Heat-resistant inner tube material and preparation method thereof

Through the combined vulcanization treatment of modified silicone and modified butyl rubber, stearic acid and sulfur, heat-resistant inner tube materials with good anti-aging, flame retardant, heat-resistant and air-tight properties were prepared, and the existing rubber materials were solved. The shortcomings in high barrier and heat resistance meet the application needs under harsh working conditions.

CN118725477BActive Publication Date: 2024-11-22NANTONG SUNCHI RUBBER PROD CO LTD
View PDF 0 Cites 0 Cited by

Patent Information

Application Number
CN202411227114.X
Authority / Receiving Office
CN · China
Patent Type
Patents(China)
Current Assignee / Owner
Filing Date
2024-09-03
Publication Date
2024-11-22
Estimated Expiration
2044-09-03

AI Technical Summary

Technical Problem

The existing rubber materials have shortcomings in high barrier and heat resistance, and it is difficult to meet the application needs under harsh working conditions.

Method used

By combining the vulcanization treatment of modified silicone with modified butyl rubber, stearic acid and sulfur, heat-resistant inner tube materials with good anti-aging, flame retardant, heat-resistant and air-tight properties were prepared.

Benefits of technology

It improves the material's wear resistance, airtightness, flame retardant and heat resistance, and meets the application needs of high barrier and heat resistance.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure SMS_5
    Figure SMS_5
  • Figure SMS_6
    Figure SMS_6
  • Figure SMS_7
    Figure SMS_7
Patent Text Reader

Abstract

The invention discloses a heat-resistant inner tube material and a preparation method thereof, and relates to the field of rubber materials. When preparing the heat-resistant inner tube material, the present invention first reacts aminopropyltrimethoxysilane, 2,7-dimethyl-2,4,6-octatriene dialdehyde with 3,5-di-tert-butyl-4-hydroxybenzylamine to obtain modified siloxane, and then reacts the modified siloxane with allyltrimethoxysilane to obtain modified polysilsesquioxane; butyl rubber is epoxidized and hydroxylated to obtain hydroxylated butyl rubber; hydroxylated butyl rubber is reacted with diallyl chlorophosphite to obtain modified butyl rubber; modified butyl rubber, modified polysilsesquioxane, stearic acid, and sulfur are mixed and vulcanized to obtain. The heat-resistant inner tube material prepared by the present invention has good anti-aging performance, flame retardant performance, heat resistance and tensile strength.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The invention relates to the field of rubber materials, in particular to a heat-resistant inner tube material and a preparation method thereof. Background Art

[0002] Rubber composites are widely used in transportation, medical and health fields due to their unique high elasticity and softness. Gas barrier is an important property of rubber composites, which can be used in products such as automobile inner tubes, medical plugs, and protective clothing. With the continuous expansion of application scenarios and increasingly harsh working conditions, higher requirements are placed on high-barrier rubber materials. The design and preparation of high-barrier rubber materials have important application significance. Among general synthetic rubbers, butyl rubber has excellent airtight properties and is also the main raw material for many current airtight structural parts.

[0003] Cage-like polysilsesquioxane is often used as a flame retardant and reinforcing filler in a polymer matrix due to its high thermal stability and good compatibility with polymers. The heat-resistant inner tube material prepared by the present invention is prepared by reacting modified polysilsesquioxane with modified butyl rubber and stearic acid, has good anti-aging performance, flame retardancy, heat resistance and tensile strength, and has good market prospects. Summary of the invention

[0004] The purpose of the present invention is to provide a method for preparing a heat-resistant inner tube material to solve the problems existing in the prior art.

[0005] In order to solve the above technical problems, the present invention provides the following technical solutions:

[0006] A method for preparing a heat-resistant inner tube material. The heat-resistant inner tube material comprises the following steps: preparing modified siloxane by reacting aminopropyltrimethoxysilane, 2,7-dimethyl-2,4,6-octatriene dialdehyde and 3,5-di-tert-butyl-4-hydroxybenzylamine; then preparing modified polysilsesquioxane by reacting the modified siloxane with allyltrimethoxysilane; preparing hydroxylated butyl rubber by epoxidizing and hydroxylating butyl rubber; preparing modified butyl rubber by reacting the hydroxylated butyl rubber with diallyl chlorophosphite; and preparing the heat-resistant inner tube material by mixing and vulcanizing the modified butyl rubber, the modified polysilsesquioxane, stearic acid and sulfur.

[0007] A method for preparing a heat-resistant inner tube material comprises the following preparation steps:

[0008] (1) Mix aminopropyltrimethoxysilane, 2,7-dimethyl-2,4,6-octatriene dialdehyde, 3,5-di-tert-butyl-4-hydroxybenzylamine and anhydrous ethanol in a mass ratio of 1: (0.7-0.9): (1-1.4): (15-25), stir at 35-45°C and 400-600 r / min for 3-5 hours, extract and wash the organic phase with dichloromethane for 3-5 times, take the organic phase, and distill under reduced pressure at 50-60°C for 4-6 hours to obtain modified siloxane;

