Soft UV printing ink for shoe curved surface printing and preparation method thereof
By grafting a combination of PEG photoinitiator and other materials, a soft UV ink suitable for shoe curved surface printing is prepared, which solves the problem of low viscosity of existing inks and achieves high viscosity, fast curing and good bending resistance. , suitable for printing on curved surfaces of shoes.
Patent Information
- Application Number
- CN202410949310.1
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Filing Date
- 2024-07-16
- Publication Date
- 2024-10-01
AI Technical Summary
The viscosity of existing UV refractive inks is too low to produce a three-dimensional effect when printing, and it is difficult to maintain appropriate viscosity and curing speed during curved surface printing.
Using a combination of grafted PEG photoinitiator and propoxylated neopentyl glycol diacrylate, epoxy acrylic resin and multifunctional polyurethane acrylate, fillers, defoaming agents and thixotropic agents are added, and prepared by stirring and ultrasonic treatment Create a soft UV printing ink with higher viscosity and suitable curing speed.
The ink achieves high viscosity and rapid curing, is suitable for printing on curved surfaces of shoes, has good hardness and bending resistance, and the preparation process is simple, environmentally friendly, and does not involve toxic solvents.
Smart Images

Figure BDA0004946708570000091 
Figure BDA0004946708570000101
Abstract
Description
Technical Field
[0001] The invention belongs to the technical field of printing, and in particular relates to a soft UV printing ink for printing on curved surfaces of shoes and a preparation method thereof. Background Art
[0002] UV refractive ink is a special type of UV ink, which is mainly used for refractive printing and can produce high-end packaging boxes and decorative paintings. This type of ink requires the substrate to be flat, smooth, and have high light reflectivity when printing, such as mirror gold and silver cardboard, aluminum film, mirror stainless steel, etc. When printing with UV refractive ink, the mesh count of the screen needs to be above 400 to ensure the fineness of the pattern. Curved printing is a printing process on a three-dimensional curved surface, which is widely used in the packaging and identification of various products. This printing method can provide rich visual effects and tactile experience, enhancing the attractiveness of the product and brand recognition.
[0003] CN104530818A discloses a UV screen printing ink, which has high adhesion, scratch resistance, short curing time and good printing effect. However, the viscosity of the UV refractive ink is too low, and the leveling is too fast during printing, which cannot meet the requirements of the three-dimensional effect of the printed paint film. Summary of the invention
[0004] In view of the above problems, the present invention proposes a method for preparing a soft UV printing ink for printing on curved surfaces of shoes, which is characterized by comprising the following steps:
[0005] S01, preparing a photoinitiator grafted with PEG;
[0006] S02, taking propoxylated neopentyl glycol diacrylate, epoxy acrylic resin and multifunctional polyurethane acrylate, adding a photoinitiator, a filler, a defoamer and, mixing, stirring to obtain a soft UV printing ink for printing on curved surfaces of shoes;
[0007] Preferably, the photoinitiator is prepared using isophorone diisocyanate, 2-hydroxy-2-methyl-1-phenyl-1-propanone and PEG as raw materials.
[0008] In some embodiments of the present invention, in S01, isophorone diisocyanate and 2-hydroxy-2-methyl-1-phenyl-1-propanone are taken, a solvent and a catalyst are added, and nitrogen is passed through, and the mixture is heated to 70-85°C, and the reaction is carried out until the -NCO is reduced to a certain level. After cooling to 60°C, PEG is added, and the reaction is carried out until the -NCO is reduced to a certain level. The solvent is removed, precipitated, washed, and dried to obtain a photoinitiator.
[0009] In some embodiments of the present invention, in S01, the solvent is ethyl acetate and the catalyst is dibutyltin dilaurate.
[0010] In some embodiments of the present invention, in S01, the molar ratio of isophorone diisocyanate to 2-hydroxy-2-methyl-1-phenyl-1-propanone is (0.8-1.2):1, and the molar ratio of isophorone diisocyanate to PEG is (1.9-2.1):1;
[0011] Preferably, the molar ratio of isophorone diisocyanate to 2-hydroxy-2-methyl-1-phenyl-1-propanone is 1:1, and the molar ratio of isophorone diisocyanate to PEG is 2:1.
[0012] In some embodiments of the present invention, in S01, before cooling, the reaction is carried out until -NCO is reduced to half of that before the reaction; before terminating the reaction, the reaction is carried out until -NCO is reduced to less than 5% of that before the reaction.
