Composite nanofluid displacement agent and preparation method thereof
By using composite nanofluid displacing agents in shale oil reservoirs, the problem of viscosity reduction of polyacrylamide drag reducing agents in high-temperature, high-salt, and high-shear environments has been solved, and good drag reduction effects and portability have been achieved. Sand capacity, excellent wetting and imbibition oil displacement functions, suitable for fracturing shale oil reservoirs.
Patent Information
- Application Number
- CN202310344290.0
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Filing Date
- 2023-03-31
- Publication Date
- 2024-10-01
AI Technical Summary
Polyacrylamide drag reducing agents are prone to fracture in high temperature, high salt and high shear reservoir environments, resulting in a decrease in viscosity and affecting the drag reduction effect.
A composite nanofluid displacing agent is used. The displacing agent is an emulsion dispersed with composite nanospheres, including polymer nanospheres and silica nanoparticles grown in situ on its surface. The polymer nanospheres and silica nanoparticles are The composite of silicon oxide nanoparticles has the properties of organic and inorganic nanomaterials and is used for fracturing shale oil reservoirs.
It has achieved good drag reduction effect and sand carrying capacity, has little damage to the reservoir, has excellent wettability reversal and imbibition oil displacement functions, can effectively penetrate into the rock, replace the crude oil inside the pore throat, and has good resistance to Temperature and salt tolerance.
Smart Images

Figure BDA0004159075790000151 
Figure BDA0004159075790000161 
Figure BDA0004159075790000162
Abstract
Description
Technical Field
[0001] The invention relates to the field of tight reservoir fracturing, and in particular to a composite nanofluid expelling agent and a preparation method thereof. Background Art
[0002] For shale oil reservoirs, the permeability is very low. In order to obtain industrial oil flow, large-scale volume fracturing is required. Since large-scale volume fracturing requires a large amount of fluid and a high displacement, the fracturing fluid is required to have low friction and low damage properties to increase the pumping displacement, and at the same time have a certain viscosity to improve the sand carrying capacity. At present, the most effective method for hydraulic fracturing of shale oil reservoirs is to use slick water for fracturing. This technology has gradually replaced the traditional guar fracturing fluid and has been applied on a large scale with significant economic benefits.
[0003] The core of slickwater is drag reducer. Currently, the most widely used is polyacrylamide drag reducer, which has a good viscosity-increasing effect and a higher drag reduction rate than guar gum drag reducers. However, in the reservoir environment of high temperature, high salt and high shear, polyacrylamide macromolecules are easily broken into small molecules, resulting in a significant decrease in its viscosity, which in turn affects its drag reduction effect.
[0004] In order to overcome the above-mentioned defects of polyacrylamide drag reducers, the present invention is proposed. Summary of the invention
[0005] The main purpose of the present invention is to provide a composite nanofluid expellant and a preparation method thereof, so as to solve the problem in the prior art that polyacrylamide drag reducers are easily broken into small molecules under high temperature, high salt and high shear reservoir environments, resulting in a significant decrease in their viscosity and affecting the drag reduction effect.
[0006] In order to achieve the above-mentioned purpose, according to the first aspect of the present invention, a composite nanofluid repellent is provided, which is an emulsion in which composite nanomicrospheres are dispersed, and the emulsion comprises an aqueous phase and an oil phase, and the oil phase is dispersed in the aqueous phase in the form of droplets; wherein the composite nanomicrospheres comprise polymer nanomicrospheres and silica nanoparticles grown in situ on the surface of the polymer nanomicrospheres.
[0007] Furthermore, the polymer nanospheres are copolymers of acrylamide and N,N-methylene acrylamide.
[0008] Furthermore, the mass ratio of acrylamide to N,N-methylene acrylamide is (10-16):(0.2-0.8).
[0009] Furthermore, the mass ratio of water to oil phase in the aqueous phase is (25-36):(75-95).
[0010] Furthermore, the D50 of the composite nano-microspheres is 30-60 nm.
[0011] Furthermore, the mass concentration of the composite nano-microspheres is 20% to 30%.
[0012] Furthermore, the emulsion also includes an emulsifier, and the emulsifier is selected from at least one of Span 80, Span 60, OP-10, NP-10 and Tween 80.
[0013] Furthermore, the oil phase is selected from at least one of cyclohexane, white oil or liquid paraffin.
