Modified acrylate glue, quantum dot glue solution, preparation method and application

By introducing hydroxyl functional groups during the UV curing process to form a highly dense structure, the modified acrylate glue wraps the quantum dots, solving the problem of fluorescence attenuation caused by the reaction of the quantum dot surface with O2 and H2O, significantly extending the luminescence lifetime and improving the luminescence stability. sex.

CN118725809APending Publication Date: 2024-10-01HEFEI FUNA TECH CO LTD
View PDF 0 Cites 0 Cited by

Patent Information

Application Number
CN202310320534.1
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Filing Date
2023-03-29
Publication Date
2024-10-01

AI Technical Summary

Technical Problem

The existing technology has shortcomings in improving the luminescence stability of quantum dots, especially the fluorescence attenuation problem caused by the reaction between the quantum dot surface and O2 or H2O. The existing polymer substrate has limited blocking ability and cannot effectively extend the quantum dot and its The luminous life of the relevant device.

Method used

Modified acrylate glue is used to introduce hydroxyl functional groups during the UV light curing process to form a highly dense three-dimensional network structure to enhance barrier properties, and the quantum dots are wrapped in this structure to reduce the probability of contact with O2 and H2O .

Benefits of technology

It significantly extends the luminescence life of quantum dots and related components, improves luminescence stability, and enhances the water and oxygen barrier capabilities of the material.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure BDA0004151524120000091
    Figure BDA0004151524120000091
  • Figure BDA0004151524120000101
    Figure BDA0004151524120000101
Patent Text Reader

Abstract

The invention relates to the technical field of quantum dot materials, in particular to modified acrylate glue, a quantum dot glue solution, a preparation method and application. The modified acrylate glue is prepared from the following components in parts by weight: 30 to 50 parts of acrylate oligomer, 10 to 20 parts of hydroxyethyl methylacrylate, 1 to 10 parts of beta-hydroxypropyl methacrylate, 3 to 10 parts of isobornyl methacrylate, 3 to 5 parts of acrylic acid, 1 to 3 parts of 1-hydroxycyclohexyl phenyl ketone and 0.1 to 0.5 part of camphene. According to the modified acrylate glue disclosed by the invention, the acrylate component with hydroxyl is adopted, so that macromolecular chains are crosslinked to form a compact three-dimensional network structure, and the modified acrylate glue is endowed with higher barrier property; the quantum dots are wrapped, so that the probability that the quantum dots make contact with O2 and H2O can be further reduced, and the light-emitting service life of quantum dot components is prolonged.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The invention relates to the technical field of quantum dot materials, and in particular to a modified acrylic ester glue, a quantum dot glue solution, and a preparation method and application thereof. Background Art

[0002] Quantum dots are a nanoscale luminescent display material with advantages such as pure chromaticity and wide color gamut. Due to the large specific surface area of ​​quantum dots, the performance degradation caused by surface defects is very significant. Under certain conditions, the metal atoms on the surface of quantum dots can easily react with O in the external environment. 2 or H 2 O reacts, resulting in the attenuation of the luminescence performance of quantum dots. In recent years, many studies have been devoted to using different methods to passivate the surface of quantum dots to increase the luminescence lifetime of quantum dots in the external environment.

[0003] The quantum dots are coated with a polymer substrate such as polymethyl methacrylate (PMMA) to reduce the contact between the quantum dots and the 2 or H 2 O probability is a feasible passivation method. However, due to the limitation of the barrier capacity of the polymer substrate itself, the fluorescence decay of quantum dots and related devices is still rapid after the polymer substrate is used to coat the quantum dots. Therefore, how to further improve the luminescence stability of quantum dots to meet industry needs is an urgent problem that the industry needs to solve, and it is also the key to the large-scale application of quantum dots in the future.

[0004] In view of this, the present invention is proposed. Summary of the invention

[0005] One object of the present invention is to provide a modified acrylic ester glue having excellent barrier properties and capable of extending the luminescence life of quantum dots and related components.