[0013] In some embodiments of the present invention, in S02, the weight ratio of propoxylated neopentyl glycol diacrylate, epoxy acrylic resin and multifunctional polyurethane acrylate is (1-2): (1-2): (1-2), preferably 1:1:1;
[0014] and / or, in S02, 5-10% of the total weight of propoxylated neopentyl glycol diacrylate, epoxy acrylic resin and multifunctional polyurethane acrylate as a photoinitiator, 3-7% of a filler, 0.5-2% of a defoamer and 0.5-2% of a thixotropic agent are added, in terms of weight percentage;
[0015] Preferably, in S02, according to weight percentage, 8% of the total weight of propoxylated neopentyl glycol diacrylate, epoxy acrylic resin and multifunctional polyurethane acrylate is added as a photoinitiator, 5% of a filler, 1% of a defoamer and 1% of a thixotropic agent.
[0016] In some embodiments of the present invention, in S02, the dispersion machine is stirred at 300-600 rpm for 10-30 min, ultrasonic treatment is performed for 20-60 min, and the dispersion machine is stirred at 800-1200 rpm for 20-40 min.
[0017] In some embodiments of the present invention, the molecular weight of the PEG is 4000-8000, preferably 6000.
[0018] In some embodiments of the present invention, the filler is fumed silica or a mixture of nano-titanium oxide, nano-zinc oxide, talc and fumed silica in a weight ratio of (1-2):(1-2):(1-3):(1-2);
[0019] Preferably, the filler is a mixture of nano titanium oxide, nano zinc oxide, talc and fumed silica in a weight ratio of 1:1:(1-3):1.
[0020] In some embodiments of the present invention, the defoaming agent is BYK-052, and the thixotropic agent is BYK-410.
[0021] The second aspect of the present invention is to disclose a soft UV printing ink for printing on curved surfaces of shoes obtained by the preparation method of the first aspect.
[0022] Beneficial effects:
[0023] In the soft UV printing ink for printing on curved surfaces of shoes, the PEG chain segments are grafted by isocyanate in the initiator, so that the hydrogen bonding effect is stronger, the visible light transmittance is greater, and the ink is not easy to turn yellow.
[0024] In some embodiments, the soft UV printing ink for printing on curved surfaces of shoes of the present invention has high viscosity and good curing speed, is suitable for printing on curved surfaces of shoes, and presents a three-dimensional effect. In some embodiments, the soft UV printing ink for printing on curved surfaces of shoes of the present invention not only has good viscosity and curing speed performance, but also has good hardness and bending resistance, good softness, and is suitable for printing on curved surfaces of shoes.
[0025] The preparation method of the soft UV printing ink for printing on curved surfaces of shoes of the present invention is simple, rapid, does not involve toxic solvents, is green and environmentally friendly, and does not require sealing and pressure equipment. The obtained soft UV printing ink for printing on curved surfaces of shoes can be stored for a long time and is stable and good. DETAILED DESCRIPTION
[0026] The following describes the embodiments of the present invention through specific examples, and those skilled in the art can easily understand other advantages and effects of the present invention from the contents disclosed in this specification. The present invention can also be implemented or applied through other different specific embodiments, and the details in this specification can also be modified or changed in various ways based on different viewpoints and applications without departing from the spirit of the present invention.
[0027] Unless otherwise specified, the examples and comparative examples are parallel tests with the same components, component contents, preparation steps and preparation parameters. The amino epoxy acrylic resin has an equivalent weight of 0.015 / 100g and a weight average molecular weight of 720, and the weight average molecular weight of the multifunctional polyurethane acrylate is 12000. The defoamer is BYK-052, and the thixotropic agent is BYK-410. The filler particles are less than 5 μm.
[0028] Example 1
[0029] Preparation method of soft UV printing ink for printing on curved surfaces of shoes
[0030] (1) A photoinitiator was prepared using isophorone diisocyanate, 2-hydroxy-2-methyl-1-phenyl-1-propanone and PEG4000 as raw materials, ethyl acetate as solvent, and dibutyltin dilaurate as catalyst.
[0031] Among them, isophorone diisocyanate and 2-hydroxy-2-methyl-1-phenyl-1-propanone are taken in a molar amount of 1:1, added into a reactor filled with ethyl acetate and dibutyltin dilaurate and purged with nitrogen for 30 minutes, heated to 75°C, and reacted until -NCO is reduced to half of that before the reaction. After cooling to 60°C, PEG4000 with a half molar amount of isophorone diisocyanate is added, reacted until -NCO is reduced to less than 3% before the reaction, evaporated to remove the solvent, and the product was precipitated with ether, washed, and dried to obtain a photoinitiator.