[0014] In order to achieve the above-mentioned purpose, according to the second aspect of the present invention, there is provided a method for preparing a composite nanofluid expelling agent, the preparation method comprising: step S1, dissolving a polymerizable monomer and an initiator in water to obtain an aqueous phase, wherein the polymerizable monomer is a water-soluble monomer; step S2, mixing the aqueous phase with an oil phase to obtain a mixed solution, heating the mixed solution so that the polymerizable monomer undergoes a polymerization reaction under the action of the initiator to form polymer nanospheres, and obtain a polymer nanosphere emulsion; step S3, adding tetraethyl orthosilicate to the polymer nanosphere emulsion to carry out a hydrolysis reaction, and the silicon dioxide nanoparticles generated by the hydrolysis reaction grow in situ on the surface of the polymer nanospheres, and obtain a composite nanofluid expelling agent.
[0015] Furthermore, in step S1, the polymerizable monomers include a first comonomer and a second comonomer, wherein the first comonomer is acrylamide, the second comonomer is N,N-methylene acrylamide, and the initiator is persulfate.
[0016] Furthermore, the initiator is potassium persulfate.
[0017] Furthermore, the mass ratio of the acrylamide, N,N-methylene acrylamide and potassium persulfate is (10-16):(0.2-0.8):(0.2-0.8).
[0018] Furthermore, in step S2, an emulsifier is dispersed in the oil phase, and the mass ratio of the emulsifier to the oil phase is (0.5-1):(75-95).
[0019] Furthermore, the emulsion also includes an emulsifier, and the emulsifier is selected from at least one of Span 80, Span 60, OP-10, NP-10 and Tween 80.
[0020] Furthermore, the emulsifier is selected from at least two of Span 80, Span 60, OP-10, NP-10 or Tween 80, and the HLB of the emulsifier is 3-6.
[0021] Furthermore, the oil phase is selected from at least one of cyclohexane, white oil or liquid paraffin.
[0022] Furthermore, in step S2, the HLB value of the mixed solution is first adjusted to 3-6, and then the temperature is increased to carry out the polymerization reaction.
[0023] Furthermore, the polymerization reaction temperature is 50-80° C., and the time is 2-6 hours.
[0024] Furthermore, the polymerization reaction is carried out under the protection of an inert gas.
[0025] Furthermore, the mass ratio of water in the aqueous phase to the oil phase is (25-36):(75-95).
[0026] Furthermore, the mass ratio of acrylamide to oil phase is (10-16):(75-95).
[0027] Furthermore, the step S2 further comprises: after the polymerization reaction is completed, adjusting the HLB value of the system to 10-15 to obtain a polymer nanosphere emulsion.
[0028] Furthermore, in step S3, tetraethyl orthosilicate is first dispersed in a mixed solvent of ethanol and water to obtain a dispersion of tetraethyl orthosilicate, and then the dispersion of tetraethyl orthosilicate is added to the polymer nanosphere emulsion for hydrolysis reaction.
[0029] Furthermore, the volume ratio of ethanol to water in the mixed solvent is (3-5):(5-7).
[0030] Furthermore, the mass ratio of tetraethyl orthosilicate to the mixed solvent is 1:(2-4).
[0031] Furthermore, the mass ratio of tetraethyl orthosilicate dispersion to polymer nanosphere emulsion is (3-5):10.
[0032] Furthermore, the hydrolysis reaction is carried out under the action of a catalyst.
[0033] Furthermore, the catalyst is selected from at least one of diethanolamine and ammonia water.
[0034] Furthermore, the mass concentration of the ammonia water is 20-30%.
[0035] Furthermore, the mass ratio of the catalyst to tetraethyl orthosilicate is (2-30):(5-10).
[0036] Furthermore, the temperature of the hydrolysis reaction is 10-40° C., and the time is 4-6 hours.
[0037] Furthermore, the composite nanofluid displacement agent prepared by the above method is used as an imbibition oil displacement agent or a slick water displacement agent in a tight reservoir.
[0038] By applying the technical solution of the present application, the composite nanofluid displacement agent provided by the present application combines polymer nano-microspheres and silica nano-particles, and has the properties of both organic and inorganic nano-materials, and can be used for shale oil reservoir fracturing. It not only has good drag reduction effect and sand carrying capacity, and causes little damage to the reservoir, but also has excellent wettability reversal and imbibition oil displacement function, and can effectively penetrate into the rock and replace the crude oil inside the pore throat, and also has good temperature and salt resistance. DETAILED DESCRIPTION
[0039] It should be noted that, in the absence of conflict, the embodiments and features in the embodiments of the present application can be combined with each other. The present invention will be described in detail below in conjunction with the embodiments.
