Quick-drying water-based single-component anticorrosive paint and preparation method thereof
Through the specific proportion compounding and component optimization of water-based styrene-acrylic emulsion and single-component epoxy resin emulsion, the shortcomings of existing water-based anticorrosive paints in terms of drying speed, adhesion and resistance are solved, and fast drying and strong adhesion are achieved. and low-VOC water-based one-component anti-corrosion paint, suitable for a variety of metal substrates.
Patent Information
- Application Number
- CN202310326678.8
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Filing Date
- 2023-03-30
- Publication Date
- 2024-10-01
AI Technical Summary
Existing water-based one-component anti-corrosion paints have deficiencies in drying speed, adhesion, salt spray resistance, water resistance and weather resistance, especially during winter construction, slow drying speed, low hardness, insufficient adhesion and high VOC content problem.
Using a specific proportion of water-based styrene-acrylic emulsion and one-component epoxy resin emulsion, combined with appropriate pH regulators, dispersants, defoaming agents, film-forming aids and other components, rapid film formation and film-forming are achieved through sanding. High adhesion, optimized glass transition temperature (Tg) to improve resistance, and reduced VOC content through optimized components and ratio adjustment.
It achieves rapid drying, improved adhesion to metal substrates, salt spray resistance, water resistance and weather resistance, while reducing VOC content. It is suitable for a variety of substrates and low or normal temperature construction, especially for aluminum materials that are difficult to adhere to.
Smart Images

Figure CN118725658A_ABST
Abstract
Description
Technical Field
[0001] The technology and embodiments of the present invention relate to the field of anti-corrosion paint. Background Art
[0002] In order to strengthen environmental protection, reduce energy consumption and improve production efficiency, more and more manufacturers require metal protective paint to be baked at low temperature or even cured at room temperature before entering the packaging process directly, and can adapt to a variety of substrates, so as to achieve efficient assembly line production operation process. In order to adapt to this efficient production and assembly packaging process of metal equipment, the performance requirements of protective coatings are becoming more and more stringent. They need to achieve fast drying speed, fast hardness increase, excellent adhesion to different substrates, fast drying and no cracking during winter construction, and at the same time meet the requirements of good salt spray resistance, water resistance, weather resistance and environmental friendliness.
[0003] At present, the fast-drying water-based one-component anti-corrosion paints on the market mostly use alkyd resins, pure acrylic resins and epoxy esters as film-forming substances. Water-based alkyd resin anti-corrosion paints have high fullness and dry quickly in summer, but they dry slowly at low temperatures in winter and are difficult to apply. Water-based pure acrylic paints have good weather resistance, are relatively cheap, and dry quickly, but they have the disadvantages of low hardness, insufficient adhesion to metals, and average salt spray resistance. Water-based one-component epoxy ester paints are newly developed one-component water-based paints that have the characteristics of good adhesion, good salt spray resistance, and relatively fast surface drying speed, but they also have the disadvantages of high viscosity, difficulty in application, the need to add drying agents (containing heavy metals and not environmentally friendly) to the formula, and poor weather resistance.
[0004] In addition, in terms of formula composition, in order to achieve quick drying performance, the above-mentioned water-based alkyd resin anti-corrosion paint, water-based pure acrylic paint, and water-based one-component epoxy ester paint are mostly added with highly volatile solvents such as ethanol and isopropanol, so the VOC content in the paint is invisibly high. Summary of the invention
[0005] The embodiment of the present invention provides a technology for making up for the deficiencies of the prior art. The present invention provides a technology for a quick-drying water-based one-component anti-corrosion paint, which achieves fast drying speed, good adhesion to the metal substrate, and at the same time has good salt spray resistance, water resistance and weather resistance as well as low VOC characteristics.
[0006] The present invention is achieved through the following technical solutions:
[0007] A quick-drying water-based one-component anti-corrosion paint, characterized in that it consists of the following components, measured by mass percentage: 40-45% of water-based styrene-acrylic emulsion, 5-15% of water-based one-component epoxy resin emulsion, 0.1-0.5% of pH regulator, 0.5-2.0% of dispersant, 0.02-0.20% of defoamer, 5-20% of pigment filler, 2-5% of film-forming aid, 0.1-0.5% of wetting and leveling agent, 0.2-0.8% of thickener, 0.3-1% of anti-flash rust agent and 0.1-0.3% of color paste, and the rest is deionized water.