[0006] Another object of the present invention is to provide a method for preparing the modified acrylate glue.

[0007] Another object of the present invention is to provide a quantum dot glue solution.

[0008] Another object of the present invention is to provide a method for preparing quantum dot colloid solution.

[0009] Another object of the present invention is to provide an application of quantum dot glue solution in the preparation of quantum dot components.

[0010] In order to achieve the above-mentioned purpose of the present invention, the following technical solutions are particularly adopted:

[0011] The modified acrylic ester glue comprises the following components in parts by weight:

[0012] 30-50 parts of acrylate oligomer, 10-20 parts of hydroxyethyl methacrylate, 1-10 parts of beta-hydroxypropyl methacrylate, 3-10 parts of isobornyl methacrylate, 3-5 parts of acrylic acid, 1-3 parts of photoinitiator and 0.1-0.5 parts of camphene.

[0013] The present invention also provides a method for preparing the modified acrylic ester glue, comprising the following steps:

[0014] The components are mixed in a vacuum manner according to proportion to obtain modified acrylic ester glue.

[0015] In a specific embodiment of the present invention, the vacuum glue mixing comprises: -1 Pa, mix at 300-500 rpm for 1-3 min, then at 800-1200 rpm for 5-7 min, and then at 300-500 rpm for 1-3 min.

[0016] The present invention also provides a quantum dot glue solution, comprising the following components in parts by weight:

[0017] 70-90 parts of modified acrylate glue, 1-2 parts of quantum dot powder and 10-30 parts of isobornyl acrylate.

[0018] In a specific embodiment of the present invention, the quantum dot glue solution further includes 2 to 3 parts of a light diffuser and / or 0.5 to 2 parts of an antioxidant.

[0019] The present invention also provides a method for preparing a quantum dot glue solution, comprising the following steps:

[0020] (a) quantum dot powder is mixed with isobornyl acrylate to obtain a quantum dot / IBOA solution;

[0021] (b) The quantum dot / IBOA solution is uniformly mixed with a light diffuser and an antioxidant to obtain a mixture, which is then mixed with modified acrylic glue to obtain a quantum dot glue solution.

[0022] The present invention also provides the use of the quantum dot glue solution in preparing quantum dot components.

[0023] Compared with the prior art, the present invention has the following beneficial effects:

[0024] (1) In the modified acrylic ester glue of the present invention, an acrylic ester component having a hydroxyl group is used. During the UV light curing process, the acrylic ester can not only form a polymer chain through the mutual connection of double bonds, but the introduced hydroxyl functional groups can also interact through hydrogen bonds to further cross-link the polymer chains and form a dense three-dimensional network structure, thereby giving it higher barrier properties;

[0025] (2) The modified acrylate glue of the present invention can be self-crosslinked under UV light and has excellent barrier properties. The use of the modified acrylate glue to wrap quantum dots can further reduce the contact between quantum dots and the surface of the quantum dots. 2 and H 2 O probability, prolong the luminescence life of quantum dot components, etc. DETAILED DESCRIPTION

[0026] The technical scheme of the present invention will be clearly and completely described below in conjunction with specific embodiments, but it will be appreciated by those skilled in the art that the following described embodiments are part of embodiments of the present invention, rather than all embodiments, and are only used to illustrate the present invention, and should not be considered as limiting the scope of the present invention. Based on the embodiments in the present invention, all other embodiments obtained by those of ordinary skill in the art without making creative work, all belong to the scope of protection of the present invention. If specific conditions are not indicated in the embodiments, they are carried out according to normal conditions or conditions recommended by the manufacturer. If the manufacturer is not indicated in the reagents or instruments used, they are all conventional products that can be purchased commercially.

[0027] The modified acrylic ester glue comprises the following components in parts by weight:

[0028] 30-50 parts of acrylate oligomer, 10-20 parts of hydroxyethyl methacrylate, 1-10 parts of beta-hydroxypropyl methacrylate, 3-10 parts of isobornyl methacrylate, 3-5 parts of acrylic acid, 1-3 parts of photoinitiator and 0.1-0.5 parts of camphene.