[0040] As analyzed in the background technology of this application, although the currently widely used polyacrylamide drag reducer has a good viscosity-increasing effect and a drag reduction rate higher than that of guar gum drag reducers, under high temperature, high salt and high shear reservoir environments, polyacrylamide macromolecules are easily broken into small molecules, resulting in a significant decrease in its viscosity, thereby affecting its drag reduction effect. In order to solve this problem, this application provides a composite nanofluid displacement agent and a preparation method thereof.
[0041] In the first typical embodiment of the present application, a composite nanofluid expellant is provided. The composite nanofluid expellant is an emulsion in which composite nanospheres are dispersed. The emulsion includes an aqueous phase and an oil phase, and the oil phase is dispersed in the aqueous phase in the form of droplets. The composite nanospheres include polymer nanospheres and silica particles grown in situ on the surface of the polymer nanospheres.
[0042] In the present application, the silica nanoparticles not only have good wettability reversal and imbibition oil displacement performance, but also have good drag reduction performance. The polymer nanospheres have good drag reduction performance, and have very good injection performance and sand carrying performance. The composite nanofluid displacement agent provided in the present application is a composite of polymer nanospheres and silica nanoparticles, and has the performance of both organic and inorganic nanomaterials, and can be used for shale oil reservoir fracturing. It not only has good drag reduction effect and sand carrying capacity, and has little damage to the reservoir, but also has excellent wettability reversal and imbibition oil displacement function, can effectively penetrate into the rock, replace the crude oil inside the pore throat, and also has good temperature and salt resistance.
[0043] In order to further improve the thickening effect of the composite nanofluid displacement agent, the polymer nanospheres are preferably copolymers of acrylic acid and N,N-methylene acrylamide, especially when the particle size of the polymer nanospheres is 30-60 nm, the polymer nanospheres are more evenly dispersed in the emulsion and have a better thickening effect.
[0044] In order to further improve the uniformity of dispersion of the polymer nanospheres in the emulsion, the mass ratio of acrylamide to N,N-methylene acrylamide is preferably (10-16):(0.2-0.8).
[0045] Typically but not limiting, the mass ratio of acrylamide to N,N-methyleneacrylamide is 10:0.2, 10:0.5, 10:0.8, 12:0.2, 12:0.5, 12:0.8, 15:0.2, 15:0.5, 15:0.8 or a range consisting of any two of these values.
[0046] In order to further improve the dispersion stability of the composite nano-microspheres in the emulsion, the mass ratio of water to oil phase in the aqueous phase is preferably (25-36):(75-95).
[0047] Typically but not limiting, the weight of water and oil phases is 25:75, 28:75, 30:75, 32:75, 35:75, 25:80, 28:80, 30:80, 32:60, 35:80, 25:80, 28:80, 30:80, 32:95, 35:95 or a range consisting of any two of these values.
[0048] In order to further improve the viscosity-increasing and drag-reducing effect of the composite nanofluid displacement agent, the D50 of the composite nanomicrospheres is preferably 30 to 60 nm, such as 30 nm, 35 nm, 40 nm, 45 nm, 50 nm, 55 nm, 60 nm or a range consisting of any two values.
[0049] In order to further improve the dispersion stability of the composite nano-microspheres in the emulsion, the mass concentration of the composite nano-microspheres is preferably 20% to 30%, such as 20%, 22%, 25%, 28%, 30% or a range consisting of any two values.
[0050] In order to further improve the dispersion effect of the emulsion on the composite nanospheres, it is preferred that the emulsion also includes an emulsifier. The specific type of the emulsifier is not specifically limited, including but not limited to any one of Pan 80, Span 60, OP-10, NP-10 or Tween 80, or a mixture of two or more emulsifiers.
[0051] The specific type of the oil phase is not specifically limited, and any organic solvent commonly used in the art can be used. From the perspective of increasing the content of composite nano-microspheres, cyclohexane, white oil or liquid paraffin, or a mixed solvent of at least two of them, is preferred.