[0032] (2) Neopentyl glycol propoxylate, epoxy acrylic resin and multifunctional polyurethane acrylate were taken in a weight ratio of 1:1:1, and then 8% of a photoinitiator, 5% of fumed silica, 1% of a defoaming agent and 1% of a thixotropic agent were added according to weight percentage, mixed, stirred at 400 rpm for 20 min in a disperser, ultrasonically treated at 200 W for 30 min, and stirred at 1000 rpm for 30 min in a disperser to obtain a soft UV printing ink for printing on curved surfaces of shoes.
[0033] Example 2
[0034] Preparation method of soft UV printing ink for printing on curved surfaces of shoes
[0035] (1) A photoinitiator was prepared using isophorone diisocyanate, 2-hydroxy-2-methyl-1-phenyl-1-propanone and PEG2000 as raw materials, ethyl acetate as solvent, and dibutyltin dilaurate as catalyst.
[0036] Among them, isophorone diisocyanate and 2-hydroxy-2-methyl-1-phenyl-1-propanone are taken in a molar amount of 1:0.9, added into a reactor filled with ethyl acetate and dibutyltin dilaurate and purged with nitrogen for 30 minutes, heated to 75°C, and reacted until -NCO is reduced to half of that before the reaction. After cooling to 60°C, PEG2000 with a half molar amount of isophorone diisocyanate is added, reacted until -NCO is reduced to less than 3% before the reaction, evaporated to remove the solvent, and the product was precipitated with ether, washed, and dried to obtain a photoinitiator.
[0037] (2) Neopentyl glycol propoxylate, epoxy acrylic resin and multifunctional polyurethane acrylate were taken in a weight ratio of 1:1:1, and then 8% of a photoinitiator, 5% of fumed silica, 1% of a defoaming agent and 1% of a thixotropic agent were added according to weight percentage, mixed, stirred at 400 rpm for 20 min in a disperser, ultrasonically treated at 200 W for 30 min, and stirred at 1000 rpm for 30 min in a disperser to obtain a soft UV printing ink for printing on curved surfaces of shoes.
[0038] Example 3
[0039] Preparation method of soft UV printing ink for printing on curved surfaces of shoes
[0040] (1) A photoinitiator was prepared using isophorone diisocyanate, 2-hydroxy-2-methyl-1-phenyl-1-propanone and PEG6000 as raw materials, ethyl acetate as solvent, and dibutyltin dilaurate as catalyst.
[0041] Among them, isophorone diisocyanate and 2-hydroxy-2-methyl-1-phenyl-1-propanone are taken in a molar amount of 1:1.2, added into a reactor filled with ethyl acetate and dibutyltin dilaurate and purged with nitrogen for 30 minutes, heated to 75°C, and reacted until -NCO is reduced to half of that before the reaction. After cooling to 60°C, PEG6000, which is half the molar amount of isophorone diisocyanate, is added to react until -NCO is reduced to less than 3% before the reaction, the solvent is evaporated, the product is precipitated with ether, washed, and dried to obtain a photoinitiator.
[0042] (2) Neopentyl glycol propoxylate, epoxy acrylic resin and multifunctional polyurethane acrylate were taken in a weight ratio of 1:1:1, and then 8% of a photoinitiator, 5% of fumed silica, 1% of a defoaming agent and 1% of a thixotropic agent were added according to weight percentage, mixed, stirred at 400 rpm for 20 min in a disperser, ultrasonically treated at 200 W for 30 min, and stirred at 1000 rpm for 30 min in a disperser to obtain a soft UV printing ink for printing on curved surfaces of shoes.
[0043] Example 4
[0044] Preparation method of soft UV printing ink for printing on curved surfaces of shoes
[0045] (1) A photoinitiator was prepared using isophorone diisocyanate, 2-hydroxy-2-methyl-1-phenyl-1-propanone and PEG4000 as raw materials, ethyl acetate as solvent, and dibutyltin dilaurate as catalyst.
[0046] Among them, isophorone diisocyanate and 2-hydroxy-2-methyl-1-phenyl-1-propanone are taken in a molar amount of 1:1, added into a reactor filled with ethyl acetate and dibutyltin dilaurate and purged with nitrogen for 30 minutes, heated to 75°C, and reacted until -NCO is reduced to half of that before the reaction. After cooling to 60°C, PEG4000 with a half molar amount of isophorone diisocyanate is added, reacted until -NCO is reduced to less than 3% before the reaction, evaporated to remove the solvent, and the product was precipitated with ether, washed, and dried to obtain a photoinitiator.