[0009] (2) Allyl trimethoxysilane, modified siloxane, methyl ethyl ketone and anhydrous methanol are mixed in a mass ratio of 1: (0.2-0.4): (18-22): (3-5), and a 0.1 mol sodium hydroxide aqueous solution (0.05-0.15 times the mass of methyl ethyl ketone) is added dropwise at a rate of 2-4 ml / min at 0°C. After the addition is completed, the reaction is continued for 0.5-1.5 h, and the temperature is raised to 70-80°C and the reaction is continued for 22-26 h. The organic phase is extracted and washed with dichloromethane for 3-5 times, and the organic phase is taken and distilled at 50-60°C under reduced pressure for 4-6 h to obtain modified polysilsesquioxane;

[0010] (3) Mix butyl rubber and n-hexane in a mass ratio of 1: (6-7), stir at 300-400 r / min for 25-35 min at 35-45°C, add m-chloroperbenzoic acid in an amount of 0.025-0.035 times the mass of butyl rubber, continue stirring for 45-75 min, adjust the pH to neutral with a 1% sodium hydroxide aqueous solution, cool to room temperature, continue stirring for 1.5-2.5 h, pour into 80-90°C hot water and stir for 1-2 h, wash with deionized water 3-5 times, and dry at 55-65°C for 3-5 h to obtain epoxidized butyl rubber; Mix epoxidized butyl rubber and n-hexane in a mass ratio of 1: (6-7), add a 36.5% concentrated hydrochloric acid solution in an amount equal to the molar amount of epoxy groups in the epoxidized butyl rubber, and continue stirring for 45-75 min. During the process, according to GB / T 4612-2008 monitors the ring-opening of the epoxy group. After the epoxy group is fully ring-opened, adjust the pH to neutral with a 1% sodium hydroxide aqueous solution, cool to room temperature, continue stirring for 1.5-2.5 hours, pour and immerse in anhydrous ethanol, filter after solid precipitation, wash the solid with anhydrous ethanol for 3-5 times, and dry at 55-65°C for 3-5 hours to obtain hydroxylated butyl rubber;

[0011] (4) Mix hydroxylated butyl rubber, diallyl chlorophosphite, triethanolamine and dimethyl sulfoxide in a mass ratio of 1: (0.7-0.9): (0.2-0.4): (8-12), stir at 80-90°C and 300-400 r / min for 3-5 hours, cool to room temperature, filter, wash the solid with anhydrous ethanol for 3-5 times, and dry at 55-65°C for 3-5 hours to obtain modified butyl rubber;

[0012] (5) The modified butyl rubber, modified polysilsesquioxane and stearic acid are mixed in a mass ratio of (8-12): 1: 0.025, and mixed on an open mill at 100-120°C for 20-40 min. The roller spacing of the open mill is adjusted to 1-3 mm. At 50-70°C, sulfur is added in an amount of 0.02-0.04 times the mass of the modified butyl rubber. The mixture is triangularly packed 3-5 times, and vulcanized on a flat vulcanizer at 140-160°C and 14-16 MPa for 10-12 h. The mixture is naturally cooled to room temperature and then taken out to obtain a heat-resistant inner tube material.

[0013] As an optimization, the modified siloxane reaction process in step (1) is as follows:

[0014] .

[0015] As an optimization, the reaction process of the modified polysilsesquioxane in step (2) is as follows:

[0016] .

[0017] As an optimization, the reaction process of hydroxylated butyl rubber in step (3) is as follows:

[0018] .

[0019] As an optimization, the butyl rubber in step (3) is a butyl rubber with a number average molecular weight of 300,000 and an unsaturation degree of 1.9%.

[0020] As an optimization, the reaction process of the modified butyl rubber in step (4) is as follows:

[0021] .

[0022] Compared with the prior art, the beneficial effects achieved by the present invention are:

[0023] When preparing the heat-resistant inner tube material, the present invention comprises the following steps: firstly reacting aminopropyltrimethoxysilane, 2,7-dimethyl-2,4,6-octatriene dialdehyde and 3,5-di-tert-butyl-4-hydroxybenzylamine to obtain modified siloxane, then reacting the modified siloxane with allyltrimethoxysilane to obtain modified polysilsesquioxane; epoxidizing and hydroxylating butyl rubber to obtain hydroxylated butyl rubber; reacting the hydroxylated butyl rubber with diallyl chlorophosphite to obtain modified butyl rubber; and mixing and vulcanizing the modified butyl rubber, the modified polysilsesquioxane, stearic acid and sulfur to obtain the heat-resistant inner tube material.

[0024] Firstly, aminopropyltrimethoxysilane, 2,7-dimethyl-2,4,6-octatriene dialdehyde and 3,5-di-tert-butyl-4-hydroxybenzylamine are reacted to obtain modified siloxane, and the modified siloxane is modified by reacting with allyltrimethoxysilane to obtain modified polysilsesquioxane. A large number of double bond structures are introduced into the modified polysilsesquioxane, which can not only improve the dispersibility of the modified polysilsesquioxane in rubber and thus improve the heat resistance of the material, but also produce a better cross-linking effect with the modified butyl rubber during vulcanization, thereby improving the wear resistance and air tightness of the material; 3,5-di-tert-butyl-4-hydroxybenzylamine introduced into the modified siloxane as a hindered phenol structure can capture free radicals and prevent oxidation reactions caused by free radicals, thereby improving the anti-aging performance of the heat-resistant inner tube material.