[0052] In a second typical embodiment of the present application, a method for preparing a composite nanofluid expellant is also provided, and the preparation method comprises: step S1, dissolving a first comonomer, a second comonomer and an initiator in water to obtain an aqueous phase, wherein the polymerized monomer is a water-soluble monomer; step S2, mixing the aqueous phase with an oil phase to obtain a mixed solution, heating the mixed solution so that the polymerized monomer undergoes a polymerization reaction under the action of the initiator to generate polymer nanospheres, and obtain a polymer nanosphere emulsion; step S4, adding tetraethyl orthosilicate to the polymer nanosphere emulsion for a hydrolysis reaction, and the silica nanoparticles generated by the hydrolysis reaction are in situ grown on the surface of the polymer nanospheres, to obtain a composite nanofluid expellant.
[0053] The preparation method of the composite nanofluid displacement agent provided in the present application comprises the steps of first dispersing the polymerization monomer and the initiator in the aqueous phase, dispersing the aqueous phase in the oil phase and then initiating polymerization, thereby facilitating the generation of polymer nanospheres with uniform and stably dispersed particle sizes, and subsequently adding tetraethyl orthosilicate to the amphiphilic polymer nanosphere emulsion for hydrolysis reaction, so that the silicon dioxide nanoparticles generated by the hydrolysis reaction are uniformly grown in situ on the surface of the polymer nanospheres, thereby making the prepared composite nanofluid displacement agent stable in performance and being used for shale oil reservoir fracturing. It not only has good drag reduction effect and sand carrying capacity, and causes little damage to the reservoir, but also has excellent wettability reversal and imbibition oil displacement functions, can effectively penetrate into the rock, displace the crude oil inside the pore throat, and also has good temperature and salt resistance.
[0054] In order to further improve the viscosity-increasing effect of the polymer nanospheres, preferably in step S1, the polymerization monomers include a first comonomer and a second comonomer, the first comonomer is acrylamide, the second comonomer is N,N-methylene acrylamide, and the initiator is a persulfate, preferably potassium persulfate, to prepare polymer nanospheres formed by copolymerization of acrylamide and N,N-methylene acrylamide.
[0055] In order to further prepare polymer nanospheres with moderate number average molecular weight and uniform particle size distribution, the mass ratio of acrylamide, N,N-methylene acrylamide and potassium persulfate is preferably (10-16):(0.2-0.8):(0.2-0.8).
[0056] Typically but not limiting, the mass ratio of acrylamide to N,N-methyleneacrylamide and potassium persulfate is, for example, 10:0.2, 10:0.5, 10:0.8, 12:0.2, 12:0.5, 12:0.8, 15:0.2, 15:0.5, 15:0.8 or a range consisting of any two values; the mass ratio of acrylamide to potassium persulfate is, for example, 10:0.2, 10:0.5, 10:0.8, 12:0.2, 12:0.5, 12:0.8, 15:0.2, 15:0.5, 15:0.8 or a range consisting of any two values.
[0057] In the above step S1, in order to facilitate uniform dispersion of the water phase in the oil phase, an emulsifier is preferably dispersed in the oil phase, and the mass ratio of the emulsifier to the oil phase is (0.5-1):(75-95).
[0058] Typically, but not limiting, the mass ratio of emulsifier to oil phase is 0.5:75, 0.5:78, 0.5:80, 0.5:85, 0.5:95, 0.8:75, 0.8:80, 0.8:85, 0.8:90, 0.8:95, 1:75, 1:80, 1:85, 1:90, 1:95 or a range consisting of any two values.
[0059] The specific type of the above emulsifier is not specifically limited, and any commonly used emulsifier in the art can be used, including but not limited to any one of Span 80, Span 60, OP-10, NP-10 or Tween 80, or a mixture of two or more emulsifiers. When the emulsifier is a mixture of two or more emulsifiers, its HLB value is 3 to 6 to further enhance the emulsion polymerization effect.
[0060] The specific type of the oil phase is not specifically limited, and any organic solvent commonly used in the art can be used. From the perspective of increasing the content of composite nano-microspheres, cyclohexane, white oil or liquid paraffin, or a mixed solvent of at least two of them, is preferred.
[0061] In order to facilitate the generation of polymer nanospheres with uniform particle sizes, preferably step S2 includes: firstly adjusting the HLB value of the mixed solution formed by mixing the water phase and the oil phase to 3-6, and then heating the mixed solution to perform a polymerization reaction.