[0008] As a preferred solution, the aqueous styrene-acrylic emulsion is an anionic aqueous styrene-acrylate copolymer emulsion, does not contain heavy metals and halogens, does not contain APEO, has a glass transition temperature Tg of 35-40° C., and has a mass solid content of 45-50%.
[0009] As a preferred embodiment, the aqueous one-component epoxy resin emulsion is a one-component epoxy resin emulsion in which the main chain epoxy groups have been completely ring-opened to form hydroxyl groups, does not contain APEO, has a glass transition temperature Tg of 38-42°C, a mass solid content of 37-41%, and a hydroxyl content of 0.2-0.5%.
[0010] The resin emulsion is the main component that determines the performance of the coating. The important feature of the present invention is that a specific styrene acrylic emulsion and a specific one-component epoxy emulsion are selected, and the compounding ratio of the two is specifically "styrene acrylic emulsion: one-component epoxy emulsion = 3:1-9:1".
[0011] The specific styrene-acrylic emulsion is characterized by being an anionic water-based styrene-acrylate copolymer emulsion, having a glass transition temperature Tg of 35-40°C and a mass solid content of 45-50%. If the Tg is too high, the rigidity is strong, the film-forming drying speed is fast, but the toughness is insufficient; if the Tg is too low, the flexibility is good, but the rigidity is insufficient, and the resistance such as salt spray resistance and water resistance will be reduced. Through experimental demonstration, the styrene-acrylic emulsion with Tg=35-40°C selected by the present invention can achieve the best film-forming drying speed and resistance after compounding with a single-component epoxy emulsion.
[0012] The specific one-component epoxy emulsion is characterized by the fact that the main chain epoxy group of the resin emulsion has been completely ring-opened to form more hydroxyl groups, which can form hydrogen bonds with the substrate to the maximum extent and strengthen the adhesion between the coating and the substrate. At the same time, the glass transition temperature Tg is 38-42℃, which is the same as the principle of styrene-acrylic emulsion. The one-component epoxy emulsion under this Tg can achieve the best film-forming drying speed and resistance after compounding with styrene-acrylic emulsion.
[0013] The compounding of the two resin emulsions selected by the present invention is also characterized in that the specific compounding ratio of the two is "styrene acrylic emulsion: single-component epoxy emulsion = 3:1~9:1. According to the principle of polymer structure, although the weather resistance of styrene acrylic emulsion is slightly lower than that of pure acrylic emulsion, it is better in water resistance and alkali resistance. The styrene acrylic emulsion selected by the present invention and the single-component epoxy emulsion can further enhance the adhesion to the substrate, improve the water resistance and alkali resistance of the coating, and improve the salt spray resistance. At the same time, the specific structure and relatively high Tg of the styrene acrylic emulsion can achieve rapid surface drying and actual drying. The compounding of the two can achieve a good complementary effect. Experimental demonstration shows that the optimal compounding ratio is the mass ratio of "styrene acrylic emulsion: single-component epoxy emulsion = 3:1~9:1. Too much styrene acrylic emulsion will damage the corrosion resistance and adhesion of the coating, and too much single-component epoxy emulsion will reduce the quick drying and weather resistance of the coating. The performance data can be referred to the examples and comparative examples.
[0014] As a preferred embodiment, the pH regulator is an alkaline regulator, comprising one or more combinations of N,N-dimethylethanolamine (DMEA), ethanolamine, ethylenediamine, triethanolamine, multifunctional auxiliary agent AMP-95, sodium hydroxide solution, sodium bicarbonate solution, sodium carbonate solution, and 30% by mass ammonia water.
[0015] As a preferred embodiment, the dispersant is one or more of a nonionic wetting dispersant and / or an anionic dispersant, preferably a nonionic wetting dispersant. The nonionic wetting dispersant is a high molecular weight block copolymer solution containing pigment affinity groups, including one or more combinations of BASF's 4585 dispersant, 4560 dispersant, BYK Chemical's BYK190 dispersant, and Evonik Chemical's 755W and 760W dispersants.