[0025] Secondly, butyl rubber is modified by epoxidation and hydroxylation and then reacted with diallyl chlorophosphite to obtain modified butyl rubber, which introduces phosphorus. The introduction of phosphorus can promote the formation of a carbon layer, thereby isolating heat and oxygen and improving the flame retardant properties of the heat-resistant inner tube material. After diallyl chlorophosphite reacts with hydroxylated butyl rubber, more double bond structures are introduced, which increases the unsaturation of butyl rubber, thereby improving the cross-linking effect during vulcanization and further improving the air tightness of the material. Modified polysilsesquioxane reacts with modified butyl rubber to obtain a heat-resistant inner tube material. The thermal stability of the Si-O bond on the modified polysilsesquioxane is higher than that of the CC bond and the CH bond, so the heat-resistant inner tube material has good heat resistance, and the modified polysilsesquioxane can also act as a filler to play a physical barrier, further improving the air tightness of the material. DETAILED DESCRIPTION

[0026] The following will be combined with the embodiments of the present invention to clearly and completely describe the technical solutions in the embodiments of the present invention. Obviously, the described embodiments are only part of the embodiments of the present invention, not all of the embodiments. Based on the embodiments of the present invention, all other embodiments obtained by ordinary technicians in this field without making creative work are within the scope of protection of the present invention.

[0027] Example 1

[0028] A method for preparing a heat-resistant inner tube material comprises the following preparation steps:

[0029] (1) Aminopropyltrimethoxysilane, 2,7-dimethyl-2,4,6-octatriene dialdehyde, 3,5-di-tert-butyl-4-hydroxybenzylamine and anhydrous ethanol were mixed in a mass ratio of 1:0.7:1:15, stirred at 400 r / min for 3 h at 35 °C, the organic phase was extracted and washed with dichloromethane for 3 times, the organic phase was taken, and vacuum distilled at 50 °C for 4 h to obtain modified siloxane;

[0030] (2) Allyl trimethoxysilane, modified siloxane, methyl ethyl ketone and anhydrous methanol were mixed in a mass ratio of 1:0.2:18:3, and a 0.1 mol sodium hydroxide aqueous solution (0.05 times the mass of methyl ethyl ketone) was added dropwise at a rate of 2 ml / min at 0°C. After the addition was completed, the reaction was continued for 0.5 h, and the temperature was raised to 70°C and the reaction was continued for 22 h. The organic phase was extracted and washed with dichloromethane for 3 times, and the organic phase was taken and distilled at 50°C under reduced pressure for 4 h to obtain modified polysilsesquioxane;

[0031] (3) Mix butyl rubber and n-hexane in a mass ratio of 1:6, stir at 300 r / min at 35°C for 25 min, add 0.025 times the mass of m-chloroperbenzoic acid to the butyl rubber, continue stirring for 45 min, adjust the pH to neutral with a 1% sodium hydroxide aqueous solution, cool to room temperature, continue stirring for 1.5 h, pour into 80°C hot water and stir for 1 h, wash with deionized water 3 times, and dry at 55°C for 3 h to obtain epoxidized butyl rubber; Mix epoxidized butyl rubber and n-hexane in a mass ratio of 1:6, add a 36.5% concentrated hydrochloric acid solution with an equal molar amount of epoxy groups in the epoxidized butyl rubber, and continue stirring for 45 min. During the process, according to GB / T 4612-2008 monitors the ring-opening of the epoxy group. After the epoxy group is fully ring-opened, adjust the pH to neutral with a 1% sodium hydroxide aqueous solution, cool to room temperature, continue stirring for 1.5 hours, pour and immerse in anhydrous ethanol, filter after solids precipitate, wash the solids with anhydrous ethanol for 3 times, and dry at 55°C for 3 hours to obtain hydroxylated butyl rubber;

[0032] (4) Mix hydroxylated butyl rubber, diallyl chlorophosphite, triethanolamine and dimethyl sulfoxide in a mass ratio of 1:0.7:0.2:8, stir at 80°C and 300 r / min for 3 h, cool to room temperature, filter, wash the solid with anhydrous ethanol three times, and dry at 55°C for 3 h to obtain modified butyl rubber;

[0033] (5) The modified butyl rubber, modified polysilsesquioxane and stearic acid were mixed in a mass ratio of 8:1:0.025, and mixed on an open mill at 100°C for 20 min. The roller spacing of the open mill was adjusted to 1 mm. At 50°C, sulfur 0.02 times the mass of the modified butyl rubber was added, and the mixture was triangularly packed three times. The mixture was vulcanized on a flat vulcanizer at 140°C and 14 MPa for 10 h. The mixture was naturally cooled to room temperature and then taken out to obtain a heat-resistant inner tube material.