[0047] (2) Nano titanium oxide, nano zinc oxide, talcum powder and fumed silica are taken in a weight ratio of 1:1:2:1, and mixed evenly to obtain a filler.
[0048] (3) Take propoxylated neopentyl glycol diacrylate, epoxy acrylic resin and multifunctional polyurethane acrylate in a weight ratio of 1:1:1, and then add 8% of photoinitiator, 5% of filler, 1% of defoamer and 1% of thixotropic agent according to weight percentage, mix, stir at 400 rpm in a disperser for 20 minutes, ultrasonically treat at 200 W for 30 minutes, and stir at 1000 rpm in a disperser for 30 minutes to obtain a soft UV printing ink for printing on curved surfaces of shoes.
[0049] Example 5
[0050] Preparation method of soft UV printing ink for printing on curved surfaces of shoes
[0051] (1) A photoinitiator was prepared using isophorone diisocyanate, 2-hydroxy-2-methyl-1-phenyl-1-propanone and PEG4000 as raw materials, ethyl acetate as solvent, and dibutyltin dilaurate as catalyst.
[0052] Among them, isophorone diisocyanate and 2-hydroxy-2-methyl-1-phenyl-1-propanone are taken in a molar amount of 1:1, added into a reactor filled with ethyl acetate and dibutyltin dilaurate and purged with nitrogen for 30 minutes, heated to 75°C, and reacted until -NCO is reduced to half of that before the reaction. After cooling to 60°C, PEG4000 with a half molar amount of isophorone diisocyanate is added, reacted until -NCO is reduced to less than 3% before the reaction, evaporated to remove the solvent, and the product was precipitated with ether, washed, and dried to obtain a photoinitiator.
[0053] (2) Nano titanium oxide, nano zinc oxide, talcum powder and fumed silica are taken in a weight ratio of 1:1:3:1, and mixed evenly to obtain a filler.
[0054] (3) Take propoxylated neopentyl glycol diacrylate, epoxy acrylic resin and multifunctional polyurethane acrylate in a weight ratio of 1:1:1, and then add 8% of photoinitiator, 5% of filler, 1% of defoamer and 1% of thixotropic agent according to weight percentage, mix, stir at 400 rpm in a disperser for 20 minutes, ultrasonically treat at 200 W for 30 minutes, and stir at 1000 rpm in a disperser for 30 minutes to obtain a soft UV printing ink for printing on curved surfaces of shoes.
[0055] Example 6
[0056] Preparation method of soft UV printing ink for printing on curved surfaces of shoes
[0057] (1) A photoinitiator was prepared using isophorone diisocyanate, 2-hydroxy-2-methyl-1-phenyl-1-propanone and PEG4000 as raw materials, ethyl acetate as solvent, and dibutyltin dilaurate as catalyst.
[0058] Among them, isophorone diisocyanate and 2-hydroxy-2-methyl-1-phenyl-1-propanone are taken in a molar amount of 1:1, added into a reactor filled with ethyl acetate and dibutyltin dilaurate and purged with nitrogen for 30 minutes, heated to 75°C, and reacted until -NCO is reduced to half of that before the reaction. After cooling to 60°C, PEG4000 with a half molar amount of isophorone diisocyanate is added, reacted until -NCO is reduced to less than 3% before the reaction, evaporated to remove the solvent, and the product was precipitated with ether, washed, and dried to obtain a photoinitiator.
[0059] (2) Nano titanium oxide, nano zinc oxide, talcum powder and fumed silica are taken in a weight ratio of 1:1:1:1, and mixed evenly to obtain a filler.
[0060] (3) Take propoxylated neopentyl glycol diacrylate, epoxy acrylic resin and multifunctional polyurethane acrylate in a weight ratio of 1:1:1, and then add 8% of photoinitiator, 5% of filler, 1% of defoamer and 1% of thixotropic agent according to weight percentage, mix, stir at 400 rpm in a disperser for 20 minutes, ultrasonically treat at 200 W for 30 minutes, and stir at 1000 rpm in a disperser for 30 minutes to obtain a soft UV printing ink for printing on curved surfaces of shoes.
[0061] Comparative Example 1
[0062] The difference from Example 1 is that when preparing the photoinitiator, isophorone diisocyanate and 2-hydroxy-2-methyl-1-phenyl-1-propanone are taken in a molar ratio of 1.5:1.