[0062] In order to further improve the efficiency of the polymerization reaction, the polymerization reaction temperature is 50-80° C. and the time is 2-4 hours. Especially when the polymerization reaction is carried out under the protection of an inert gas, the polymerization reaction efficiency is higher.
[0063] Typically but not limiting, the polymerization temperature is 50°C, 55°C, 60°C, 65°C, 70°C, 75°C, 80°C or any range of two values; the polymerization time is 2h, 2.5h, 3h, 3.5h, 4h or any range of two values. The above-mentioned inert gas includes but is not limited to nitrogen, argon or helium.
[0064] In order to facilitate the control of the dispersion of the water phase in the oil phase, the mass ratio of water in the water phase to the oil phase is preferably (25-36):(75-95).
[0065] In order to further improve the dispersion uniformity of the generated polymer nanospheres in the emulsion formed by mixing the oil phase and water, the mass ratio of acrylamide to the oil phase is preferably (10-16):(75-95).
[0066] Typically but not limiting, the weight ratio of water to oil phase in the aqueous phase is, for example, 25:75, 25:80, 25:85, 25:95, 30:75, 30:85, 30:95, 35:75, 35:85, 35:90 or a range consisting of any two values; the weight ratio of acrylamide to oil phase is, for example, 10:75, 12:85, 15:95, 10:75, 12:85, 15:95, 15:75, 15:85, 15:95 or a range consisting of any two values.
[0067] In order to further improve the hydrophilicity of the generated polymer nanoemulsion, after the polymerization reaction is completed, the HLB value of the system is adjusted to 10-15, so that the emulsion is converted into an oil-in-water system to obtain a polymer nanosphere emulsion with an HLB value of 10-15.
[0068] In order to further improve the efficiency of the hydrolysis reaction, preferably, in step S3, tetraethyl orthosilicate is first dispersed in a mixed solvent of ethanol and water to obtain a dispersion of tetraethyl orthosilicate, and then the dispersion of tetraethyl orthosilicate is added to the polymer nanosphere emulsion. Preferably, the volume ratio of ethanol and water in the mixed solvent is (2-5): (5-8) to facilitate the rapid dispersion of tetraethyl orthosilicate. Preferably, the mass ratio of tetraethyl orthosilicate to the mixed solvent is 1: (2-4), and the mass ratio of tetraethyl orthosilicate dispersion to polymer nanosphere emulsion is (3-5): 10 to further improve the efficiency of tetraethyl orthosilicate in situ generation of silicon dioxide.
[0069] Typically but not limiting, the volume ratio of ethanol to water in the mixed solution is 3:7, 4:6, 5:5. The mass ratio of tetraethyl orthosilicate to the mixed solvent is 1:2, 1:3, 1:4; the mass ratio of tetraethyl orthosilicate to the polymer nanosphere emulsion is 3:10, 4:10, 5:10 or a range of any two values.
[0070] In order to further improve the efficiency of the hydrolysis reaction, the hydrolysis reaction is preferably carried out under the action of a catalyst. The specific type of the catalyst is not specifically limited, and any catalyst commonly used in the art can be used, including but not limited to any one or both of diethanolamine or ammonia water, wherein the mass concentration of ammonia water is preferably 20-30%.
[0071] In order to promote the complete hydrolysis of ethyl tetrasilicate and further improve the hydrolysis reaction efficiency, the hydrolysis reaction temperature is preferably 10 to 30° C. and the time is 4 to 6 hours.
[0072] Typically but not limiting, the temperature of the hydrolysis reaction is 10°C, 15°C, 20°C, 25°C, 30°C or a range consisting of any two values; the time of the hydrolysis reaction is 4h, 4.5h, 5h, 5.5h, 6h or a range consisting of any two values.
[0073] In order to reduce the waste of catalyst while ensuring the catalytic efficiency, the mass ratio of catalyst to tetraethyl orthosilicate is preferably (2-30):(5-10).
[0074] Typically but not limiting, the mass ratio of catalyst to tetraethyl orthosilicate is 2:5, 2:8, 2:10, 5:5, 5:8, 5:10, 10:5, 10:8, 15:5, 15:8, 15:10, 20:5, 20:8, 20:10, 30:5, 30:8 or a range consisting of any two values.