[0016] As a preferred solution, the defoamer is a polyether siloxane copolymer emulsion, with an active ingredient of 20%-100%, and includes one or more of the following: Deco 901W, 902W, Fomex 810, Wuhan Longhua Zhengze's 8825, 8835 defoamers, and BYK-019.
[0017] As a preferred embodiment, the pigments and fillers are organic pigments and inorganic pigments and fillers. The organic pigments are organic substances with chromogenic groups of various colors, including phthalocyanine blue, phthalocyanine green, permanent yellow, permanent purple, permanent red and pigments of derived colors; the inorganic pigments and fillers include one or more combinations of natural barium sulfate, precipitated barium sulfate, titanium dioxide, mica powder, wollastonite, heavy calcium carbonate, light calcium carbonate, talc, kaolin, ferrophosphorus powder, aluminum tripolyphosphate, and zinc phosphate.
[0018] As a preferred embodiment, the film-forming aid is a high-boiling point solvent that can reduce the film-forming temperature of the film-forming material, including one or more combinations of alcohol ether film-forming aids propylene glycol methyl ether (PM), dipropylene glycol methyl ether (DPM), dipropylene glycol butyl ether (DPNB), ethylene glycol butyl ether (BCS), diethylene glycol monobutyl ether (DB), ester film-forming materials alcohol ester dodecaned, propylene glycol methyl ether acetate (PMA), and propylene glycol diacetate (PGDA).
[0019] As a preferred embodiment, the wetting and leveling agent is a silicone wetting and leveling agent, including Evonik's Tego410, Wet270, and Dow Chemical's DC501W; an acetylene alcohol wetting agent, including Longhua Zhengze's LZ-457B, Liansheng Chemical's GS-4035, and Evonik's Surfynol 118; and a twin-structured silicone wetting and leveling agent, including one or more combinations of Evonik's Tego 4100, Yueyang Kaimen's GS-194, and Oak Chemical's JC-7000R.
[0020] As a preferred embodiment, the thickener is a nonionic polyurethane associative thickener (HEUR), including low shear thickeners Dow Chemical RM-12W, Bochers Gel 0620, PW25, Wanhua Chemical U605, BYK Chemical BYK425, and / or high shear thickeners Dow Chemical RM-2020, Bochers Gel 0434, one or more combinations thereof.
[0021] As a preferred embodiment, the flash rust preventer is a mixed solution of an organic complex and a polymer compound, including one or more combinations of JD-020, JD-508, JD-538 of Shanghai Jieda, 335A of Jiangxi Longhai, CK34, HY72, HY71, CK35 of Qingdao Enze. The color paste is an inorganic and organic resin-free color paste, including inorganic resin-free color pastes of carbon black paste, iron oxide red paste, iron oxide black paste, and iron oxide green paste, and / or one or more combinations of resin-free organic color pastes obtained by grinding pigment powders of phthalocyanine blue, phthalocyanine green, permanent yellow, permanent purple, permanent red, and their derivative colors.
[0022] The method for preparing the quick-drying water-based one-component anticorrosive paint is characterized by comprising the following steps:
[0023] (1) Add deionized water, pH adjuster, dispersant and defoamer into a container, pre-disperse with mechanical stirring for 5-10 minutes at a speed of 100-500 rpm; then add pigments and fillers one by one while stirring, and mechanically stir and mix for 10-20 minutes after adding. Premix A is obtained.
[0024] (2) Transfer the premixed liquid A to a sand mill and continue sand milling for 20-50 minutes. The filling rate of zirconium oxide beads in the sand mill is 70-85%, and the speed of the sand mill is 1000-3000 rpm. The sand mill can be a vertical, horizontal or basket sand mill. After sand milling, sand mill slurry B is obtained.
[0025] (3) Remove the sand-grinded slurry B and add the water-based styrene acrylic emulsion, water-based one-component epoxy resin emulsion, film-forming aid, wetting and leveling agent, anti-flash rust agent, thickener and remaining deionized water one by one under low-speed stirring. After adding, mechanically stir for 15-45 minutes at a speed of 100-500 rpm. Obtain the blended material and filter it with a 100-200 mesh filter or filter cloth to obtain the finished quick-drying water-based one-component anticorrosive paint.
