Preparation method of adhesive and pressure-sensitive adhesive tape

By preparing a cost-effective two-component adhesive, the problems of water seepage, flying materials and residual glue in pressure-sensitive adhesive tapes during semiconductor substrate cutting are solved, and a high peeling force and low-cost adhesive is achieved, which is suitable for semiconductor substrate encapsulation and cutting.

CN118725784APending Publication Date: 2024-10-01SONGTIAN SEMICONDUCTOR MATERIALS TECHNOLOGY (SUZHOU) CO LTD
View PDF 0 Cites 0 Cited by

Patent Information

Application Number
CN202410962438.1
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Filing Date
2024-07-18
Publication Date
2024-10-01

AI Technical Summary

Technical Problem

Existing pressure-sensitive adhesive tapes have insufficient viscosity during the packaging and cutting process of semiconductor substrates, resulting in problems such as water seepage, flying materials and residual glue. The existing improved adhesives only take into account some of the characteristics and fail to comprehensively solve these problems.

Method used

The two-component adhesive is prepared using cost-effective raw materials, and acrylic esters and modified acrylic esters are prepared by adding initiators in multiple steps, and mixed and diluted in a specific ratio to form a high peeling force, no water penetration, and reduce flying materials and Adhesive residue.

Benefits of technology

It achieves high peeling force when cutting semiconductor substrates, avoids water seepage, flying materials and residual glue, and has low raw material cost, making it suitable for large-scale production.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN118725784A_ABST
    Figure CN118725784A_ABST
Patent Text Reader

Abstract

The invention provides a preparation method of an adhesive and an adhesive tape. The preparation method comprises the following steps: preparing acrylics A in a manner of supplementing an initiator in multiple steps, and generating modified acrylics B by carrying out electrophilic reaction on polyisocyanates and hydroxyl groups on polyfunctional groups; the acrylic ester A and the modified acrylic ester B are mixed according to a corresponding proportion and then diluted to 40% of solid content to obtain the adhesive. The adhesive tape realized by the adhesive is resistant to high-speed blade extrusion and high-speed aqueous solution flushing, and has the effects of no adhesive residue, no water seepage and no material flying when being used for packaging and cutting a semiconductor substrate.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The invention belongs to the technical field of acrylates as the main body and mixed modified acrylates, and mainly relates to a pressure-sensitive adhesive tape suitable for semiconductor substrate packaging and cutting, and a preparation method of a corresponding adhesive. Background Art

[0002] At present, for the pressure-sensitive adhesive tape used for semiconductor substrate packaging cutting, the adhesive itself has insufficient viscosity strength and has a certain permeability to water, which leads to water seepage and flying materials along the edges of the cut substrate due to the squeezing of the high-speed blade and the flushing of the high-speed aqueous solution during the semiconductor substrate packaging cutting. Although some improved adhesives have appeared on the market, these improved adhesives only have one of the characteristics of high peeling force, water resistance, and preventing flying materials or residual adhesive. Adhesives that take into account the above-mentioned multiple characteristics are ideal adhesives for pressure-sensitive adhesive tapes used in semiconductor substrate cutting. Summary of the invention

[0003] In order to solve the problems of water seepage, flying materials, and residual adhesive when the existing pressure-sensitive adhesive tape is used for cutting semiconductor substrates, the present invention provides a method for preparing an adhesive and a pressure-sensitive adhesive tape. The adhesive uses high-cost-effective raw materials to achieve a two-component adhesive layer with a large molecular weight and a large peeling force. The pressure-sensitive adhesive tape achieved on this basis can meet the requirements of high peeling force, no water seepage, and reduced flying materials and residual adhesive when used for cutting semiconductor substrates.