[0029] Quantum dots will generate photoinduced carriers under the condition of light of a certain wavelength. After the photoinduced carriers are transferred to the surface of quantum dots, there is a certain probability that the O in the environment will be 2 and H 2O is converted into active oxygen. Active oxygen will further react with elements (such as Zn, S, etc.) on the surface of quantum dots to generate corresponding oxides. Since the lattices of these generated oxides do not match the original lattices or are amorphous in themselves, the fluorescence performance of quantum dots will be attenuated. Under UV light irradiation, the double bond structure in the acrylate oligomer can be broken, and then reconnected to each other in the form of CC single bonds to form a polymer chain, and the material can be cured. With the development of microelectronics technology, high-precision electronic components have put forward higher requirements on the water and oxygen barrier ability of materials. In the present invention, an acrylate component with hydroxyl groups is added to the acrylate. During the UV light irradiation and curing process, the acrylate molecules can not only form polymer chains through the mutual connection of double bonds; the newly introduced hydroxyl functional groups can also interact through hydrogen bonds, so that the polymer chains are further cross-linked and form a dense three-dimensional network structure. This highly dense acrylate network structure can give the material higher barrier properties. On this basis, injecting quantum dots into this modified acrylate glue can extend the luminescence life of quantum dots and related components. Camphene in the system can improve the stability of organic matter and prolong the aging decay rate.

[0030] For example, in different embodiments, the dosage of each component in the modified acrylate glue may be as follows:

[0031] The amount of acrylate oligomer can be 30 parts, 32 parts, 34 parts, 35 parts, 36 parts, 38 parts, 40 parts, 42 parts, 44 parts, 45 parts, 46 parts, 48 ​​parts, 50 parts, etc.;

[0032] The amount of hydroxyethyl methacrylate can be 10 parts, 12 parts, 14 parts, 15 parts, 16 parts, 18 parts, 20 parts, etc.;

[0033] The amount of β-hydroxypropyl methacrylate can be 1 part, 2 parts, 3 parts, 4 parts, 5 parts, 6 parts, 7 parts, 8 parts, 9 parts, 10 parts, etc.;

[0034] The amount of isobornyl methacrylate can be 3 parts, 4 parts, 5 parts, 6 parts, 7 parts, 8 parts, 9 parts, 10 parts, etc.;

[0035] The amount of acrylic acid can be 3 parts, 3.5 parts, 4 parts, 4.5 parts, 5 parts, etc.;

[0036] The amount of photoinitiator can be 1 part, 1.5 parts, 2 parts, 2.5 parts, 3 parts, etc.;

[0037] The amount of camphene can be 0.1 part, 0.2 part, 0.3 part, 0.4 part, 0.5 part, etc.

[0038] In a specific embodiment of the present invention, the modified acrylate glue includes the following components in parts by weight: 35-45 parts of acrylate oligomer, 12-18 parts of hydroxyethyl methacrylate, 2-8 parts of β-hydroxypropyl methacrylate, 5-8 parts of isobornyl methacrylate, 3.5-4.5 parts of acrylic acid, 1.5-2.5 parts of photoinitiator and 0.2-0.4 parts of camphene.

[0039] In a specific embodiment of the present invention, the modified acrylate glue includes the following components in parts by weight: 38 to 42 parts of acrylate oligomer, 14 to 16 parts of hydroxyethyl methacrylate, 4 to 6 parts of β-hydroxypropyl methacrylate, 6 to 8 parts of isobornyl methacrylate, 3.8 to 4.2 parts of acrylic acid, 1.8 to 2.2 parts of photoinitiator and 0.2 to 0.4 parts of camphene.

[0040] In a specific embodiment of the present invention, the acrylate oligomer includes a multifunctional acrylate oligomer. Further, the acrylate oligomer includes a multifunctional aliphatic urethane acrylate oligomer.