[0026] The invention has the beneficial effects that the quick-drying water-based one-component anticorrosive paint of the invention adopts a one-component epoxy resin emulsion with strong adhesion and high glass transition temperature Tg and a styrene acrylic emulsion with high glass transition temperature Tg, which can achieve rapid film formation and good adhesion to metal substrates, especially aluminum materials that are difficult to adhere to. Therefore, it has a fast surface drying speed, a fast increase in the hardness of the paint film, and has outstanding adhesion to metal substrates, especially aluminum materials that are difficult to adhere to. It can be fast dried and crack-free during construction in winter, and at the same time has good salt spray resistance, water resistance and weather resistance, as well as extremely low VOC and other performance characteristics, making up for the respective defects of water-based alkyd resin paint, water-based pure acrylic paint and water-based epoxy ester paint.
[0027] The quick-drying water-based one-component anticorrosive paint of the present invention can be applied to the protection of industrial equipment, machine accessories, textile machinery, engineering machinery, etc. of various metal substrates, and is particularly suitable for efficient assembly line production operation processes with quick drying at low or room temperature, and has outstanding adhesion to aluminum substrates that are difficult to adhere to. BRIEF DESCRIPTION OF THE DRAWINGS
[0028] Figure 1 This is a diagram showing the adhesion effect of a quick-drying water-based one-component anticorrosive paint (Example 1) on a metal aluminum substrate;
[0029] Figure 2 This is a rendering of the effect of quick-drying water-based single-component anti-corrosion paint (Example 1) applied to the reducer;
[0030] Figure 3 This is a picture of the effect of the sample after the UV resistance test of the quick-drying water-based single-component anti-corrosion paint (Example 2) for 1000 hours. DETAILED DESCRIPTION
[0031] In order to more clearly illustrate the technical solutions in the embodiments of the present invention, the drawings required for use in the description of the embodiments will be briefly introduced below. Obviously, the drawings described below are only some embodiments of the present invention. For ordinary technicians in this field, other drawings can be obtained based on these drawings without creative work.
[0032] In order to make the purpose, technical scheme and advantages of the present invention clearer, the present invention will be further described in detail below with reference to the accompanying drawings. Obviously, the described embodiments are only part of the embodiments of the present invention, rather than all the embodiments. Based on the embodiments of the present invention, all other embodiments obtained by ordinary technicians in this field without creative work are within the scope of protection of the present invention.
[0033] Example 1 (styrene acrylic emulsion: epoxy emulsion = 4.3:1)
[0034] The quick-drying water-based one-component anti-corrosion paint of this embodiment is composed of the following components: 43% of water-based styrene acrylic emulsion - Baolijia BLJ319, 10% of water-based one-component epoxy resin emulsion DCZ-2020, 0.2% of DMEA, 0.5% of dispersant - BASF 4560, 0.05% of defoamer LZ-8835, 3% of R996 titanium dioxide, 15% of barium sulfate, 0.5% of ultrafine ferrophosphorus powder, 2% of alcohol ester twelve and 1% of DPNB film-forming aid, 0.2% of wetting agent - Yueyang Kaimen GS194, 0.3% of thickener Wanhua U605, 0.5% of anti-flash rust agent - Qingdao Enze CK-34 and 0.2% of carbon black slurry and 0.05% of phthalocyanine blue slurry, and the rest is deionized water.
[0035] The preparation method of the quick-drying water-based one-component anticorrosive paint comprises the following steps:
[0036] (1) Add deionized water, pH adjuster, dispersant and defoamer into a container, pre-disperse with mechanical stirring for 10 minutes at a speed of 300-400 rpm; then add pigments and fillers one by one while stirring, and mechanically stir and mix for 15 minutes after adding. Premix A is obtained.
[0037] (2) Transfer the premixed liquid A to a sand mill and continue sand milling for 30 minutes. The filling rate of zirconium oxide beads in the sand mill is 80%, and the speed of the sand mill is 2000-2500 rpm. The sand mill can be a vertical, horizontal or basket sand mill. After sand milling, sand mill slurry B is obtained.