[0004] In order to achieve the above-mentioned objectives, the present invention provides a method for preparing an adhesive. The preparation method comprises: preparing acrylate A by adding an initiator in multiple steps, and generating a modified acrylate B by an electrophilic reaction between polyisocyanate and the hydroxyl groups on the multifunctional groups; mixing the acrylate A and the modified acrylate B in corresponding proportions, and diluting the mixture with ethyl acetate to a solid content of 40% to obtain the adhesive. Preferably, the acrylate A and the modified acrylate B are mixed in a ratio of 4:1-5:1. Preferably, the initiator is dimethyl azobisisobutyrate or ethyl acetate.

[0005] The method for preparing the adhesive further includes: preparing a first group of raw materials and a solvent for preparing acrylic ester A according to the following weight percentages, excluding the mass of the solvent. The first group of raw materials includes:

[0006] The weight ratio of the solvent is 20% to 40% of 2-ethylhexyl acrylate, the weight ratio of 20% to 40% of 2-ethylhexyl methacrylate, the weight ratio of n-butyl acrylate is 10% to 30%, the weight ratio of N-vinyl pyrrolidone is 0.3% to 0.5%, the weight ratio of isobornyl acrylate is 0.5% to 2%, the weight ratio of acrylic acid is 1% to 3%, the weight ratio of methyl acrylate is 1% to 3%, and the weight ratio of initiator dimethyl azobisisobutyrate is 0.1% to 0.5%. The solvent is ethyl acetate, and the total weight ratio of ethyl acetate to the first group of raw materials is 5:5-6:4.

[0007] The second group of raw materials for making modified acrylate B is prepared according to the following weight percentages: 0-40% by weight of hexamethylene isocyanate trimer (solid content 70%), 0-40% by weight of 3-isocyanate methylene methyl cyclohexyl isocyanate trimer (solid content 70%), 25%-30% by weight of pentaol triacrylate, 0.01%-0.05% by weight of organotin, 0.01%-0.05% by weight of phenothiazine, 0.01%-0.05% by weight of ethyl acetate, and 0-5% by weight of toluene.

[0008] Furthermore, the method of preparing acrylic ester A by adding initiators in multiple steps includes: putting 75% ethyl acetate of monomers other than acrylic acid in a good ratio into a reactor, taking 2 / 5 initiator and 5% ethyl acetate, stirring them evenly and then putting them into the reactor,

[0009] Pass nitrogen and raise the temperature; start timing after a small reflux occurs for 30 minutes; after reacting at 78°C-82°C for one hour, add 1 / 5 of the initiator, 5% of ethyl acetate and 1 / 3 of acrylic acid for the first time and keep reflux; maintain the reaction temperature at 82°C-85°C for 2 hours, and add 1 / 5 of the initiator, 5% of ethyl acetate and 1 / 3 of acrylic acid after each reaction hour; after the addition is completed, keep the temperature and keep reflux for a preset time to wait for the reaction to be completed; cool down and pass air, and filter out acrylate A.

[0010] Furthermore, the modified acrylate B is produced by electrophilic reaction between polyisocyanate and hydroxyl groups on multifunctional groups, comprising: putting all hexamethylene cyanate trimer and pentaol triacrylate into a reaction kettle, passing air, and heating to 55° C.; taking 1 / 3 of organic tin diluted to 5% by ethyl acetate, stirring evenly, and then putting it into the reaction kettle, heating to 70° C. and starting timing; maintaining the temperature at 70° C., taking 1 / 3 of organic tin diluted to 5% by ethyl acetate, stirring evenly, and then putting it into the reaction kettle twice at intervals of 10 minutes, and keeping reflux; when the timing reaches 120 minutes, adding phenothiazine diluted to 5% by ethyl acetate, and adding the remaining solvent to dilute to 75% solid content; stirring for 1 hour, and filtering out the modified acrylate B.

[0011] Correspondingly, the present invention also provides a pressure-sensitive adhesive tape, which includes a carrier and an adhesive; characterized in that the adhesive is obtained by the above-mentioned adhesive preparation method.

