Polymer composition for cable material
By using liquid antioxidants and 1,2,4-triethylcyclohexane in cable materials, the problems of surface residue and degassing time of cross-linked polyethylene cable materials are solved, achieving more stable electrical performance and Efficient degassing process.
Patent Information
- Application Number
- CN202410962708.9
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Filing Date
- 2024-07-18
- Publication Date
- 2024-10-01
AI Technical Summary
It is difficult to effectively control the surface residual amount of cross-linked polyethylene in existing cable materials and reduce the degassing time after cable formation, which affects the stability of electrical performance.
Liquid hindered phenol antioxidant and non-polar additive 1,2,4-triethylcyclohexane are used, mixed through a reciprocating single-screw extruder and post-absorption cross-linked in a drum to reduce antioxidant The amount of agent and cross-linking agent used can improve the electrical performance stability and degassing efficiency.
The amount of surface residue is significantly reduced, the stability of electrical properties and degassing efficiency are improved, while the electrical properties, mechanical properties and thermal extension properties of the material are maintained.
Smart Images

Figure BDA0004950755360000061
Abstract
Description
Technical Field
[0001] The invention relates to the field of high-voltage insulating materials, and in particular to a polymer composition for cable materials and a preparation method thereof. Background Art
[0002] At present, with the vigorous construction and development of infrastructure, the power network is also in a stage of rapid development. Renewable energy such as wind energy, solar energy and tidal energy are increasingly used, which also requires higher long-distance and large-capacity power transmission technology. Cross-linked polyethylene is the current mainstream polymer insulation material. It has excellent electrical properties such as high breakdown strength and low dielectric loss. At the same time, its thermal and mechanical properties are also relatively excellent. It has gradually replaced traditional impregnated paper insulation and self-contained oil-filled insulation. The control of the surface residue of cross-linked polyethylene particles and the reduction of the degassing time after cabling are the focus of researchers. Some existing methods are to reduce the precipitation of additives by adding a certain amount of polar substances, but this is very unfavorable for the stability of electrical properties during cabling operation. Summary of the invention
[0003] In view of the above problems existing in the prior art, the specific technical solutions adopted by the present invention are as follows:
[0004] In a first aspect, the present invention provides a polymer composition for cable materials.
[0005] In a particular embodiment, the polymer composition comprises:
[0006] (1) polyethylene, 92.0-99.9 parts, preferably 95.0-99.9 parts, for example 92, 95, 98, 99 parts;
[0007] (2) Liquid hindered phenol antioxidant 1315, 0.01-1.0 part, for example 0.01, 0.05, 0.1, 0.2,
[0008] 0.3, 0.4, 0.5, 0.6, 0.7, 0.8, 0.9, 1 part; preferably 0.025-0.5 part, most preferably 0.05-0.3 part.
[0009] The polyethylene is a low-density polyethylene commonly used in the cable material industry, preferably with a melt index of 1.6-2.4 g / min (190°C, 2.16 kg) and a density of 0.920-0.924 g / cm 3 .
[0010] In a specific embodiment, the polymer composition of the present invention further comprises a crosslinking agent, wherein the crosslinking agent is selected from one or more of tert-butyl perbenzoate, dibenzoyl peroxide, dicumyl peroxide, and tert-butyl peroxide isopropylbenzene, preferably dicumyl peroxide;
[0011] The amount of the crosslinking agent added is 0.25-3 parts, for example 0.25, 0.5, 0.8, 1, 1.2, 1.5, 1.8, 2, 2.3, 2.5, 3 parts; preferably 0.5-2.5 parts, most preferably 0.5-2 parts.
[0012] In another specific embodiment, the polymer composition of the present invention further comprises an auxiliary agent 1,2,4-triethylcyclohexane.
[0013] Preferably, the amount of 1,2,4-triethylcyclohexane added is 0.05-3 parts, for example 0.05, 0.08, 0.1, 0.12, 0.15, 0.2, 0.3, 0.4, 0.5, 0.6, 0.7, 0.8, 0.9, 1, 1.5, 1.8, 2, 2.5, 3 parts; preferably 0.1-2 parts, more preferably 0.2-1 parts; the addition of the auxiliary agent has a significant effect on reducing the amount of crosslinking agent added.