[0034] Example 2

[0035] A method for preparing a heat-resistant inner tube material comprises the following preparation steps:

[0036] (1) Aminopropyltrimethoxysilane, 2,7-dimethyl-2,4,6-octatriene dialdehyde, 3,5-di-tert-butyl-4-hydroxybenzylamine and anhydrous ethanol were mixed in a mass ratio of 1:0.8:1.2:20, stirred at 40°C and 500 r / min for 4 hours, the organic phase was extracted and washed with dichloromethane for 4 times, the organic phase was taken, and vacuum distilled at 55°C for 5 hours to obtain modified siloxane;

[0037] (2) Allyl trimethoxysilane, modified siloxane, methyl ethyl ketone and anhydrous methanol were mixed in a mass ratio of 1:0.3:20:4, and a 0.1 mol sodium hydroxide aqueous solution (0.1 times the mass of methyl ethyl ketone) was added dropwise at a rate of 3 ml / min at 0°C. After the addition was completed, the reaction was continued for 1 hour, and the temperature was raised to 75°C and the reaction was continued for 24 hours. The organic phase was extracted and washed with dichloromethane for 4 times, and the organic phase was taken and distilled at 55°C under reduced pressure for 5 hours to obtain modified polysilsesquioxane;

[0038] (3) Butyl rubber and n-hexane were mixed in a mass ratio of 1:6.5, stirred at 350 r / min at 40°C for 30 min, m-chloroperoxybenzoic acid (0.03 times the mass of butyl rubber) was added, and stirring was continued for 60 min. The pH was adjusted to neutral with a 1% sodium hydroxide aqueous solution, cooled to room temperature, and stirred for 2 h. The mixture was poured into 85°C hot water and stirred for 1.5 h. The mixture was washed with deionized water for 4 times and dried at 60°C for 4 h to obtain epoxidized butyl rubber. Epoxidized butyl rubber and n-hexane were mixed in a mass ratio of 1:6.5, and a 36.5% concentrated hydrochloric acid solution (equimolar to the epoxy group in the epoxidized butyl rubber) was added, and stirring was continued for 60 min. During the process, the reaction mixture was heated to 40 ℃ and the reaction mixture was heated to 85 ... 4612-2008 monitors the ring-opening of the epoxy group. After the epoxy group is fully ring-opened, adjust the pH to neutral with a 1% sodium hydroxide aqueous solution, cool to room temperature, continue stirring for 2 hours, pour and immerse in anhydrous ethanol, filter after solid precipitation, wash the solid with anhydrous ethanol for 4 times, and dry at 60°C for 4 hours to obtain hydroxylated butyl rubber;

[0039] (4) Mix hydroxylated butyl rubber, diallyl chlorophosphite, triethanolamine and dimethyl sulfoxide in a mass ratio of 1:0.8:0.3:10, stir at 85°C and 350 r / min for 4 h, cool to room temperature, filter, wash the solid with anhydrous ethanol 4 times, and dry at 60°C for 4 h to obtain modified butyl rubber;

[0040] (5) The modified butyl rubber, modified polysilsesquioxane and stearic acid were mixed in a mass ratio of 10:1:0.025, and mixed on an open mill at 110°C for 30 min. The roller spacing of the open mill was adjusted to 2 mm. At 60°C, sulfur 0.03 times the mass of the modified butyl rubber was added, and the mixture was triangularly packed 4 times. The mixture was vulcanized on a flat vulcanizer at 150°C and 15 MPa for 11 h. The mixture was naturally cooled to room temperature and then taken out to obtain a heat-resistant inner tube material.

[0041] Example 3

[0042] A method for preparing a heat-resistant inner tube material comprises the following preparation steps:

[0043] (1) Aminopropyltrimethoxysilane, 2,7-dimethyl-2,4,6-octatriene dialdehyde, 3,5-di-tert-butyl-4-hydroxybenzylamine and anhydrous ethanol were mixed in a mass ratio of 1:0.9:1.4:25, stirred at 45°C and 600 r / min for 5 h, the organic phase was extracted and washed with dichloromethane for 5 times, the organic phase was taken, and vacuum distilled at 60°C for 6 h to obtain modified siloxane;

[0044] (2) Allyl trimethoxysilane, modified siloxane, methyl ethyl ketone and anhydrous methanol were mixed in a mass ratio of 1:0.4:22:5, and a 0.1 mol sodium hydroxide aqueous solution (0.15 times the mass of methyl ethyl ketone) was added dropwise at a rate of 4 ml / min at 0°C. After the addition was completed, the reaction was continued for 1.5 hours, and the temperature was raised to 80°C and the reaction was continued for 26 hours. The organic phase was extracted and washed with dichloromethane for 5 times, and the organic phase was taken and distilled at 60°C under reduced pressure for 6 hours to obtain modified polysilsesquioxane;

[0045] (3) Mix butyl rubber and n-hexane in a mass ratio of 1:7, stir at 400 r / min at 45°C for 35 min, add 0.035 times the mass of m-chloroperbenzoic acid to the butyl rubber, continue stirring for 75 min, adjust the pH to neutral with a 1% sodium hydroxide aqueous solution, cool to room temperature, continue stirring for 2.5 h, pour into 90°C hot water and stir for 2 h, wash with deionized water 5 times, and dry at 65°C for 5 h to obtain epoxidized butyl rubber; Mix epoxidized butyl rubber and n-hexane in a mass ratio of 1:7, add a 36.5% concentrated hydrochloric acid solution with an equal molar amount of epoxy groups in the epoxidized butyl rubber, and continue stirring for 75 min. During the process, according to GB / T 4612-2008 monitors the ring-opening of the epoxy group. After the epoxy group is fully ring-opened, adjust the pH to neutral with a 1% sodium hydroxide aqueous solution, cool to room temperature, continue stirring for 2.5 hours, pour and immerse in anhydrous ethanol, filter after solid precipitation, wash the solid with anhydrous ethanol for 5 times, and dry at 65°C for 5 hours to obtain hydroxylated butyl rubber;