[0038] (3) Remove the sand-grinded slurry B and add the water-based styrene acrylic emulsion, water-based one-component epoxy resin emulsion, film-forming aid, wetting and leveling agent, anti-flash rust agent, thickener and remaining deionized water one by one under low-speed stirring. After adding, mechanical stirring is carried out for 30 minutes at a speed of 300-400 rpm. The prepared material is filtered through a 100-200 mesh filter or filter cloth to obtain a finished quick-drying water-based one-component anticorrosive paint.
[0039] Test: The coating was sprayed onto standard sandblasted steel and aluminum plates with a film thickness of 40-60um, and the surface drying time and actual drying time were tested. Other samples were dried at room temperature for 168 hours to test salt spray resistance, water resistance, weather resistance and adhesion.
[0040] Combination Figure 1 , shows the adhesion test results of the quick-drying water-based single-component anticorrosive paint Example 1 on the metal aluminum substrate. It can be seen that for the metal aluminum substrate that is difficult to adhere to, the cross-cut adhesion can still reach level 1 at a ratio of styrene acrylic emulsion: epoxy emulsion = 4.3:1.
[0041] Further integration Figure 2 , shows the effect diagram of the quick-drying water-based single-component anti-corrosion paint (Example 1) applied to the reducer. As can be seen from the figure, the quick-drying water-based single-component anti-corrosion paint is applied to the surfaces of samples of various materials and different roughness, such as carbon steel, cast iron, alloy aluminum, etc., and its appearance is uniform and the gloss is high. The hardness and adhesion of the sample surface tested meet the requirements. The data refer to Table 1.
[0042] Example 2 (styrene acrylic emulsion: epoxy emulsion = 9:1)
[0043] The fast-drying water-based one-component anti-corrosion paint in this embodiment is composed of the following components: 45% of water-based styrene acrylic emulsion - Baolijia BLJ319, 5% of water-based one-component epoxy resin emulsion DCZ-2020, 0.3% of AMP-95, 0.8% of dispersant - BYK190, 0.15% of defoaming agent Digao 901W, 5% of R996 titanium dioxide, 20% of wollastonite, 1% of modified aluminum tripolyphosphate, 1.5% of diethylene glycol butyl ether and 1.5% of ethylene glycol butyl ether film-forming aid, 0.5% of wetting agent - Evonik 4100, 0.5% of thickener Dow RM-12W, 1% anti-flash rust agent - Shanghai Jie Da JD-020 and 0.1% of phthalocyanine green, and the rest is deionized water.
[0044] The preparation method of the quick-drying water-based one-component anticorrosive paint comprises the following steps:
[0045] (1) Add deionized water, pH adjuster, dispersant and defoamer into a container, pre-disperse with mechanical stirring for 15 minutes at a speed of 350-500 rpm; then add pigments and fillers one by one while stirring, and mechanically stir and mix for 10 minutes after adding. Premix A is obtained.
[0046] (2) Transfer the premixed liquid A to a sand mill and continue sand milling for 45 minutes. The filling rate of zirconium oxide beads in the sand mill is 80%, and the speed of the sand mill is 2500-3000 rpm. The sand mill can be a vertical, horizontal or basket sand mill. After sand milling, sand mill slurry B is obtained.
[0047] (3) Remove the sand-grinded slurry B and add the water-based styrene acrylic emulsion, water-based one-component epoxy resin emulsion, film-forming aid, wetting and leveling agent, anti-flash rust agent, thickener and remaining deionized water one by one under low-speed stirring. After adding, mechanical stirring is carried out for 45 minutes at a speed of 350-450 rpm. The prepared material is filtered through a 100-200 mesh filter or filter cloth to obtain a finished quick-drying water-based one-component anti-corrosion paint.
[0048] Test: The coating was airless sprayed onto standard sandblasted steel and aluminum plates with a film thickness of 30-50um, and the surface drying time and actual drying time were tested. Other samples were dried at room temperature for 168 hours, and the salt spray resistance, water resistance, weather resistance and adhesion were tested. The performance is shown in Table 1.