[0014] The second aspect of the present invention provides a method for preparing the above-mentioned polymer composition for cable materials, wherein the antioxidant and other optional additives are added to polyethylene, firstly mixed and granulated by a reciprocating single-screw extruder, and the obtained particles are post-absorption cross-linked in a rotating drum to obtain the polymer composition for cable materials.
[0015] Preferably, the mixing temperature is 110-190°C, preferably 120-180°C; the post-absorption temperature is 40-100°C, preferably 50-80°C; and the post-absorption time is 6-48h, preferably 8-24h.
[0016] The third aspect of the present invention provides the use of the above polymer composition in cross-linked polyethylene high-voltage insulation composite materials, such as wires and cables.
[0017] Compared with the prior art, the present invention has the following beneficial effects:
[0018] By replacing traditional antioxidants with liquid antioxidants, not only the amount of antioxidants used is reduced, but the amount of surface residues can also be significantly reduced. Compared with the method of reducing the precipitation of additives by adding a certain amount of polar substances, the stability of electrical properties during the cabling operation can be effectively improved; in addition, by adding non-polar additives that assist in cross-linking, the amount of cross-linking agent added can be reduced without affecting the electrical properties of the material, which will greatly improve the degassing efficiency after cabling. DETAILED DESCRIPTION
[0019] The present invention is further described below in conjunction with embodiments, but the protection scope of the present invention is not limited to the embodiments, but also includes any other known changes within the scope of the claims of the present invention.
[0020] Main raw material sources of embodiments:
[0021] Polyethylene: commercially available LDPE, BASF-YPC 2220H;
[0022] Cross-linking agent: dicumyl peroxide DCP, Arkema, purity 99.0%;
[0023] Cross-linking agent: tert-butyl peroxide isopropylbenzene, Lanzhou Additive Factory, purity 90.0%;
[0024] Antioxidant: Antioxidant 300, Extremely Easy Company, purity 99.0%;
[0025] Antioxidant: Antioxidant 1315, SI Group, purity 99.0%;
[0026] Auxiliary agent: 1,2,4-triethylcyclohexane, Qiyuan Chemical Co., Ltd., purity 99.0%.
[0027] Other materials, unless otherwise specified, are common raw materials purchased from the market.
[0028] The blended materials prepared in the following examples were tested for anti-aging properties, thermal elongation properties, mechanical properties, electrical properties, and anti-scorch properties.
[0029] Mechanical properties: A tensile machine (INSTRON 5966) was used to test the mechanical properties of the samples. The sample preparation method was the molding method. The specific test conditions were in accordance with the standard GB / T1040.2.
[0030] Aging performance: Aging was carried out at 135°C for 168h, in accordance with GB / T 2951.12.
[0031] Anti-scorch performance: tested by rotorless rheometer (Alpha, MDR), the test temperature is 160°C, the oscillation angle is 0.5°, and the result is expressed by the scorch time TS1.
[0032] Thermal elongation performance: The test is carried out by combined equipment in an oven at a test temperature of 200°C and a test time of 15 minutes.
[0033] Conductivity: Tested with a high resistance meter (Keithley), and the specific test standard is in accordance with GB / T 1410.
[0034] Breakdown strength: The breakdown strength tester of Hafele Company is used, and the specific test standard is in accordance with GB / T1408.1.
[0035] Surface residue: alcohol washing measurement method is adopted, which is carried out in accordance with Q / GDW 11883.1-2018.
[0036] Example 1
[0037] Preparation of polymer composition:
[0038] 98.85 parts of base material LDPE, 0.15 parts of antioxidant 1315, and 1 part of 1,2,4-triethylcyclohexane were accurately weighed, and the above composition was mixed and extruded in a reciprocating single screw extruder at an extrusion temperature of 120-150-180° C. After granulation, it was put into a rotary drum for post-absorption, and 1 part of crosslinking agent DCP was added. The post-absorption temperature was 80° C. and the time was 16 hours to obtain a polymer composition sample.