[0012] The adhesive and pressure-sensitive adhesive tape obtained by the technical solution provided by the present invention have large molecular weight and large peeling force, and can effectively avoid water seepage, flying materials and residual adhesive when used for cutting semiconductor substrates; and the production raw material cost is low and has a very high cost performance, so it is suitable for large-scale production and is widely used in the packaging and cutting of semiconductor substrates. BRIEF DESCRIPTION OF THE DRAWINGS

[0013] Figure 1 The present invention is a schematic diagram of the overall process of the method for preparing the adhesive provided by the present invention. DETAILED DESCRIPTION

[0014] The technical solutions in the embodiments of the present invention will be described clearly and completely below in conjunction with the accompanying drawings in the embodiments of the present invention. Obviously, the described embodiments are only some embodiments of the present invention, not all embodiments. Generally, the components of the embodiments of the present invention described and shown in the accompanying drawings here can be arranged and designed in various different configurations.

[0015] like Figure 1 As shown, the preparation method of the adhesive provided by the present invention comprises: preparing acrylate A by adding initiator in multiple steps, and generating modified acrylate B by electrophilic reaction between polyisocyanate and hydroxyl groups on multifunctional groups; mixing the acrylate A and the modified acrylate B in corresponding proportions, and diluting with ethyl acetate to a solid content of 40% to obtain the adhesive.

[0016] To prepare the adhesive, it is necessary to prepare in advance a first group of raw materials and a solvent for preparing acrylate A, and a second group of raw materials for preparing modified acrylate B.

[0017] Wherein, the first group of raw materials (excluding the mass of the solvent) includes: the first group of raw materials for preparing acrylate A are prepared according to the following weight percentages:

[0018] 20% to 40% by weight of 2-ethylhexyl acrylate, 20% to 40% by weight of 2-ethylhexyl methacrylate, 10% to 30% by weight of n-butyl acrylate, 0.3% to 0.5% by weight of N-vinyl pyrrolidone, 0.5% to 2% by weight of isobornyl acrylate, 1% to 3% by weight of acrylic acid, 1% to 3% by weight of methyl acrylate, and 0.1% to 0.5% by weight of initiator dimethyl azobisisobutyrate. The solvent is ethyl acetate, and the total mass ratio of ethyl acetate to the first group of raw materials is 5:5-6:4.

[0019] The second group of raw materials for making modified acrylate B is prepared according to the following weight percentages: 0-40% by weight of hexamethylene isocyanate trimer (solid content 70%), 0-40% by weight of 3-isocyanate methylene methyl cyclohexyl isocyanate trimer (solid content 70%), 25%-30% by weight of pentaol triacrylate, 0.01%-0.05% by weight of organotin, 0.01%-0.05% by weight of phenothiazine, 0.01%-0.05% by weight of ethyl acetate, and 0-5% by weight of toluene.

[0020] After preparing the corresponding raw materials, the preparation of acrylate A is carried out by the following steps:

[0021] S10, put the monomers except acrylic acid in a good ratio and 75% ethyl acetate into the reactor, take 2 / 5 initiator and 5% ethyl acetate (first time), stir evenly and put into the reactor, pass nitrogen (0.2-0.4L / min), and heat up; start timing (0:00) 30 minutes after a small reflux occurs.

[0022] S11, after reacting for 60 minutes at a temperature range of 78°C-82°C, add 1 / 5 of the initiator, 5% of ethyl acetate and 1 / 3 of acrylic acid, stir evenly and put into the reactor, and keep reflux;

[0023] S12, maintaining the reaction temperature at 82°C-85°C for 2 hours, adding 1 / 5 of the initiator, 5% of ethyl acetate and 1 / 3 of acrylic acid after each hour of reaction, and maintaining reflux;

[0024] S13, heat preservation and reflux and then heat preservation for a preset time to wait for the reaction to be completed;

[0025] S14, cooling (40°C-50°C) and letting in air, and filtering out acrylate A.