[0046] (4) Mix hydroxylated butyl rubber, diallyl chlorophosphite, triethanolamine and dimethyl sulfoxide in a mass ratio of 1:0.9:0.4:12, stir at 90°C and 400 r / min for 5 h, cool to room temperature, filter, wash the solid with anhydrous ethanol 5 times, and dry at 65°C for 5 h to obtain modified butyl rubber;

[0047] (5) The modified butyl rubber, modified polysilsesquioxane and stearic acid were mixed in a mass ratio of 12:1:0.025, and mixed on an open mill at 120°C for 40 min. The roller spacing of the open mill was adjusted to 3 mm. At 70°C, sulfur 0.04 times the mass of the modified butyl rubber was added, and the mixture was triangularly packed 5 times. The mixture was vulcanized on a flat vulcanizer at 160°C and 16 MPa for 12 h. The mixture was naturally cooled to room temperature and then taken out to obtain a heat-resistant inner tube material.

[0048] Comparative Example 1

[0049] A method for preparing a heat-resistant inner tube material comprises the following preparation steps:

[0050] (1) Aminopropyltrimethoxysilane, 2,7-dimethyl-2,4,6-octatriene dialdehyde, 3,5-di-tert-butyl-4-hydroxybenzylamine and anhydrous ethanol were mixed in a mass ratio of 1:0.8:1.2:20, stirred at 40°C and 500 r / min for 4 hours, the organic phase was extracted and washed with dichloromethane for 4 times, the organic phase was taken, and vacuum distilled at 55°C for 5 hours to obtain modified siloxane;

[0051] (2) Allyl trimethoxysilane, modified siloxane, methyl ethyl ketone and anhydrous methanol were mixed in a mass ratio of 1:0.3:20:4, and a 0.1 mol sodium hydroxide aqueous solution (0.1 times the mass of methyl ethyl ketone) was added dropwise at a rate of 3 ml / min at 0°C. After the addition was completed, the reaction was continued for 1 hour, and the temperature was raised to 75°C and the reaction was continued for 24 hours. The organic phase was extracted and washed with dichloromethane for 4 times, and the organic phase was taken and distilled at 55°C under reduced pressure for 5 hours to obtain modified polysilsesquioxane;

[0052] (3) Butyl rubber, modified polysilsesquioxane and stearic acid are mixed in a mass ratio of 10:1:0.025, and kneaded on an open mill at 110°C for 30 min. The roller spacing of the open mill is adjusted to 2 mm. At 60°C, sulfur 0.03 times the mass of the modified butyl rubber is added, and the mixture is triangularly packaged 4 times. The mixture is vulcanized on a flat vulcanizer at 150°C and 15 MPa for 11 h. The mixture is naturally cooled to room temperature and then taken out to obtain a heat-resistant inner tube material.

[0053] Comparative Example 2

[0054] A method for preparing a heat-resistant inner tube material comprises the following preparation steps:

[0055] (1) Butyl rubber and n-hexane were mixed in a mass ratio of 1:6.5, stirred at 350 r / min at 40°C for 30 min, m-chloroperoxybenzoic acid (0.03 times the mass of butyl rubber) was added, and stirring was continued for 60 min. The pH was adjusted to neutral with a 1% sodium hydroxide aqueous solution, cooled to room temperature, and stirred for 2 h. The mixture was poured into 85°C hot water and stirred for 1.5 h. The mixture was washed with deionized water for 4 times and dried at 60°C for 4 h to obtain epoxidized butyl rubber. Epoxidized butyl rubber and n-hexane were mixed in a mass ratio of 1:6.5, and a 36.5% concentrated hydrochloric acid solution (equimolar to the epoxy group in the epoxidized butyl rubber) was added, and stirring was continued for 60 min. During the process, the reaction mixture was heated to 40 ℃ and the reaction mixture was heated to 85 ... 4612-2008 monitors the ring-opening of the epoxy group. After the epoxy group is fully ring-opened, adjust the pH to neutral with a 1% sodium hydroxide aqueous solution, cool to room temperature, continue stirring for 2 hours, pour and immerse in anhydrous ethanol, filter after solid precipitation, wash the solid with anhydrous ethanol for 4 times, and dry at 60°C for 4 hours to obtain hydroxylated butyl rubber;

[0056] (2) Mix hydroxylated butyl rubber, diallyl chlorophosphite, triethanolamine and dimethyl sulfoxide in a mass ratio of 1:0.8:0.3:10, stir at 85°C and 350 r / min for 4 h, cool to room temperature, filter, wash the solid with anhydrous ethanol 4 times, and dry at 60°C for 4 h to obtain modified butyl rubber;

[0057] (3) The modified butyl rubber, polymethylsiloxane and stearic acid were mixed in a mass ratio of 10:1:0.025, and mixed on an open mill at 110°C for 30 min. The roller spacing of the open mill was adjusted to 2 mm. At 60°C, sulfur 0.03 times the mass of the modified butyl rubber was added, and the mixture was triangularly packed 4 times. The mixture was vulcanized on a flat vulcanizer at 150°C and 15 MPa for 11 h. The mixture was naturally cooled to room temperature and then taken out to obtain a heat-resistant inner tube material.