[0063] Comparative Example 2
[0064] The difference from Example 4 is that the filler is talc powder and fumed silica in a weight ratio of 1:1.
[0065] Comparative Example 3
[0066] The difference from Example 4 is that the filler is nano titanium oxide and nano zinc oxide in a weight ratio of 1:1.
[0067] Comparative Example 4
[0068] The difference from Example 4 is that after mixing, the disperser is stirred at a rotation speed of 400 rpm for 30 minutes to obtain a soft UV printing ink for printing on curved surfaces of shoes.
[0069] Performance Testing
[0070] The viscosity and curing speed of the UV printing inks obtained in Examples 1-3 and Comparative Example 1 were measured, wherein the viscosity was measured according to the coating viscosity measurement method specified in GB / T1723-1993. The results are shown in Table 1.
[0071] Table 1 Performance test
[0072] <![CDATA[Viscosity / cps · 25 °C -1 > Curing speed / s Example 1 19438 18 Example 2 18908 19 Example 3 21469 20 Comparative Example 1 16488 23
[0073] The results show that compared with comparative example 1, the photoinitiators of examples 1-3 have good compatibility in the ink, uniform distribution, and fast curing speed, among which example 1 is the best. The inks of examples 1-3 have higher viscosity and better curing speed, and are suitable for printing on curved surfaces of shoes to present a three-dimensional effect.
[0074] The ink obtained in Example 1 has poor hardness and bending resistance. Based on Example 1, Examples 4-6 optimize the components and content of the filler. Comparative Examples 2 and 3 are comparative examples.
[0075] Take the UV printing ink obtained in Examples 1, 4, 5, 6 and Comparative Examples 2 and 3, print it on the surface of gold card paper through a 350-mesh screen, and cure it with a 2-kilowatt UV curing instrument. Determine the performance of the refractive ink and the cured film layer, wherein the hardness is tested according to the pencil hardness test method specified in GB / T6739-2006. The viscosity is measured according to the coating viscosity determination method specified in GB / T1723-1993. Bending resistance test, bend 50 times, visually check whether there is any shedding, 5 points for excellent (no visible shedding); 4 points for good, 3 points for better than average, 2 points for average; 1 point for poor, 0 points for too poor (most of it falls off).
[0076] The results are shown in Table 2.
[0077] Table 2 Performance test
[0078]
[0079]
[0080] The results show that, compared with comparative examples 2 and 3, the viscosity and curing speed of the inks of examples 4-6 are slightly improved after optimizing the filler, but the hardness and bending resistance are significantly improved, especially the bending resistance is greatly improved, the softness is good, and it is suitable for printing on curved surfaces of shoes. Among them, example 4 is the best.
[0081] Take the UV printing ink obtained in Example 4 and Comparative Example 4 and store it at room temperature for 6 months. Then print it on the surface of gold card paper through a 350-mesh screen and cure it with a 2-kilowatt UV curing instrument. Determine the performance of the refractive ink and the cured film layer, wherein the hardness is tested according to the pencil hardness test method specified in GB / T6739-2006. The viscosity is measured according to the coating viscosity determination method specified in GB / T1723-1993. Bending resistance test, bend 50 times, visually check whether there is any shedding, 5 points for excellent (no visible shedding); 4 points for good, 3 points for better than average, 2 points for average; 1 point for poor, 0 points for too poor (most of it falls off). The results are shown in Table 3.
[0082] Table 3 Performance test
[0083] <![CDATA[Viscosity / cps · 25°C -1 > Curing speed / s hardness Bending resistance Example 4 20639 16 3H 4.8 Comparative Example 4 20741 17 3H 4.6
[0084] The results show that compared with Example 4, the viscosity, curing speed and hardness of the ink of Comparative Example 4 do not change much, but the bending resistance is significantly reduced, indicating the beneficial effects of high-speed dispersion and ultrasonic treatment during the preparation process.
[0085] The UV printing inks obtained in Examples 1 and 4 and Comparative Examples 1 and 4 were screen printed on the surface of gold card paper with a mesh size of 350, cured with a 2-kilowatt UV curing device, and stored at room temperature for 6 months. The color difference before and after storage was observed and compared. The results showed that there was no significant difference between Examples 1 and 3 and Comparative Example 4, except that Comparative Example 1 turned slightly yellow.
[0086] The preferred specific implementation modes and embodiments of the present invention are described in detail above, but the present invention is not limited to the above implementation modes and embodiments, and various changes can be made within the knowledge scope of those skilled in the art without departing from the concept of the present invention.