[0026] The modified acrylate B was prepared by the following steps:

[0027] S20, put all the hexamethylene cyanate trimer and pentaol triacrylate into the reaction kettle, ventilate with air, and raise the temperature to 55°C; take 1 / 3 of the organotin diluted to 5% by ethyl acetate, stir evenly and put it into the reaction kettle, raise the temperature to 70°C, and start timing;

[0028] S21, maintaining the temperature at 70°C, twice in a row, once every 10 minutes, taking 1 / 3 of the organic tin diluted to 5% by ethyl acetate, stirring evenly, and then putting it into the reactor, and maintaining reflux;

[0029] S22. When the timer reaches 120 minutes, add phenothiazine which is diluted to 5% by ethyl acetate, and add the remaining solvent to dilute to 75% solid content; after stirring for 1 hour, filter out the modified acrylate B.

[0030] Correspondingly, the present invention also provides a pressure-sensitive adhesive tape, the tape comprising a carrier and an adhesive, wherein the adhesive is obtained by the above-mentioned adhesive preparation method.

[0031] As shown in Table 1, in Example 1, Example 2, Example 3, Example 4, and Example 5, the amount of each raw material is prepared as shown in Table 1 to prepare acrylate A. The relevant preparation process is carried out according to the preparation method of acrylate A mentioned above: react at 78-82°C for 1 hour to obtain a low viscosity adhesive; then add initiator once every hour within 2 hours, add 3 times in total, and control the reaction at 82-85°C. To make the polymer chain grow further, the water bath temperature is set at 85°C, and after the addition is completed, the temperature is kept at 82-87°C (with reflux) for 4 hours; after the insulation is completed, cool with cooling water, and when the temperature drops to 40-50°C, turn off the nitrogen and turn on the air, stir quickly for 1 hour and filter out the material.

[0032] Table 1. Amount of each material of acrylic ester A (in grams)

[0033]

[0034] As shown in Table 2, in Example 6, Example 7, Example 8, Example 9, and Example 10, the amounts of various raw materials were prepared as shown in Table 2 to prepare modified acrylate B respectively, and the preparation process was carried out according to the steps of preparing modified acrylate B described above.

[0035] Table 2. Amount of raw materials for preparing modified acrylate B (in grams):

[0036]

[0037]

[0038] The acrylate A prepared in the above-mentioned embodiments 1-5 was mixed with the modified acrylate B at a ratio of 4:1 to 5:1 and diluted to a solid content of 40%, to obtain the adhesives of embodiments 1, 2, 3, 4 and 5 shown in Table 3, respectively, with a solid content of 40% and a viscosity of 3000-10000 mPa.s.

[0039] Table 3. Auxiliary material ratio

[0040] name Implementation 1 Implementation 2 Implementation 3 Implementation 4 Implementation 5 adhesive 4.00:1 4.25:1 4.50:1 4.75:1 5.00:1 Curing agent 0.5 0.5 0.5 0.5 0.5 Initiator 0.5 1.5 0.3 0.3 20 Ethyl acetate 1.5 0.5 0.3 0.3 20

[0041] The crosslinking agent in Table 3 is L75 curing agent; the initiator is 184. Add L75, 184 and other additives according to the proportion of the solid content of the adhesive, stir evenly, and apply on the 36um release film. The dry adhesive thickness is 20u. After crosslinking and curing at 120℃ / 3min, adhere to the 150umPO film and mature at 40-55℃ for 24h. Among them, the ratio of adhesive A to adhesive B is 4.75:1. The peeling force is 12-18N before UV, within 20g after UV, and 10-15N in a circular shape. After being attached to the substrate, after cutting test, there is no residual glue, no water seepage, and no flying materials.

[0042] The above description is only an embodiment of the present invention and is not intended to limit the present invention. For those skilled in the art, the present invention may have various modifications and variations. Any modification, equivalent replacement, improvement, etc. made within the spirit and principle of the present invention shall be included in the protection scope of the present invention.