[0058] Comparative Example 3

[0059] A method for preparing a heat-resistant inner tube material comprises the following preparation steps:

[0060] (1) Butyl rubber and n-hexane were mixed in a mass ratio of 1:6.5, stirred at 350 r / min at 40°C for 30 min, m-chloroperoxybenzoic acid (0.03 times the mass of butyl rubber) was added, and stirring was continued for 60 min. The pH was adjusted to neutral with a 1% sodium hydroxide aqueous solution, cooled to room temperature, and stirred for 2 h. The mixture was poured into 85°C hot water and stirred for 1.5 h. The mixture was washed with deionized water for 4 times and dried at 60°C for 4 h to obtain epoxidized butyl rubber. Epoxidized butyl rubber and n-hexane were mixed in a mass ratio of 1:6.5, and a 36.5% concentrated hydrochloric acid solution (equimolar to the epoxy group in the epoxidized butyl rubber) was added, and stirring was continued for 60 min. During the process, the reaction mixture was heated to 40 ℃ and the reaction mixture was heated to 85 ... 4612-2008 monitors the ring-opening of the epoxy group. After the epoxy group is fully ring-opened, adjust the pH to neutral with a 1% sodium hydroxide aqueous solution, cool to room temperature, continue stirring for 2 hours, pour and immerse in anhydrous ethanol, filter after solid precipitation, wash the solid with anhydrous ethanol for 4 times, and dry at 60°C for 4 hours to obtain hydroxylated butyl rubber;

[0061] (2) Mix hydroxylated butyl rubber, diallyl chlorophosphite, triethanolamine and dimethyl sulfoxide in a mass ratio of 1:0.8:0.3:10, stir at 85°C and 350 r / min for 4 h, cool to room temperature, filter, wash the solid with anhydrous ethanol 4 times, and dry at 60°C for 4 h to obtain modified butyl rubber;

[0062] (3) The modified butyl rubber, octavinyl cage polysilsesquioxane and stearic acid were mixed in a mass ratio of 10:1:0.025, and mixed on an open mill at 110°C for 30 min. The roller spacing of the open mill was adjusted to 2 mm. At 60°C, sulfur 0.03 times the mass of the modified butyl rubber was added, and the mixture was triangularly packaged 4 times. The mixture was vulcanized on a flat vulcanizer at 150°C and 15 MPa for 11 h. The mixture was naturally cooled to room temperature and then taken out to obtain a heat-resistant inner tube material.

[0063] Comparative Example 4

[0064] A method for preparing a heat-resistant inner tube material comprises the following preparation steps:

[0065] (1) Butyl rubber and n-hexane were mixed in a mass ratio of 1:6.5, stirred at 350 r / min at 40°C for 30 min, m-chloroperoxybenzoic acid (0.03 times the mass of butyl rubber) was added, and stirring was continued for 60 min. The pH was adjusted to neutral with a 1% sodium hydroxide aqueous solution, cooled to room temperature, and stirred for 2 h. The mixture was poured into 85°C hot water and stirred for 1.5 h. The mixture was washed with deionized water for 4 times and dried at 60°C for 4 h to obtain epoxidized butyl rubber. Epoxidized butyl rubber and n-hexane were mixed in a mass ratio of 1:6.5, and a 36.5% concentrated hydrochloric acid solution (equimolar to the epoxy group in the epoxidized butyl rubber) was added, and stirring was continued for 60 min. During the process, the reaction mixture was heated to 40 ℃ and the reaction mixture was heated to 85 ... 4612-2008 monitors the ring-opening of the epoxy group. After the epoxy group is fully ring-opened, adjust the pH to neutral with a 1% sodium hydroxide aqueous solution, cool to room temperature, continue stirring for 2 hours, pour and immerse in anhydrous ethanol, filter after solid precipitation, wash the solid with anhydrous ethanol for 4 times, and dry at 60°C for 4 hours to obtain hydroxylated butyl rubber;

[0066] (2) Mix hydroxylated butyl rubber, diallyl chlorophosphite, triethanolamine and dimethyl sulfoxide in a mass ratio of 1:0.8:0.3:10, stir at 85°C and 350 r / min for 4 h, cool to room temperature, filter, wash the solid with anhydrous ethanol 4 times, and dry at 60°C for 4 h to obtain modified butyl rubber;

[0067] (3) The modified butyl rubber and stearic acid were mixed in a mass ratio of 10:0.025, and mixed on an open mill at 110°C for 30 min. The roller spacing of the open mill was adjusted to 2 mm. At 60°C, sulfur 0.03 times the mass of the modified butyl rubber was added, and the mixture was triangularly packed 4 times. The mixture was vulcanized on a flat vulcanizer at 150°C and 15 MPa for 11 h. The mixture was naturally cooled to room temperature and then taken out to obtain a heat-resistant inner tube material.

[0068] Test Example 1

[0069] Flame retardant properties: The heat-resistant inner tube materials obtained in each embodiment and the comparative example were tested for limiting oxygen index according to GB / T2406. The results are shown in Table 1.

[0070] Table 1

[0071]

[0072] From the comparison of the experimental data of Examples 1 to 3 and Comparative Examples 1 to 4 in Table 1, it can be found that the heat-resistant inner tube material prepared by the present invention has good flame retardant properties.