[0075] In some embodiments of the present application, the composite nanofluid repellent is prepared according to the following steps:
[0076] (1) dissolving the emulsifier in the oil phase, stirring at a speed of 350 r / min for 30 min to obtain an emulsified oil phase;
[0077] (2) dissolving acrylamide, N,N-methylene acrylamide, and potassium persulfate in deionized water to obtain an aqueous phase;
[0078] (3) At a stirring speed of 350 r / min, the aqueous phase was dripped into the emulsified oil phase to obtain a stable emulsion. After the HLB value was adjusted to 5 using NH4OH, stirring was continued for 30 min to form a stable emulsion. The temperature was then raised to the reaction temperature and reacted for a certain period of time under N2 protection. The HLB value of the emulsion system was then adjusted to 12 to obtain a water-in-oil emulsion-like polymer nanosphere emulsion.
[0079] (4) Tetraethyl orthosilicate is first added to a mixed solvent of ethanol and water to obtain a dispersion of tetraethyl orthosilicate, and then the dispersion of tetraethyl orthosilicate is added to a polymer nanosphere emulsion for hydrolysis reaction, and then a catalyst is added for hydrolysis. After reacting at room temperature for 4 to 6 hours, the silica nanoparticles generated by hydrolysis grow in situ on the active sites on the surface of the polymer microspheres, thereby obtaining a composite nanofluid expelling agent.
[0080] In the third typical embodiment of the present application, the present application also provides the use of any composite nanofluid displacement agent provided in the above-mentioned first typical embodiment or a composite nanofluid displacement agent obtained by any preparation method provided in the above-mentioned second typical embodiment as an imbibition oil displacement agent or for displacing slick water in tight reservoirs.
[0081] When the composite nanofluid displacement agent provided in the present application is configured into a solution with a mass concentration of 0.1 to 0.3 wt% as an imbibition oil displacement agent, the surface tension is less than 30 mN / m, the interfacial tension is less than 0.1 mN / m, the rock surface can be transformed from oil-wetting to hydrophilic wetting, and the imbibition oil washing efficiency can reach 10 to 20%.
[0082] The composite nanofluid displacement agent provided in the present application is configured into a solution with a mass concentration of 0.05-0.2wt% as displacement slip water, with a viscosity of 5-15mPa·s, a drag reduction rate of more than 70%, and good temperature and salt resistance.
[0083] The beneficial effects of the present application will be further illustrated below in combination with embodiments and comparative examples.
[0084] The chemical reagents used in the following examples and comparative examples, such as acrylamide, potassium persulfate, N,N-methylene acrylamide, ammonia (25 wt%), emulsifiers such as Span 80, cyclohexane, white oil, liquid paraffin, tetraethyl orthosilicate, and diethanolamine, were all purchased from Sinopharm Group.
[0085] Example 1
[0086] This embodiment provides a composite nanofluid repellent, which is prepared according to the following steps:
[0087] (1) Dissolve 0.3 g of Span 80 and 0.1 g of Tween 80 in 40 mL of white oil and stir at a speed of 350 r / min for 30 min to obtain an emulsified oil phase;
[0088] (2) dissolving 7 g of acrylamide, 0.15 g of N,N-methylene acrylamide, and 0.14 g of potassium persulfate in 15 mL of deionized water to obtain an aqueous phase;
[0089] (3) At a stirring speed of 350 r / min, the water phase was dripped into the emulsified oil phase to obtain a stable emulsion, and the HLB value was adjusted to 5 with NH4OH, and the stirring was continued for 30 min to form a stable emulsion, and then the temperature was raised to 75°C, and acrylamide and N,N-methylene acrylamide were polymerized under N2 protection for 4 h, and the HLB value of the emulsion system was adjusted to 12 to obtain a water-in-oil emulsion liquid polymer nanosphere emulsion;
[0090] (4) First, 1 g of tetraethyl orthosilicate was added to a mixed solvent of 2 g of ethanol and water, wherein the volume ratio of ethanol to water was 5:5, to obtain a tetraethyl orthosilicate dispersion. The tetraethyl orthosilicate dispersion was then added to 10 g of a polymer nanosphere emulsion, and then 0.5 g of diethanolamine was added for catalytic hydrolysis. After reacting at room temperature for 4 h, the silica nanoparticles generated by the hydrolysis reaction were in situ grown on the surface of the polymer nanospheres, to obtain 12.5 g of a composite nanofluid expellant.