[0041] In a specific embodiment of the present invention, the acrylate oligomer includes aliphatic polyurethane hexaacrylate oligomer and / or DR-U384. Among them, the aliphatic polyurethane hexaacrylate oligomer is 6150-100, a product of Changxing Materials Industry. 6150-100 has the advantages of good yellowing resistance, good water resistance, fast curing speed, high Tg, etc.; DR-U384 has good yellowing resistance and ultra-high elongation at break.

[0042] In a specific embodiment of the present invention, the acrylate oligomer includes 6150-100 and DR-U384. Further, the mass ratio of the 6150-100 to the DR-U384 is (1-5) : 1, such as (3-4) : 1.

[0043] For example, in different embodiments, the mass ratio of the 6150-100 and the DR-U384 can be 1:1, 1.5:1, 2:1, 2.5:1, 3:1, 3.5:1, 4:1, 4.5:1, 5:1, and the like.

[0044] In a specific embodiment of the present invention, the photoinitiator includes 1-hydroxycyclohexyl phenyl ketone.

[0045] The present invention also provides a method for preparing the modified acrylic ester glue, comprising the following steps:

[0046] The components are mixed in a vacuum manner according to proportion to obtain modified acrylic ester glue.

[0047] In a specific embodiment of the present invention, the vacuum glue mixing comprises:-1 Pa, mix at 300-500 rpm for 1-3 min, then at 800-1200 rpm for 5-7 min, and then at 300-500 rpm for 1-3 min.

[0048] In actual operation, the vacuum glue mixing can be carried out in a vacuum glue mixing machine.

[0049] The present invention also provides a quantum dot glue solution, comprising the following components in parts by weight:

[0050] 70-90 parts of modified acrylate glue, 1-2 parts of quantum dot powder and 10-30 parts of isobornyl acrylate.

[0051] In a specific embodiment of the present invention, the quantum dot powder includes red quantum dots and green quantum dots, and the weight ratio of the red quantum dots to the green quantum dots is 1:(8-10).

[0052] For example, in different embodiments, the weight ratio of the red quantum dots to the green quantum dots can be 1:8, 1:8.5, 1:9, 1:9.5, 1:10, etc.

[0053] In a specific embodiment of the present invention, the quantum dot glue solution further includes 2 to 3 parts of a light diffuser and / or 0.5 to 2 parts of an antioxidant.

[0054] For example, in different embodiments, the dosage of each component in the quantum dot colloid solution may be as follows:

[0055] The amount of modified acrylic glue can be 70 parts, 72 parts, 74 parts, 75 parts, 76 parts, 78 parts, 80 parts, 82 parts, 84 parts, 85 parts, 86 parts, 88 parts, 90 parts, etc.;

[0056] The amount of quantum dot powder can be 1 part, 1.1 parts, 1.2 parts, 1.3 parts, 1.4 parts, 1.5 parts, 1.6 parts, 1.7 parts, 1.8 parts, 1.9 parts, 2 parts, etc.;

[0057] The amount of isobornyl acrylate can be 10 parts, 12 parts, 14 parts, 15 parts, 16 parts, 18 parts, 20 parts, 22 parts, 24 parts, 25 parts, 26 parts, 28 parts, 30 parts, etc.;

[0058] The amount of light diffuser can be 2 parts, 2.2 parts, 2.4 parts, 2.5 parts, 2.6 parts, 2.8 parts, 3 parts, etc.;

[0059] The amount of antioxidant used can be 0.5 parts, 0.6 parts, 0.8 parts, 1 parts, 1.2 parts, 1.4 parts, 1.5 parts, 1.6 parts, 1.8 parts, 2 parts, etc.

[0060] In a specific embodiment of the present invention, the quantum dot glue solution includes the following components by weight: 75-85 parts of modified acrylate glue, 1-2 parts of quantum dot powder and 15-25 parts of isobornyl acrylate, 2.2-2.8 parts of light diffuser and 0.8-1.5 parts of antioxidant.