[0049] Combination Figure 3 , shows a sample picture of the quick-drying water-based single-component anticorrosive paint (Example 2) after 1000 hours of UV resistance test. The figure shows that the anticorrosive coating of the present invention has good UV aging resistance at this ratio (styrene acrylic emulsion: epoxy emulsion = 9:1). From the comparison between the irradiated area and the covered area in the figure, the color difference of green is larger than that of gray, but both are in a very small range. The color difference DE detected by the colorimeter is less than 3, and the gloss loss detected by the gloss meter is less than 30%.
[0050] Example 3 (styrene acrylic emulsion: epoxy emulsion = 10:1)
[0051] The quick-drying water-based one-component anti-corrosion paint of this embodiment is composed of the following components: 48% of water-based styrene-acrylic emulsion - Baolijia BLJ319, 4.8% of water-based one-component epoxy resin emulsion DCZ-2020, 0.35% of ammonia water (30% by mass), 1% of dispersant - Evonik 760W, 0.2% of defoamer LZ-8825, 8% of R996 titanium dioxide, 18% of wollastonite, 1% of modified aluminum tripolyphosphate, 1% of propylene glycol methyl ether and 2% of ethylene glycol butyl ether film-forming aid, 0.5% of wetting agent - Evonik 270, 0.6% of thickener Wanhua U605, 0.8% of anti-flash rust agent - Qingdao Enze HY72 and 0.1% of carbon black slurry, and the rest is deionized water.
[0052] The preparation method of the quick-drying water-based one-component anticorrosive paint comprises the following steps:
[0053] (1) Add deionized water, pH adjuster, dispersant and defoamer into a container, pre-disperse with mechanical stirring for 15 minutes at a speed of 350-500 rpm; then add pigments and fillers one by one while stirring, and mechanically stir and mix for 10 minutes after adding. Premix A is obtained.
[0054] (2) Transfer the premixed liquid A to a sand mill and continue sand milling for 45 minutes. The filling rate of zirconium oxide beads in the sand mill is 80%, and the speed of the sand mill is 2500-3000 rpm. The sand mill can be a vertical, horizontal or basket sand mill. After sand milling, sand mill slurry B is obtained.
[0055] (3) Remove the sand-grinded slurry B and add the water-based styrene acrylic emulsion, water-based one-component epoxy resin emulsion, film-forming aid, wetting and leveling agent, anti-flash rust agent, thickener and remaining deionized water one by one under low-speed stirring. After adding, mechanical stirring is carried out for 45 minutes at a speed of 350-450 rpm. The prepared material is filtered through a 100-200 mesh filter or filter cloth to obtain a finished quick-drying water-based one-component anti-corrosion paint.
[0056] Test: The coating was airless sprayed onto standard sandblasted steel and aluminum plates with a film thickness of 30-50um, and the surface drying time and actual drying time were tested. Other samples were dried at room temperature for 168 hours, and the salt spray resistance, water resistance, weather resistance and adhesion were tested. The performance is shown in Table 1.
[0057] Table 1 Performance test results of the embodiment
[0058]
[0059]
[0060] Compared with this invention, alkyd resin is currently widely used in the market to prepare fast-drying one-component anti-corrosion paints, such as the "Preparation of Fast-Drying Epoxy-Modified Waterborne Alkyd Resin Coatings" reported by Hunan Xiangjiang Paint Group, authored by Liu Shoubing, Zeng Lihua, Zhang Guliang, and Zhou Liqiong. The literature explains that the primer prepared with epoxy-modified alkyd resin system has improved water resistance and acid and alkali resistance, but the surface drying and actual drying speed are slow, requiring more than 1 hour. In addition, fast-drying and highly anti-corrosion coatings prepared with new epoxy esters are also popular and highly recommended recently, such as the "Preparation and Research of Water-Based Fast-Drying, Environmentally Friendly, Highly Anti-Corrosion Coatings" reported by Guo Kai of Shandong Yili Paint Co., Ltd. The author explains that the water-based anti-corrosion paint prepared with water-based epoxy ester emulsion has the characteristics of fast drying, environmental protection, and good anti-corrosion performance, but its drying speed is still slow and its salt spray resistance is also average.
