 3

[0048] The method is the same as the above-mentioned Example 1, except that: in step (1), 15 wt% PVA solution and 1.5 wt% CS solution are mixed in a volume ratio of 6:1, and the mixture is stirred at 800 rpm to obtain a PVA / CS mixed solution; in step (2), triethanolamine is added to the PVA / CS mixed solution while stirring until the pH value is adjusted to 7.3, and then sodium alginate powder is added to the mixed solution to obtain a concentration of 2.5 wt%.

[0049] 2. Comparative Test

[0050] 1. Comparison of water loss rate between the product and PVA hydrogel, PVA / SA hydrogel and PVA / CS hydrogel

[0051] Preparation methods of PVA hydrogel, PVA / SA hydrogel and PVA / CS hydrogel:

[0052] The PVA hydrogel is prepared by dissolving PVA in deionized water to obtain a PVA solution with a mass concentration of 10%wt, and then subjecting the solution to freeze-thaw cycles to obtain the final product. The PVA / SA hydrogel is prepared by adding sodium alginate with a final concentration of 2.25%wt to a PVA solution with a mass concentration of 10%wt, stirring the mixture evenly, and then subjecting the mixture to freeze-thaw cycles to obtain the final product. The PVA / CS hydrogel is prepared by mixing a 10wt% PVA solution with a 1wt% CS solution in a volume ratio of 4:1, adding triethanolamine while stirring, adjusting the pH to 7.3, and then subjecting the mixture to freeze-thaw cycles to obtain the final product.

[0053] The product and PVA hydrogel, PVA / SA hydrogel and PVA / CS hydrogel were prepared using 12-well cell culture plates as molds to obtain cylindrical hydrogel samples of the same shape and size. First, the samples were placed in distilled water to absorb water to a constant weight, and the initial weight was recorded. Then, they were placed in food storage boxes to simulate the water loss of the hydrogel during logistics. The weight of the hydrogel was recorded every 24 hours, and its water loss rate was calculated. This was repeated three times.

[0054] The water loss rate of hydrogel is calculated according to the following formula:

[0055]

[0056] Depend on Figure 3It can be seen that the water loss rate of PVA / SA / CS hydrogel at 48h and 72h was the lowest at 36.34% and 47.94%, the water loss rates of PVA hydrogel, PVA / SA hydrogel and PVA / CS hydrogel at 48h and 72h were 37.65%, 37.14%, 38.39% and 48.31%, 50.99%, 52.15%, respectively, and the water loss rate of PVA / SA / CS hydrogel at 24h was 20.77%, which was only slightly higher than the water loss rate of PVA / SA hydrogel at 24h, which was 20.03%. This shows that PVA / SA / CS hydrogel is superior to PVA hydrogel, PVA / SA hydrogel and PVA / CS hydrogel in water loss rate.

[0057] 2. Comparison of swelling rate and water content between the product and PVA hydrogel, PVA / SA hydrogel and PVA / CS hydrogel

[0058] The swelling rate was determined as follows: the hydrogel samples were dried in an oven at 50 °C until they reached a constant weight, and the weight of the dried samples was recorded as W dry The dried samples were immersed in distilled water at room temperature. At specified time intervals, the samples were taken out of the water and the surface moisture was wiped with filter paper. Their weight was weighed until the hydrogel reached a constant weight, and the sample weight at this time was recorded as W. wet The swelling ratio (SR) of a sample is the weight ratio of the swollen sample to the dried sample.

[0059]

[0060] Where SR is the swelling ratio of the hydrogel, W wet is the maximum weight of the P hydrogel after water absorption and swelling, W dry is the weight of the hydrogel after drying.

[0061] The water content was determined as follows: the hydrogel was immersed in distilled water until constant weight was obtained and the initial weight was recorded as W. h The hydrogel was placed in an oven at 50°C and dried until it reached a constant weight. The weight of the hydrogel was recorded as W. d . Use W h and W d The water content W of each hydrogel sample was calculated by c .

[0062]

[0063] Where W c is the water content of the hydrogel, W h is the initial weight of the hydrogel, W d is the weight of the hydrogel after drying.

[0064] Table 1 Water content and swelling rate of different hydrogels

[0065]

[0066] As can be seen from Table 1, experiments show that the water content of pure PVA hydrogel is 85.32%, and the swelling rate is 25.79%; adding only chitosan to the PVA hydrogel will increase the water content of the hydrogel to 88.16%, and the swelling rate will slightly increase to 46.91; adding only sodium alginate to the PVA hydrogel will reduce the water content of the hydrogel to 83.82%, and the swelling rate will be greatly increased to 260.25%. After adding chitosan and sodium alginate to the PVA hydrogel, a hydrogel with a water content of 86.46% and a swelling rate of 264.08% with better properties is obtained.

[0067] 3. Comparison of hardness and gel strength between the product and PVA hydrogel, PVA / SA hydrogel and PVA / CS hydrogel

[0068] The sample preparation method in comparative experiment 2 was the same, and the hardness and gel strength of the hydrogel were determined using a texture analyzer. The hardness determination method was as follows: a P / 0.5 probe was selected, and in TPA mode, the speed before, during and after the test was 5 mm / s, the trigger force was 1 N, the test time was 5 s, and the compression percentage was 75%.