[0061] In a specific embodiment of the present invention, the quantum dot glue solution includes the following components in parts by weight: 78-82 parts of modified acrylate glue, 1.2-1.8 parts of quantum dot powder and 18-22 parts of isobornyl acrylate, 2.4-2.6 parts of light diffuser and 1-1.5 parts of antioxidant.

[0062] In a specific embodiment of the present invention, the quantum dots are oil phase quantum dots.

[0063] In a specific embodiment of the present invention, the light diffuser includes organic silicon dioxide and / or titanium oxide.

[0064] In a specific embodiment of the present invention, the antioxidant includes antioxidant 626 and / or antioxidant 1010.

[0065] The present invention also provides a method for preparing a quantum dot glue solution, comprising the following steps:

[0066] (a) quantum dot powder is mixed with isobornyl acrylate to obtain a quantum dot / IBOA solution;

[0067] (b) The quantum dot / IBOA solution is uniformly mixed with a light diffuser and an antioxidant to obtain a mixture, which is then mixed with modified acrylic glue and vacuum mixed to obtain a quantum dot glue solution.

[0068] In a specific embodiment of the present invention, the preparation of the quantum dot powder includes: filtering a solution containing oil-phase quantum dots to remove the solvent (n-hexane) to obtain the quantum dot powder.

[0069] In actual operation, the preparation of the quantum dot / IBOA solution includes: adding isobornyl acrylate to the quantum dot powder, and performing ultrasonic treatment to completely dissolve the quantum dot powder to obtain the quantum dot / IBOA solution.

[0070] In a specific embodiment of the present invention, in step (b), the preparation of the mixture comprises: adding a light diffuser and an antioxidant to the quantum dot / IBOA solution, and subjecting the solution to ultrasonic treatment until the solid matter is dissolved to obtain a mixture.

[0071] In a specific embodiment of the present invention, in step (b), the vacuum mixing comprises: -1Pa, mix at 300-500 rpm for 1-3 min, then at 800-1200 rpm for 5-7 min, and then at 300-500 rpm for 1-3 min.

[0072] The present invention also provides the use of the quantum dot glue solution in preparing quantum dot components.

[0073] In a specific embodiment of the present invention, the preparation of the quantum dot device includes:

[0074] The quantum dot glue solution is coated on the surface of the substrate and UV cured under a protective atmosphere.

[0075] In actual operation, the substrate is modified and adjusted according to the requirements of the quantum dot components.

[0076] In a specific embodiment of the present invention, the protective atmosphere may be N 2 .

[0077] In a specific embodiment of the present invention, the UV curing conditions include: using 360-370nm UV light, the radiation intensity is 1800-2200mj / cm 2 .

[0078] For example, 365nm UV light can be used, with a radiation intensity of 2000mj / cm 2 .

[0079] Examples 1 to 5

[0080] This embodiment provides a modified acrylate glue and a preparation method. Specifically, the preparation method of the modified acrylate glue comprises the following steps:

[0081] Take acrylate oligomer, add hydroxyethyl methacrylate, β-hydroxypropyl methacrylate, isobornyl methacrylate, acrylic acid, 1-hydroxycyclohexyl phenyl ketone and camphene, and then mix them evenly in a vacuum glue mixer to obtain modified acrylate glue.

[0082] Among them, the parameters of the vacuum glue mixer are: when the vacuum degree is less than 10 -1 Pa, mixed at 400 rpm for 2 min, then at 1000 rpm for 6 min, and then at 400 rpm for 2 min.

[0083] The component information of the modified acrylate glue of each embodiment is shown in Table 1.

[0084] Table 1 Component information of different modified acrylic ester glues (parts by weight)

[0085]

[0086]

[0087] In each embodiment, the acrylate oligomer is 6150-100 and DR-U384 at a mass ratio of 3:1.