[0061] At the same time, the use of pure acrylic emulsion and one-component epoxy emulsion to improve quick-drying and corrosion resistance is also a hot topic of research, such as the patent "Low-temperature quick-drying base-surface all-in-one water-based paint and its preparation method" written by Hebei Chenyang Industry and Trade Group Co., Ltd. The inventor provides a low-temperature quick-drying base-surface all-in-one water-based paint and a preparation method thereof, which comprises an anionic one-component epoxy emulsion and a pure acrylic emulsion. By adjusting the formula, its drying speed is improved, and it has good winter construction properties and dries quickly and does not crack during winter construction. The water-based paint produced by it has a very fast drying speed, which can reach 15min to 25min, but its actual drying speed is slow, and there is no mention of its durability, and the hardness improvement speed and adhesion to aluminum are not described.
[0062] The performance of the specific comparative examples is shown in the following table:
[0063] Table 2 Performance test results of comparative examples
[0064]
[0065] Although the preferred embodiments of the present invention have been described, those skilled in the art may make other changes and modifications to these embodiments once they have learned the basic creative concept. Therefore, the appended claims are intended to be interpreted as including the preferred embodiments and all changes and modifications that fall within the scope of the present invention.
[0066] Obviously, those skilled in the art can make various changes and modifications to the present invention without departing from the spirit and scope of the present invention. Thus, if these modifications and variations of the present invention fall within the scope of the claims of the present invention and their equivalents, the present invention is also intended to include these modifications and variations.
Claims
1. A quick-drying water-based one-component anticorrosive paint, characterized in that: The invention comprises the following components by mass percentage: 40-45% of aqueous styrene acrylic emulsion, 5-15% of aqueous one-component epoxy resin emulsion, 0.1-0.5% of pH regulator, 0.5-2.0% of dispersant, 0.02-0.20% of defoamer, 5-20% of pigment and filler, 2-5% of film-forming aid, 0.1-0.5% of wetting and leveling agent, 0.2-0.8% of thickener, 0.3-1% of anti-flash rust agent, 0.1-0.3% of color paste, and deionized water.
2. The anticorrosive paint according to claim 1, characterized in that: The aqueous styrene-acrylic emulsion is an anionic aqueous styrene-acrylate copolymer emulsion, does not contain heavy metals and halogens, does not contain APEO, has a glass transition temperature Tg of 35-40° C., and has a mass solid content of 45-50%.
3. The anticorrosive paint according to claim 1, characterized in that: The water-based one-component epoxy resin emulsion is a one-component epoxy resin emulsion in which the main chain epoxy groups are completely ring-opened to form hydroxyl groups, does not contain APEO, has a glass transition temperature Tg of 38-42° C., a mass solid content of 37-41%, and a hydroxyl content of 0.2-0.5%.
4. The anticorrosive paint according to claim 1, characterized in that: The pH regulator is an alkaline regulator, which includes one or more combinations of N,N-dimethylethanolamine (DMEA), ethanolamine, ethylenediamine, triethanolamine, multifunctional auxiliary agent AMP-95, sodium hydroxide solution, sodium bicarbonate solution, sodium carbonate solution, and 30% by mass ammonia water.
5. The anticorrosive paint according to claim 1, characterized in that: The dispersant is one or more of a nonionic wetting dispersant and / or an anionic dispersant; the nonionic wetting dispersant is a high molecular weight block copolymer solution containing pigment affinity groups, including one or more combinations of BASF's 4585 dispersant, 4560 dispersant, BYK Chemical's BYK190 dispersant, and Evonik Chemical's 755W and 760W dispersants.
6. The anticorrosive paint according to claim 1, characterized in that: The defoamer is a polyether siloxane copolymer emulsion with an active ingredient content of 20%-100%, and comprises a combination of one or more of Dego 901W, 902W, Fomex 810, Wuhan Longhua Zhengze's 8825, 8835 defoamers, and BYK-019.