[0039] The prepared samples were subjected to relevant performance tests.
[0040] Example 2
[0041] Preparation of polymer composition:
[0042] Accurately weigh 99.85 parts of base material LDPE and 0.15 parts of antioxidant 1315, and extrude and mix the above composition in a reciprocating single screw extruder at an extrusion temperature of 120-150-180° C. After granulation, enter the drum for post-absorption, add 1.6 parts of crosslinking agent DCP, the post-absorption temperature is 80° C., and the time is 16 hours to obtain a polymer composition sample.
[0043] The prepared samples were subjected to relevant performance tests.
[0044] Example 3
[0045] Preparation of polymer composition:
[0046] Accurately weigh 99.4 parts of base material LDPE, 0.10 parts of antioxidant 1315, and 0.5 parts of 1,2,4-triethylcyclohexane, and extrude and mix the above composition in a reciprocating single-screw extruder at an extrusion temperature of 120-150-180° C. After granulation, enter the drum for post-absorption, add 1.4 parts of crosslinking agent DCP, the post-absorption temperature is 70° C., and the time is 24 hours to obtain a polymer composition sample.
[0047] The prepared samples were subjected to relevant performance tests.
[0048] Example 4
[0049] Preparation of polymer composition:
[0050] 96.7 parts of base material LDPE, 0.8 parts of antioxidant 1315, and 2.5 parts of 1,2,4-triethylcyclohexane were accurately weighed, and the above composition was extruded and mixed in a reciprocating single-screw extruder at an extrusion temperature of 120-150-180° C. After granulation, it was put into a rotary drum for post-absorption, 1.7 parts of crosslinking agent DCP was added, the post-absorption temperature was 70° C., and the time was 20 hours to obtain a polymer composition sample.
[0051] The prepared samples were subjected to relevant performance tests.
[0052] Example 5
[0053] Preparation of polymer composition:
[0054] Accurately weigh 98.85 parts of base material LDPE, 0.15 parts of antioxidant 1315, and 1 part of 1,2,4-triethylcyclohexane, and extrude and mix the above composition in a reciprocating single-screw extruder at an extrusion temperature of 120-150-180° C. After granulation, enter the drum for post-absorption, add 1.0 parts of cross-linking agent tert-butyl peroxide isopropylbenzene, the post-absorption temperature is 70° C., and the time is 20 hours to obtain a polymer composition sample.
[0055] The prepared samples were subjected to relevant performance tests.
[0056] Example 6
[0057] Accurately weigh 99.4 parts of base material LDPE, 0.10 parts of antioxidant 1315, and 1.5 parts of 1,2,4-triethylcyclohexane, and extrude and mix the above composition in a reciprocating single screw extruder at an extrusion temperature of 120-150-180° C. After granulation, enter the drum for post-absorption, add 0.8 parts of crosslinking agent DCP, the post-absorption temperature is 70° C., and the time is 24 hours to obtain a polymer composition sample.
[0058] The prepared samples were subjected to relevant performance tests.
[0059] Comparative Example 1
[0060] Accurately weigh 98.85 parts of base material LDPE, 0.15 parts of antioxidant 300, and 1 part of 1,2,4-triethylcyclohexane, and extrude and mix the above composition in a reciprocating single screw extruder at an extrusion temperature of 120-150-180° C. After granulation, enter the drum for post-absorption, add 1.0 parts of crosslinking agent DCP, the post-absorption temperature is 80° C., and the time is 16 hours to obtain a polymer composition sample.
[0061] The prepared samples were subjected to relevant performance tests.
[0062] Comparative Example 2
[0063] 99.85 parts of base material LDPE and 0.15 parts of antioxidant 300 were accurately weighed, and the above composition was extruded and mixed in a reciprocating single screw extruder at an extrusion temperature of 120-150-180° C. After granulation, it was put into a rotary drum for post-absorption, and 1.6 parts of crosslinking agent DCP were added, the post-absorption temperature was 80° C., and the time was 16 hours to obtain a polymer composition sample.