[0088] Embodiments 6 to 9

[0089] Examples 6 to 9 provide modified acrylate glue and preparation methods, with reference to Example 1, except that the acrylate oligomers are different.

[0090] The acrylate oligomer of Example 6 is 6150-100 and DR-U384 in a mass ratio of 5:1;

[0091] The acrylate oligomer of Example 7 is 6150-100 and DR-U384 in a mass ratio of 4:1;

[0092] The acrylate oligomer of Example 8 is 6150-100 and DR-U384 in a mass ratio of 2:1;

[0093] The acrylate oligomer of Example 9 is 6150-100 and DR-U384 in a mass ratio of 1:1.

[0094] Embodiments 10 to 14

[0095] This embodiment provides a quantum dot glue solution and a preparation method. Specifically, the preparation method of the quantum dot glue solution includes the following steps:

[0096] (1) filtering the oil phase quantum dot (n-hexane) solution to remove the n-hexane solvent to obtain quantum dot powder;

[0097] (2) adding isobornyl acrylate to the quantum dot powder and subjecting the quantum dots to complete dissolution by ultrasonic oscillation to obtain a quantum dot / IBOA solution;

[0098] (3) adding organic silicon dioxide, antioxidant 626, antioxidant 1010 and titanium oxide to the quantum dot / IBOA solution, and performing ultrasonic oscillation until all the solid additives are dissolved; then adding modified acrylic glue, performing vacuum mixing, and obtaining quantum dot glue solution.

[0099] Among them, the parameters of vacuum mixing are: when the vacuum degree is less than 10 -1 Pa, mixed at 400 rpm for 2 min, then at 1000 rpm for 6 min, and then at 400 rpm for 2 min.

[0100] The component information of the quantum dot colloid solution of each embodiment is shown in Table 2.

[0101] Table 2 Component information of different quantum dot glue solutions (parts by weight)

[0102]

[0103] The quantum dot powder includes red quantum dots and green quantum dots in a mass ratio of 1:4. The composition of the quantum dot powder is not limited thereto and can be adjusted according to the actual optical properties of the quantum dots.

[0104] Embodiments 15 to 18

[0105] Examples 15 to 18 provide quantum dot glue solutions and preparation methods, with reference to Example 10, except that the modified acrylate glue is different.

[0106] The modified acrylic glue used in Example 15 is prepared in Example 6;

[0107] The modified acrylic ester glue used in Example 16 is prepared in Example 7;

[0108] The modified acrylate glue used in Example 17 is prepared in Example 8;

[0109] The modified acrylic ester glue used in Example 18 is prepared in Example 9.

[0110] Comparative Example 1

[0111] Comparative Example 1 provides a quantum dot glue solution, which specifically refers to the preparation method of Example 10, except that the glue is different.

[0112] The glue used in Comparative Example 1 is the same as that in Example 1, except that camphene is not added.

[0113] Comparative Example 2

[0114] Comparative Example 2 provides a quantum dot glue solution, which specifically refers to the preparation method of Example 10, except that the glue is different.

[0115] The glue used in Comparative Example 2 is the same as that in Example 1, except that: the amount of each component is different;

[0116] The glue used in Comparative Example 2 includes 60 parts of acrylate oligomer, 5 parts of hydroxyethyl methacrylate, 5 parts of β-hydroxypropyl methacrylate, 5 parts of isobornyl methacrylate, 2 parts of acrylic acid, 2 parts of 1-hydroxycyclohexyl phenyl ketone and 0.3 parts of camphene.

[0117] Comparative Example 3

[0118] Comparative Example 3 provides a quantum dot glue solution, which specifically refers to the preparation method of Example 10, except that the glue is different.

[0119] The glue used in Comparative Example 3 is the same as that in Example 1, except that: the amount of each component is different;

[0120] The glue used in Comparative Example 3 includes 25 parts of acrylate oligomer, 25 parts of hydroxyethyl methacrylate, 10 parts of β-hydroxypropyl methacrylate, 10 parts of isobornyl methacrylate, 1 part of acrylic acid, 2 parts of 1-hydroxycyclohexyl phenyl ketone and 0.3 parts of camphene.