[0069] The gel strength determination method is as follows: select a P / 0.5 probe, in the gel strength determination mode, the speed before and during the test is 1 mm / s, the speed after the test is 3 mm / s, the trigger force is 5 g, and the distance is 10 mm.

[0070] Hardness reflects the ability of the hydrogel to resist the pressure of hard objects on its surface. Gel strength is a comprehensive indicator of the stability and elasticity of the hydrogel.

[0071] Depend on Figure 4 and Figure 5 It can be seen that the hardness of the pure PVA hydrogel is 32.576N and the gel strength is 147.196g*mm; after adding only sodium alginate, the hardness of the hydrogel increases to 53.19N and the gel strength increases to 295.416g*mm; after adding only chitosan, the hardness of the hydrogel decreases to 28.782N and the gel strength decreases to 116.374g*mm; after adding chitosan and sodium alginate to the PVA hydrogel, the hardness of the hydrogel becomes 38.796N and the gel strength increases to 172.967g*mm. After adding only sodium alginate, the hardness of the hydrogel is too high, but the stability of the gel is good, while after adding only chitosan, the hardness of the hydrogel decreases and the stability of the gel becomes worse. After adding sodium alginate and chitosan together, a PVA / SA / CS hydrogel with moderate hardness and good stability is obtained.

[0072] 4. PVA / SA / CS hydrogel FTIR experiment

[0073] according to Figure 6 The FTIR results of each substance in the sample showed that the FTIR spectrum of PVA showed that at 1048 cm -1 The stretching vibration absorption peak of CO skeleton appears near 2922cm -1 The stretching vibration absorption peak of the CH bond appears near 1076cm -1 The CC skeleton stretching vibration absorption peak appears nearby at 1595 cm -1 The bending vibration of NH (amide II) occurs at 1650cm -1 The absorption peak near is the stretching vibration absorption peak of the C=O group, 2872 cm -1 The absorption peak at 3445cm is caused by the stretching vibration of the CH bond. -1 The broad peaks near the OH bond and the NH bond are overlapped by the stretching vibration absorption peaks. In the FTIR spectrum of SA, 1417 and 1609 cm -1 The symmetric and asymmetric stretching vibrations of -COO- are shown in Table 1. By comparing the spectra of PVA, CS, SA and PVA / SA / CS hydrogels, the PVA / SA / CS has a peak at 1076 cm -1 The absorption peak near is the CC skeleton stretching vibration absorption peak of CS, at 1609cm -1 The nearby absorption peak is the stretching vibration of the -COO- group of SA, which appears at 2922 cm -1 The nearby peak is the stretching vibration of the C-H bond of PVA, 3353 cm -1 The FTIR spectrum of PVA / SA / CS hydrogel contains the characteristic peaks of PVA, CS, and SA, and no new characteristic peaks are generated, indicating that PVA / SA / CS hydrogel is formed by the combination of three substances through physical action. -1 The stretching vibration peaks of the OH bond and the NH bond at α-H bond are significantly enhanced, which may be caused by the hydrogen bond interaction between PVA and CS and SA, further indicating that the three substances are physically combined.

[0074] 3. Application Examples

[0075] PVA / SA / CS hydrogel was prepared into vibration-damping packaging and applied to peach fruit logistics to verify its protective effect

[0076] 1. Simulated logistics random vibration test

[0077] Random vibration test standard (same as the second level of random vibration spectrum for truck road transport in ASTM D 4169-16 Standard Practice for Performance Testing of Containers and Systems), the spectrum comparison table is as follows Table 2;

[0078] Table 2 Spectrum comparison table

[0079]

[0080] After determining the vibration parameters, according to I AD Value Selection I AD The commercially mature peach fruits with a value of >0.8 were divided into three groups: a non-vibration group, an EPE pearl cotton packaging vibration group, and a PVA / SA / CS hydrogel vibration group. The vibration groups were all packaged in the same way and transported to the laboratory in a pre-cooled state. The peach fruits were then taken out and placed at room temperature for 30 minutes, and then placed on a vibration platform for simulated transportation random vibration. The sweep frequency method was used, and the input parameters were an acceleration of 0.52 grms and vibration for 90 minutes. There were 8 peach fruits in each group, and 4 peach fruits were in one package. The vibration damage of the fruit was observed and recorded, and its ethylene release was measured. Since peach fruit is a respiratory climacteric fruit, after the fruit is damaged by vibration, the respiratory metabolism of the tissue in the injured part will be enhanced, resulting in an increase in ethylene release. Therefore, the ethylene release of peach fruit can reflect the damage of peach fruit.