Claims

1. A method for preparing an adhesive, characterized in that: The preparation method comprises: preparing acrylate A by adding initiators in multiple steps, generating modified acrylate B by electrophilic reaction between polyisocyanate and hydroxyl groups on multifunctional groups; mixing the acrylate A and the modified acrylate B in corresponding proportions, and diluting with ethyl acetate to a solid content of 40% to obtain the adhesive.

2. The preparation method according to claim 1, characterized in that The initiator is dimethyl azobisisobutyrate and ethyl acetate.

3. The preparation method according to claim 2, characterized in that: The preparation method also includes: excluding the mass of the solvent, preparing a first group of raw materials and a solvent for making acrylate A according to the following weight percentages; the first group of raw materials includes: 20% to 40% by weight of 2-ethylhexyl acrylate, 20% to 40% by weight of 2-ethylhexyl methacrylate, 10% to 30% by weight of n-butyl acrylate, 0.3% to 0.5% by weight of N-vinyl pyrrolidone, 0.5% to 2% by weight of isobornyl acrylate, 1% to 3% by weight of acrylic acid, 1% to 3% by weight of methyl acrylate, and 0.1% to 0.5% by weight of initiator dimethyl azobisisobutyrate; the solvent is ethyl acetate, and the total mass ratio of ethyl acetate to the first group of raw materials is 5:5-6:

4.

4. The preparation method according to claim 3, characterized in that: The method of preparing acrylic ester A by adding initiators in multiple steps comprises: putting monomers other than acrylic acid and 75% ethyl acetate in a well-proportioned ratio into a reactor, passing nitrogen and heating; after a small reflux occurs, taking 2 / 5 of the initiator and 5% of ethyl acetate, stirring them evenly and then putting them into the reactor, reacting at 78°C-82°C for one hour, adding 1 / 5 of the initiator, 5% of ethyl acetate and 1 / 3 of acrylic acid for the first time; maintaining the reaction temperature at 82°C-85°C for two hours, and adding 1 / 5 of the initiator, 5% of ethyl acetate and 1 / 3 of acrylic acid every one hour of reaction.

5. The preparation method according to claim 4, characterized in that: The second group of raw materials for making modified acrylate B is prepared according to the following weight percentages: 0-40% by weight of hexamethylene isocyanate trimer (solid content 70%), 0-40% by weight of 3-isocyanate methylene methyl cyclohexyl isocyanate trimer (solid content 70%), 25%-30% by weight of pentaol triacrylate, 0.01%-0.05% by weight of organotin, 0.01%-0.05% by weight of phenothiazine, 0.01%-0.05% by weight of ethyl acetate, and 0-5% by weight of toluene.

6. The preparation method according to claim 5, characterized in that: The modified acrylate B is produced by electrophilic reaction between polyisocyanate and hydroxyl groups on multifunctional groups, comprising: putting all hexamethylene cyanate trimer and pentaol triacrylic acid into a reaction kettle, passing air, and heating to 55° C.; taking 1 / 3 of organic tin diluted to 5% by ethyl acetate, stirring evenly, and then putting it into the reaction kettle, heating to 70° C. and starting timing; maintaining the temperature at 70° C., taking 1 / 3 of organic tin diluted to 5% by ethyl acetate, stirring evenly, and then putting it into the reaction kettle twice at intervals of 10 minutes, and keeping reflux; when the timing reaches 120 minutes, adding phenothiazine diluted to 5% by ethyl acetate, and adding the remaining solvent to dilute to 75% solid content; stirring for 1 hour, and filtering out the modified acrylate B.

7. A pressure-sensitive adhesive tape, comprising a carrier and an adhesive; characterized in that: The adhesive is obtained by the preparation method of the adhesive according to any one of claims 1 to 6.