[0121] Comparative Example 4

[0122] Comparative Example 4 provides a quantum dot glue solution, which specifically refers to the preparation method of Example 10, except that the glue is different.

[0123] The glue used in Comparative Example 4 is the same as that in Example 1, except that: the amount of each component is different;

[0124] The glue used in Comparative Example 4 includes 40 parts of acrylate oligomer, 27 parts of hydroxyethyl methacrylate, 4 parts of acrylic acid, 2 parts of 1-hydroxycyclohexyl phenyl ketone and 0.3 parts of camphene.

[0125] Comparative Example 5

[0126] Quantum dot / PMMA, the preparation method includes: melting PMMA at high temperature to form a liquid, adding quantum dots into the liquid, and cooling to room temperature. The quantum dots account for 1.5wt% of the final product, and the composition of red quantum dots and green quantum dots in the quantum dots is the same as in Example 10.

[0127] Experimental example

[0128] In order to compare the performance of the quantum dot solutions of different embodiments and comparative examples, the performance of the quantum dot solutions of embodiments 10 to 18 and comparative examples 1 to 4 and the quantum dot / PMMA product of comparative example 5 were tested, and the testing method is as follows.

[0129] Take a 6 cm × 6 cm glass sheet respectively, clean the surface of the glass sheet with ethanol and dry it. Apply the quantum dot glue solutions of Examples 10 to 18 and Comparative Examples 1 to 4 uniformly on the respective glass sheets according to the same coating parameters, and then 2 In the atmosphere, UV curing (365nm UV light, radiation intensity 2000mj / cm 2 ) to obtain the corresponding product.

[0130] Test different products under strong blue light (light intensity of 100mW / cm 2 , peak at 460nm) under irradiation (I / I 0 -1, I is the real-time test fluorescence intensity, I 0 is the initial test fluorescence intensity), and the test results are shown in Table 3.

[0131] Table 3 Fluorescence intensity change rate of different products under strong blue light irradiation conditions

[0132] serial number Irradiate for 50h Irradiation 100h Irradiation 200h Irradiation 300h Irradiation 400h Example 10 7% 3% 1% -4% -8% Embodiment 11 7% 2% 0% -5% -9% Example 12 6% 3% -3% -9% -9% Example 13 4% 2% -4% -8% -10% Embodiment 14 5% 1% -6% -9% -10% Embodiment 15 4% 1% -3% -7% -9% Example 16 4% 3% 0% -1% -4% Embodiment 17 2% 0% -4% -8% -12% Embodiment 18 0% -2% -5% -11 -14% Comparative Example 1 2% 0% -7% -13% -18% Comparative Example 2 1% -1% -6% -14% -20% Comparative Example 3 -1% -3% -8% -13% -19% Comparative Example 4 -3% -8% -11 -14% -21% Comparative Example 5 -11% -25% — — —

[0133] From the above test results, it can be seen that the modified acrylate glue of the present invention can be self-crosslinked under UV light and has excellent barrier properties. The use of it to wrap quantum dots can further reduce the contact between quantum dots and the surface of the quantum dots. 2 and H 2 O probability, extending the luminescence life of quantum dot components.

[0134] Finally, it should be noted that the above embodiments are only used to illustrate the technical solutions of the present invention, rather than to limit it. Although the present invention has been described in detail with reference to the aforementioned embodiments, those skilled in the art should understand that they can still modify the technical solutions described in the aforementioned embodiments, or replace some or all of the technical features therein with equivalents. However, these modifications or replacements do not cause the essence of the corresponding technical solutions to deviate from the scope of the technical solutions of the embodiments of the present invention.

Claims

1. Modified acrylic glue, characterized in that: It includes the following components by weight: 30-50 parts of acrylate oligomer, 10-20 parts of hydroxyethyl methacrylate, 1-10 parts of beta-hydroxypropyl methacrylate, 3-10 parts of isobornyl methacrylate, 3-5 parts of acrylic acid, 1-3 parts of photoinitiator and 0.1-0.5 parts of camphene.