7. The anticorrosive paint according to claim 1, characterized in that: The color fillers are organic pigments and inorganic color fillers; the organic pigments are organic substances with chromogenic groups of various colors, including phthalocyanine blue, phthalocyanine green, permanent yellow, permanent violet, permanent red and pigments of derived colors; the inorganic color fillers include one or more combinations of natural barium sulfate, precipitated barium sulfate, titanium dioxide, mica powder, wollastonite, heavy calcium carbonate, light calcium carbonate, talc, kaolin, ferrophosphorus powder, aluminum tripolyphosphate, and zinc phosphate.
8. The anticorrosive paint according to claim 1, characterized in that: The film-forming aid is a high-boiling point solvent that can reduce the film-forming temperature of the film-forming material, and includes one or more combinations of alcohol ether film-forming aids propylene glycol methyl ether (PM), dipropylene glycol methyl ether (DPM), dipropylene glycol butyl ether (DPNB), ethylene glycol butyl ether (BCS), diethylene glycol monobutyl ether (DB), ester film-forming materials alcohol ester dodecaned, propylene glycol methyl ether acetate (PMA), and propylene glycol diacetate (PGDA).
9. The anticorrosive paint according to claim 1, characterized in that: The wetting and leveling agent is a silicone wetting and leveling agent, including Evonik's Tego 410, Wet270, and Dow Chemical's DC501W; acetylene alcohol wetting agents include Longhua Zhengze's LZ-457B, Liansheng Chemical's GS-4035, and Evonik's Surfynol 118; and / or a twin-structure silicone wetting and leveling agent, including Evonik's Tego 4100, Yueyang Kaimen's GS-194, and Aoke Chemical's JC-7000R. One or more combinations; the thickener is a non-ionic polyurethane associative thickener (HEUR), including low-shear thickeners Dow Chemical RM-12W, Boshes Gel0620, PW25, Wanhua Chemical U605, BYK Chemical BYK425, and / or high-shear thickeners Dow Chemical RM-2020, Boshes Gel 0434; the flash rust preventer is a mixed solution of an organic complex and a polymer compound, including one or more combinations of JD-020, JD-508, JD-538 of Shanghai Jieda, 335A of Jiangxi Longhai, CK34, HY72, HY71, CK35 of Qingdao Enze. The color paste is an inorganic and organic resin-free color paste, including inorganic resin-free color pastes of carbon black paste, iron oxide red paste, iron oxide black paste, and iron oxide green paste, and / or one or more combinations of resin-free organic color pastes obtained by grinding pigment powders of phthalocyanine blue, phthalocyanine green, permanent yellow, permanent purple, permanent red and their derivative colors.
10. The method for preparing the anticorrosive paint according to claim 1, characterized in that: The following steps are involved: (1) Add deionized water, pH adjuster, dispersant and defoamer into a container, and pre-disperse them by mechanical stirring for 5-10 minutes at a speed of 100-500 rpm; then add pigments and fillers one by one while stirring, and mechanically stir and mix for 10-20 minutes after adding, to obtain premix A; (2) transferring the premixed liquid A into a sand mill and continuing sand milling for 20-50 minutes, wherein the filling rate of zirconium oxide beads in the sand mill is 70-85%, the speed of the sand mill is 1000-3000 rpm, and the sand mill is a vertical, horizontal or basket sand mill. After sand milling, a sand mill slurry B is obtained; (3) Remove the sand-grinded slurry B, add the water-based styrene acrylic emulsion, water-based one-component epoxy resin emulsion, film-forming aid, wetting and leveling agent, anti-flash rust agent, thickener and remaining deionized water one by one under low-speed stirring, and mechanically stir for 15-45 minutes at a speed of 100-500 rpm to obtain a blended material, and filter with a 100-200 mesh filter or filter cloth to obtain a finished quick-drying water-based one-component anti-corrosion paint.
Citation Information
Patent Citations
Single-component epoxy rust inhibiting primer and preparation method thereof
CN106243851A
High-temperature-baking resistant and water-based paint
CN107880654A
Water-soluble paint for rail wagons and preparation method of water-soluble paint
CN110791154A
Water-based single-component epoxy anticorrosive paint for coating automobile plate spring and preparation method thereof
CN111320917A