[0081] Depend on Figure 7 It can be seen that the ethylene release of commercially mature peach fruits after simulated logistics vibration was 45.878 mg kg at 24 h and 48 h respectively. -1 ·h -1 , 50.285mg·kg -1 ·h -1 The ethylene release of the hydrogel group at 24h and 48h was 50.27mg·kg -1 ·h -1 , 53.275mg·kg -1 ·h -1 The ethylene release of the EPE pearl cotton group at 24h and 48h was 56.318mg·kg -1 ·h -1 、62.645mg·kg -1 ·h -1 , indicating that at 24h and 48h after vibration, the ethylene release of EPE pearl cotton was higher than that of the hydrogel group and the non-vibration group, and the ethylene release of the hydrogel group was only slightly higher than that of the non-vibration group. The use of PVA / SA / CS hydrogel vibration-damping packaging in simulated vibration has a good protective effect on peach fruits.

[0082] 2. Logistics test

[0083] Commercially ripe peach fruits were selected and placed in PVA / SA / CS hydrogel and EPE pearl cotton packaging respectively, and divided into two groups. The two groups were sent out at the same time by a courier company. All express deliveries were repackaged according to fresh food standards and transported by road. After 2 days of express transportation, the anti-injury effect of the two experimental groups was studied and determined by the same simulated vibration test as above.

[0084] Depend on Figure 8 It can be seen that after 2 days of logistics transportation, the ethylene release of the EPE group was 82.237 mg kg -1 ·h -1 , while the ethylene release of the hydrogel group was only 34.803 mg·kg -1 ·h -1 , which shows that hydrogel packaging has a better protective effect on peach fruits during the logistics process.

[0085] observe Fig. 9 and Fig.10 It is known that after logistics transportation, the top, bottom and protruding parts of the peach fruits packaged in EPE packaging have certain mechanical damage, resulting in browning of the skin and flesh, while the fruit surface of the fruit packaged in PVA / SA / CS hydrogel packaging does not show obvious browning caused by mechanical damage after logistics transportation. This can intuitively illustrate that the protection effect of PVA / SA / CS hydrogel packaging on peach fruits during the logistics process is better than that of traditional EPE packaging.

[0086] The above description is not intended to limit the present invention, and the present invention is not limited to the above examples. Any changes, modifications, additions or substitutions made by a person skilled in the art within the spirit and scope of the present invention shall also fall within the protection scope of the present invention.

Claims

1. A method for preparing a polyvinyl alcohol / sodium alginate / chitosan hydrogel vibration damping package, Features The following steps are involved: (1) Preparation of polyvinyl alcohol / chitosan hydrogel solution Mixing 5-15wt% PVA solution and 0.5-1.5wt% CS solution in a volume ratio of (2-6):1, stirring and mixing at 400-800rpm to obtain a PVA / CS mixed solution; (2) Preparation of polyvinyl alcohol / sodium alginate / chitosan hydrogel The PVA / CS mixed solution prepared in step (1) is added with triethanolamine while stirring until the pH is adjusted to 7-7.3, and sodium alginate powder is added to make its concentration 2-2.5wt%, and stirred evenly to obtain a PVA / SA / CS hydrogel precursor stock solution, which is poured into a mold and freeze-thawed to obtain a PVA / SA / CS hydrogel vibration-damping package.

2. A method for preparing a polyvinyl alcohol / sodium alginate / chitosan hydrogel vibration damping package according to claim 1, Features The following steps are involved: (1) Preparation of polyvinyl alcohol / chitosan hydrogel solution 10 wt % PVA solution and 1 wt % CS solution were mixed at a volume ratio of 4:1, and stirred at 600 rpm for 15 min to obtain a PVA / CS mixed solution; (2) Preparation of polyvinyl alcohol / sodium alginate / chitosan hydrogel The PVA / CS mixed solution prepared in step (1) was added with triethanolamine while stirring until the pH value was adjusted to 7-7.3, and sodium alginate powder was added to make its concentration 2.25wt%, and stirred for 30min to obtain the PVA / SA / CS hydrogel precursor solution, which was poured into a mold and frozen at -20°C for 12h. After thawing, the PVA / SA / CS hydrogel vibration-damping package was obtained.

3. A method for preparing a polyvinyl alcohol / sodium alginate / chitosan hydrogel vibration damping package according to claim 2, Features The preparation method of the PVA solution is as follows: weigh polyvinyl alcohol particles and pour them into a beaker, heat and stir them at 90°C and 425rpm with a magnetic stirrer until the polyvinyl alcohol is completely dissolved, and then stir at 425rpm for 15-30min to obtain a PVA solution with a mass concentration of 10%.

4. A method for preparing a polyvinyl alcohol / sodium alginate / chitosan hydrogel vibration damping package according to claim 2, Features The preparation method of the CS solution is as follows: weigh chitosan powder, pour it into a beaker filled with 1wt% glacial acetic acid aqueous solution, stir it at 800rpm with a magnetic stirrer at room temperature for 20-40min until the chitosan powder is completely dissolved to obtain a 1wt% CS solution.

5. Use of the polyvinyl alcohol / sodium alginate / chitosan hydrogel vibration-damping packaging prepared by the preparation method according to any one of claims 1 to 4 in the logistics and transportation process of peach fruits.