Claims
1. A method for preparing a soft UV printing ink for printing on curved surfaces of shoes, characterized in that: The following steps are involved: S01, preparing a photoinitiator grafted with PEG; S02, taking propoxylated neopentyl glycol diacrylate, epoxy acrylic resin and multifunctional polyurethane acrylate, adding a photoinitiator, a filler, a defoamer and, mixing, stirring to obtain a soft UV printing ink for printing on curved surfaces of shoes; Preferably, the photoinitiator is prepared using isophorone diisocyanate, 2-hydroxy-2-methyl-1-phenyl-1-propanone and PEG as raw materials.
2. The method for preparing the soft UV printing ink for printing on curved surfaces of shoes according to claim 1, characterized in that: In S01, isophorone diisocyanate and 2-hydroxy-2-methyl-1-phenyl-1-propanone are added to a mixture containing a solvent and a catalyst, and nitrogen is passed through the mixture, and the mixture is heated to 70-85° C. to react until -NCO is reduced to a certain level, and then cooled to 60° C., PEG is added to react until -NCO is reduced to a certain level, and the solvent is removed, precipitated, washed, and dried to obtain a photoinitiator; And / or, in S01, the solvent is ethyl acetate and the catalyst is dibutyltin dilaurate.
3. The method for preparing the soft UV printing ink for printing on curved surfaces of shoes according to claim 1 or 2, characterized in that: In S01, the molar ratio of isophorone diisocyanate to 2-hydroxy-2-methyl-1-phenyl-1-propanone is (0.8-1.2):1, and the molar ratio of isophorone diisocyanate to PEG is (1.9-2.1):1; Preferably, the molar ratio of isophorone diisocyanate to 2-hydroxy-2-methyl-1-phenyl-1-propanone is 1:1, and the molar ratio of isophorone diisocyanate to PEG is 2:
1.
4. The method for preparing the soft UV printing ink for printing on curved surfaces of shoes according to claims 1-3, characterized in that: In S01, before cooling, the reaction is carried out until -NCO is reduced to half of that before the reaction; before terminating the reaction, the reaction is carried out until -NCO is reduced to less than 5% of that before the reaction.
5. The method for preparing the soft UV printing ink for printing on curved surfaces of shoes according to claims 1-4, characterized in that: In S02, the weight ratio of propoxylated neopentyl glycol diacrylate, epoxy acrylic resin and multifunctional polyurethane acrylate is (1-2): (1-2): (1-2), preferably 1:1:1; and / or, by weight percentage, adding 5-10% of a photoinitiator, 3-7% of a filler, 0.5-2% of a defoamer and 0.5-2% of a thixotropic agent to the total weight of propoxylated neopentyl glycol diacrylate, epoxy acrylic resin and multifunctional polyurethane acrylate; Preferably, in S02, according to weight percentage, 8% of the total weight of propoxylated neopentyl glycol diacrylate, epoxy acrylic resin and multifunctional polyurethane acrylate is added as a photoinitiator, 5% of a filler, 1% of a defoamer and 1% of a thixotropic agent.
6. The method for preparing the soft UV printing ink for printing on curved surfaces of shoes according to claims 1-5, characterized in that: In S02, the dispersion machine is stirred at 300-600 rpm for 10-30 min, ultrasonic treatment is performed for 20-60 min, and the dispersion machine is stirred at 800-1200 rpm for 20-40 min.
7. The method for preparing the soft UV printing ink for printing on curved surfaces of shoes according to claims 1-6, characterized in that: The molecular weight of the PEG is 4000-8000, preferably 6000.
8. The method for preparing the soft UV printing ink for printing on curved surfaces of shoes according to claims 1-7, characterized in that: The filler is fumed silica or a mixture of nano titanium oxide, nano zinc oxide, talcum powder and fumed silica in a weight ratio of (1-2): (1-2): (0.5-5): (1-2); Preferably, the filler is a mixture of nano titanium oxide, nano zinc oxide, talc and fumed silica in a weight ratio of 1:1:(1-3):
1.
9. The method for preparing the soft UV printing ink for printing on curved surfaces of shoes according to claims 1-8, characterized in that: The defoaming agent is BYK-052, and the thixotropic agent is BYK-410.
10. A soft UV printing ink for printing on curved surfaces of shoes obtained according to the preparation method of claims 1-9.
Citation Information
Patent Citations
Preparation method of UV refractive ink for silk-screen printing
CN112239611A
Single-component water-based composite nano-modified PP primer and preparation method thereof
CN115491095A