[0073] By comparison, the limiting oxygen index of Examples 1 to 3 is significantly greater than that of Comparative Example 1, indicating that the reaction of diallyl chlorophosphite with hydroxylated butyl rubber introduces phosphorus element, and the introduction of phosphorus element can promote the formation of a carbon layer, thereby achieving the effect of isolating heat and oxygen, and improving the flame retardant properties of the heat-resistant inner tube material; the limiting oxygen index of Examples 1 to 3 is significantly greater than that of Comparative Example 4, indicating that the modified polysilsesquioxane and the phosphorus element on the modified butyl rubber synergistically flame retardant, can promote cross-linking carbonization of rubber, effectively hinder heat transfer and oxygen diffusion, and improve the flame retardant properties of the heat-resistant inner tube material.

[0074] Test Example 2

[0075] Wear resistance: The heat-resistant inner tube materials obtained in each embodiment and the comparative example were tested for wear according to GB / T9867. The results are shown in Table 2.

[0076] Table 2

[0077]

[0078] From the comparison of the experimental data of Examples 1 to 3 and Comparative Examples 1 to 4 in Table 2, it can be found that the heat-resistant inner tube material prepared by the present invention has good wear resistance.

[0079] By comparison, the wear amount of Examples 1 to 3 is significantly less than that of Comparative Example 1, indicating that more double bonds are introduced into the diallyl chlorophosphite on the modified butyl rubber, which improves the cross-linking effect during vulcanization, thereby improving the wear resistance of the heat-resistant inner tube material; the wear amount of Examples 1 to 3 is significantly less than that of Comparative Example 2, indicating that the abundant double bonds on the modified polysilsesquioxane improve the cross-linking effect during vulcanization, thereby improving the wear resistance of the heat-resistant inner tube material; the wear amount of Examples 1 to 3 is significantly less than that of Comparative Example 4, indicating that the modified polysilsesquioxane as an inorganic filler can effectively improve the wear resistance of the heat-resistant inner tube material.

[0080] Test Example 3

[0081] Heat resistance: The heat-resistant inner tube materials obtained in each embodiment and the comparative example were cut into dumbbell pieces as specified in GB / T528, and placed in a tensile fixture in a high temperature box. The samples were preheated at the test temperature of 175°C for 10 minutes, and the testing machine was started to test the breaking strength. The results are shown in Table 3.

[0082] Table 3

[0083]

[0084] From the comparison of the experimental data of Examples 1 to 3 and Comparative Examples 1 to 4 in Table 3, it can be found that the heat-resistant inner tube material prepared by the present invention has good heat resistance.

[0085] By comparison, the breaking strength of Examples 1 to 3 is significantly greater than that of Comparative Example 2, indicating that the modified siloxane obtained by reacting aminopropyltrimethoxysilane, 2,7-dimethyl-2,4,6-octatriene dialdehyde, and 3.5-di-tert-butyl-4-hydroxybenzylamine has a relatively long chain segment and multiple double bonds on the modified polysilsesquioxane obtained by reacting the modified siloxane with vinyltrimethoxysilane, thereby improving the dispersibility of the modified polysilsesquioxane in rubber and thus improving the internal heat performance of the heat-resistant inner tube material; the breaking strength of Examples 1 to 3 is significantly greater than that of Comparative Example 3, indicating that the thermal stability of the Si-O bond on the modified polysilsesquioxane is higher than that of the CC bond and the CH bond, so the heat-resistant inner tube material obtained by reacting the modified polysilsesquioxane with modified butyl rubber has good heat resistance.

[0086] Test Example 4

[0087] Anti-aging performance: The heat-resistant inner tube materials obtained in each embodiment and the comparative example were aged in a constant temperature aging box at 100°C for 24 hours according to GB / T3512, then taken out and left for 16 hours to test the tensile strength. The results are shown in Table 4.

[0088] Table 4

[0089]

[0090] From the comparison of the experimental data of Examples 1 to 3 and Comparative Examples 1 to 4 in Table 4, it can be found that the heat-resistant inner tube material prepared by the present invention has good anti-aging performance.

[0091] By comparison, the tensile strength of Examples 1 to 3 is significantly greater than that of Comparative Examples 2 to 4, indicating that 3,5-di-tert-butyl-4-hydroxybenzylamine on the modified polysilsesquioxane as a hindered phenol structure can capture free radicals and prevent oxidation reactions caused by free radicals, thereby improving the anti-aging properties of the heat-resistant inner tube material.

[0092] Test Example 5

[0093] Air tightness test: The VAC-2C differential pressure airtightness instrument produced by Jinan Languang Electromechanical Technology Co., Ltd. was used to measure the nitrogen permeability coefficient of the sample. The specific operation is as follows: ① Wipe the surface of the sample with ethanol and dry it, apply vacuum sealing silicone grease evenly on the test cavity, measure the sample thickness and put the sample into the test cavity and close the cavity; ② Open the nitrogen cylinder to adjust the air pressure between 0.4 and 0.5 MPa; ③ Turn on the vacuum pump and the temperature control box, and click on the operating computer to start the test. First, the vacuum pump evacuates the test cavity for about 12 hours to keep the pressure below 25 Pa; ④ After the vacuum time is reached, the nitrogen permeation test is started. When the pressure difference no longer changes with time, it reaches stable penetration. The instrument will automatically terminate the test and calculate the gas permeability coefficient according to the prescribed procedure. The test sample uses a 1mm thick square sheet and the test temperature is 23℃. The results are shown in Table 5.