2. The modified acrylic glue according to claim 1, characterized in that: The invention comprises the following components in parts by weight: 35-45 parts of acrylate oligomer, 12-18 parts of hydroxyethyl methacrylate, 2-8 parts of beta-hydroxypropyl methacrylate, 5-8 parts of isobornyl methacrylate, 3.5-4.5 parts of acrylic acid, 1.5-2.5 parts of photoinitiator and 0.2-0.4 parts of camphene.

3. The modified acrylic glue according to claim 1, characterized in that: The invention comprises the following components in parts by weight: 38-42 parts of acrylate oligomer, 14-16 parts of hydroxyethyl methacrylate, 4-6 parts of beta-hydroxypropyl methacrylate, 6-8 parts of isobornyl methacrylate, 3.8-4.2 parts of acrylic acid, 1.8-2.2 parts of photoinitiator and 0.2-0.4 parts of camphene.

4. The modified acrylic glue according to claim 1, characterized in that: The acrylate oligomer includes a multifunctional acrylate oligomer; The photoinitiator includes 1-hydroxycyclohexyl phenyl ketone; Preferably, the acrylate oligomer comprises a multifunctional aliphatic polyurethane acrylate oligomer; Preferably, the acrylate oligomer includes aliphatic polyurethane hexaacrylate oligomer and / or DR-U384.

5. The method for preparing the modified acrylic ester glue according to any one of claims 1 to 4, characterized in that: The steps include: Vacuum-mix the components according to proportion to obtain modified acrylic glue; Preferably, the vacuum mixing comprises: -1 Pa, mix at 300-500 rpm for 1-3 min, then at 800-1200 rpm for 5-7 min, and then at 300-500 rpm for 1-3 min.

6. Quantum dot glue solution, characterized in that: It includes the following components by weight: 70-90 parts of the modified acrylate glue according to any one of claims 1 to 4, 1-2 parts of quantum dot powder and 10-30 parts of isobornyl acrylate; Preferably, it also includes 2 to 3 parts of light diffuser and / or 0.5 to 2 parts of antioxidant; Preferably, the quantum dot powder includes red quantum dots and green quantum dots, and the weight ratio of the red quantum dots to the green quantum dots is 1:(8-10).

7. The quantum dot glue solution according to claim 6, characterized in that: The invention comprises the following components by weight: 75-85 parts of modified acrylate glue, 1-2 parts of quantum dot powder, 15-25 parts of isobornyl acrylate, 2.2-2.8 parts of light diffuser and 0.8-1.5 parts of antioxidant; Preferably, the composition comprises the following components in parts by weight: 78-82 parts of modified acrylate glue, 1.2-1.8 parts of quantum dot powder and 18-22 parts of isobornyl acrylate, 2.4-2.6 parts of light diffuser and 1-1.5 parts of antioxidant.

8. The quantum dot glue solution according to claim 6, characterized in that: The quantum dots are oil phase quantum dots; and / or, the light diffuser comprises organic silicon dioxide and / or titanium oxide; And / or, the antioxidant includes antioxidant 626 and / or antioxidant 1010.

9. The method for preparing the quantum dot glue solution according to any one of claims 6 to 8, characterized in that: The steps include: (a) quantum dot powder is mixed with isobornyl acrylate to obtain a quantum dot / IBOA solution; (b) The quantum dot / IBOA solution is uniformly mixed with a light diffuser and an antioxidant to obtain a mixture, which is then mixed with modified acrylic glue and vacuum mixed to obtain a quantum dot glue solution.

10. Use of the quantum dot glue solution according to any one of claims 6 to 8 in the preparation of quantum dot components; Preferably, the preparation of the quantum dot device includes: The quantum dot glue solution is coated on the surface of the substrate and UV cured under a protective atmosphere.