[0064] The prepared samples were subjected to relevant performance tests.
[0065] The performance test results of the embodiments and comparative examples are shown in Table 1.
[0066] Table 1 Summary of sample performance test results
[0067]
[0068] By comparing the performance data of different samples in the above table, it can be found that the solution provided by the present invention can achieve better aging resistance with less antioxidant added, and greatly reduce the amount of cross-linking agent used (Example 3 and Example 6), which is very beneficial for later degassing. At the same time, using the solution of the present invention, under the premise of qualified hot stretching, the amount of alcohol washing residue is also greatly reduced, which is beneficial to the stability of cable extrusion. Other properties such as electrical properties and mechanical properties also maintain relatively excellent performance.
[0069] The above embodiments are only used to describe the preferred implementation modes of the present invention, rather than to limit the protection scope of the present invention. Although the present invention has been described in detail with reference to the preferred embodiments, those skilled in the art should understand that various modifications and improvements made by modifying or equivalently replacing the technical solutions of the present invention should all fall within the protection scope determined by the claims of the present invention.
Claims
1. A polymer composition for cable materials, comprising: (1) polyethylene, 92.0-99.9 parts, preferably 95.0-99.9 parts; (2) Liquid hindered phenol antioxidant 1315, 0.01-1.0 part, preferably 0.025-0.5 part, most preferably 0.05-0.3 part; (3) Cross-linking agent: 0.25-3 parts, preferably 0.5-2.5 parts, more preferably 0.5-2 parts.
2. A polymer composition for cable materials, comprising: (1) polyethylene, 92.0-99.9 parts, preferably 95.0-99.9 parts; (2) Liquid hindered phenol antioxidant 1315, 0.01-1.0 part, preferably 0.025-0.5 part, most preferably 0.05-0.3 part; (3) cross-linking agent, 0.25-3 parts, preferably 0.5-2.5 parts, more preferably 0.5-2 parts; (4) 1,2,4-triethylcyclohexane, the addition amount is 0.05-3 parts, preferably 0.1-2 parts, more preferably 0.2-1 parts.
3. The composition according to claim 1 or 2, wherein the polyethylene is a low-density polyethylene, preferably with a melt index of 1.6-2.4 g / min, tested at 190°C, 2.16 kg; more preferably, the density of the polyethylene is 0.920-0.924 g / cm 3 .
4. The composition according to claim 1 or 2, wherein the cross-linking agent is selected from one or more of tert-butyl perbenzoate, dibenzoyl peroxide, dicumyl peroxide, and tert-butyl peroxide isopropylbenzene, preferably dicumyl peroxide.
5. A method for preparing the polymer composition for cable materials according to any one of claims 1 to 4, comprising mixing the antioxidant and optional auxiliary agents with polyethylene, first mixing and granulating through a reciprocating single-screw extruder, and post-absorbing and cross-linking the obtained particles to obtain the polymer composition for cable materials.
6. The preparation method according to claim 5, wherein the mixing temperature is 110-190°C, preferably 120-180°C; The post-absorption temperature is 40-100°C, preferably 50-80°C; The post-absorption time is 6-48h, preferably 8-24h.
7. Use of the polymer composition according to any one of claims 1 to 4 or the polymer composition prepared by the preparation method according to any one of claims 5 to 6 in the field of high-voltage wires and cables.
Citation Information
Patent Citations
Polyethylene powder, process for its preparation and its use for rotomolding
CN107922669A
Composite liquid antioxidant and preparation method thereof
CN114805929A
Composite material for shielding direct-current / alternating-current high-voltage cable and preparation method thereof
CN115403853A
Toughening compatible flame retardant as well as preparation method and application thereof
CN117487046A
Crosslinked polyethylene composition for manufacturing insulator of middle-high voltage electric wire and cable and application of crosslinked polyethylene composition
CN117683289A