[0094] Table 5

[0095]

[0096] From the comparison of the experimental data of Examples 1 to 3 and Comparative Examples 1 to 4 in Table 5, it can be found that the heat-resistant inner tube material prepared by the present invention has good air tightness.

[0097] By comparison, the nitrogen permeabilities of Examples 1 to 3 are significantly lower than that of Comparative Example 1, indicating that more double bonds are introduced into the diallyl chlorophosphite on the modified butyl rubber, which improves the cross-linking effect during vulcanization and improves the air tightness of the material; the nitrogen permeabilities of Examples 1 to 3 are significantly lower than that of Comparative Example 2, indicating that the abundant double bonds on the modified polysilsesquioxane enable better cross-linking with the double bonds on the modified butyl rubber during vulcanization, thereby improving the air tightness of the material; the nitrogen permeabilities of Examples 1 to 3 are significantly lower than that of Comparative Example 2, indicating that the modified polysilsesquioxane not only has a good cross-linking effect, but can also act as a filler to play a role of physical barrier, further improving the air tightness of the material.

[0098] The specific implementation methods described above further illustrate the objectives, technical solutions and beneficial effects of the present invention in detail. It should be understood that the above description is only a specific implementation method of the present invention and is not intended to limit the scope of protection of the present invention. Any modifications, equivalent substitutions, improvements, etc. made within the spirit and principles of the present invention should be included in the scope of protection of the present invention.

Claims

1. A method for preparing a heat-resistant inner tube material, characterized in that: The method comprises the following preparation steps: (1) Mix aminopropyltrimethoxysilane, 2,7-dimethyl-2,4,6-octatriene dialdehyde, 3.5-di-tert-butyl-4-hydroxybenzylamine and anhydrous ethanol in a mass ratio of 1: (0.7-0.9): (1-1.4): (15-25), stir at 35-45°C and 400-600 r / min for 3-5 hours, extract and wash the organic phase with dichloromethane for 3-5 times, take the organic phase, and distill under reduced pressure at 50-60°C for 4-6 hours to obtain modified siloxane; (2) Allyl trimethoxysilane, modified siloxane, methyl ethyl ketone and anhydrous methanol are mixed in a mass ratio of 1: (0.2-0.4): (18-22): (3-5), and a 0.1 mol sodium hydroxide aqueous solution (0.05-0.15 times the mass of methyl ethyl ketone) is added dropwise at a rate of 2-4 ml / min at 0°C. After the addition is completed, the reaction is continued for 0.5-1.5 h, and the temperature is raised to 70-80°C and the reaction is continued for 22-26 h. The organic phase is extracted and washed with dichloromethane for 3-5 times, and the organic phase is taken and distilled at 50-60°C under reduced pressure for 4-6 h to obtain modified polysilsesquioxane; (3) Select butyl rubber with a number average molecular weight of 300,000 and an unsaturation degree of 1.9%, mix butyl rubber and n-hexane in a mass ratio of 1:(6-7), stir at 300-400 r / min for 25-35 min at 35-45 °C, add 0.025-0.035 times the mass of butyl rubber m-chloroperbenzoic acid, continue stirring for 45-75 min, adjust the pH to neutral with a 1% mass concentration of sodium hydroxide aqueous solution, and cool to room temperature. , continue stirring for 1.5~2.5h, pour into 80~90℃ hot water and stir for 1~2h, wash with deionized water 3~5 times, dry at 55~65℃ for 3~5h to obtain epoxidized butyl rubber; mix epoxidized butyl rubber and n-hexane in a mass ratio of 1:(6~7), add a 36.5% concentrated hydrochloric acid solution with an equimolar amount of epoxy groups in the epoxidized butyl rubber, and continue stirring for 45~75min. During the process, monitor the ring opening of the epoxy group according to GB / T 4612-2008. After the epoxy group is fully opened, adjust the pH to neutral with a 1% sodium hydroxide aqueous solution, cool to room temperature, continue stirring for 1.5~2.5h, pour into and immerse in anhydrous ethanol, filter after the solid is precipitated, wash the solid with anhydrous ethanol 3~5 times, and dry at 55~65℃ for 3~5h to obtain hydroxylated butyl rubber; (4) Mix hydroxylated butyl rubber, diallyl chlorophosphite, triethanolamine and dimethyl sulfoxide in a mass ratio of 1: (0.7-0.9): (0.2-0.4): (8-12), stir at 80-90°C and 300-400 r / min for 3-5 hours, cool to room temperature, filter, wash the solid with anhydrous ethanol for 3-5 times, and dry at 55-65°C for 3-5 hours to obtain modified butyl rubber; (5) The modified butyl rubber, modified polysilsesquioxane and stearic acid are mixed in a mass ratio of (8-12): 1: 0.025, and mixed on an open mill at 100-120°C for 20-40 min. The roller spacing of the open mill is adjusted to 1-3 mm. At 50-70°C, sulfur is added in an amount of 0.02-0.04 times the mass of the modified butyl rubber. The mixture is triangularly packed 3-5 times, and vulcanized on a flat vulcanizer at 140-160°C and 14-16 MPa for 10-12 h. The mixture is naturally cooled to room temperature and then taken out to obtain a heat-resistant inner tube material.

2. A heat-resistant inner tube material prepared according to the method for preparing a heat-resistant inner tube material according to claim 1.