[0091] Example 2
[0092] This embodiment provides a composite nanofluid repellent, which is prepared according to the following steps:
[0093] (1) Dissolve 0.3 g of Span 80 and 0.1 g of Tween 80 in 40 mL of liquid paraffin and stir at a speed of 350 r / min for 30 min to obtain an emulsified oil phase;
[0094] (2) dissolving 7.5 g of acrylamide, 0.18 g of N,N-methylene acrylamide, and 0.18 g of potassium persulfate in 15 mL of deionized water to obtain an aqueous phase;
[0095] (3) At a stirring speed of 350 r / min, the aqueous phase was dripped into the emulsified oil phase to obtain a stable emulsion. After adjusting the HLB value to 5 using NH4OH, stirring was continued for 30 min to form a stable emulsion. The temperature was then raised to 75°C. Under the protection of N2, acrylamide and N,N-methylene acrylamide were polymerized for 4 h to adjust the HLB value of the emulsion system to 13, thereby obtaining a water-in-oil emulsion-like polymer nanosphere emulsion.
[0096] (4) First, 1 g of tetraethyl orthosilicate was dispersed in a mixed solvent of 3 g of ethanol and water to obtain a tetraethyl orthosilicate dispersion, wherein the volume ratio of ethanol to water was 4:6. The tetraethyl orthosilicate dispersion was then added to 10 g of polymer nanosphere emulsion, and then 2 g of ammonia water was added for catalytic hydrolysis. After reacting at room temperature for 5 h, the silica nanoparticles generated by the hydrolysis reaction grew in situ on the surface of the polymer nanospheres to obtain 13 g of a composite nanofluid expellant.
[0097] Example 3
[0098] This embodiment provides a composite nanofluid repellent, which is prepared according to the following steps:
[0099] (1) Dissolve 0.3 g of Span 80 and 0.1 g of Tween 80 in 40 mL of liquid paraffin and stir at a speed of 350 r / min for 30 min to obtain an emulsified oil phase;
[0100] (2) dissolving 8 g of acrylamide, 0.2 g of N,N-methylene acrylamide, and 0.2 g of potassium persulfate in 15 mL of deionized water to obtain an aqueous phase;
[0101] (3) At a stirring speed of 350 r / min, the aqueous phase was dripped into the oil phase to obtain a stable emulsion. After adjusting the HLB value to 5 using NH4OH, stirring was continued for 30 min to form a stable emulsion. The temperature was then raised to 75°C. Under the protection of N2, acrylamide and N,N-methylene acrylamide were polymerized for 4 h to adjust the HLB value of the emulsion system to 14, thereby obtaining a water-in-oil emulsion-like polymer nanosphere emulsion.
[0102] (4) First, 1 g of tetraethyl orthosilicate was added to a mixed solvent of 4 g of ethanol and water to obtain a tetraethyl orthosilicate dispersion, wherein the volume ratio of ethanol to water was 3:7. The tetraethyl orthosilicate dispersion was then added to 10 g of a polymer nanosphere emulsion, and then 0.5 g of diethanolamine was added for catalytic hydrolysis. After reacting at room temperature for 5 h, the silica nanoparticles generated by the hydrolysis reaction grew in situ on the surface of the polymer microspheres to obtain 13.5 g of a composite nanofluid expellant.
[0103] Example 4
[0104] This embodiment provides a composite nanofluid repellent, which is prepared according to the following steps:
[0105] (1) Dissolve 0.3 g of Span 80 and 0.1 g of OP-10 in 40 mL of white oil and stir at 350 r / min for 30 min to obtain an emulsified oil phase;
[0106] (2) dissolving 7 g of acrylamide, 0.15 g of N,N-methylene acrylamide, and 0.14 g of potassium persulfate in 15 mL of deionized water to obtain an aqueous phase;
[0107] (3) At a stirring speed of 350 r / min, the aqueous phase was dripped into the emulsified oil phase to obtain a stable emulsion. After adjusting the HLB value to 5 using NH4OH, stirring was continued for 30 min to form a stable emulsion. The temperature was then raised to 75°C. Under the protection of N2, acrylamide and N,N-methylene acrylamide were polymerized for 4 h. The HLB value of the emulsion system was adjusted to 15 to obtain a water-in-oil emulsion-like polymer nanosphere emulsion.
[0108] (4) First, 1 g of tetraethyl orthosilicate was added to a mixed solvent of 3 g of ethanol and water to obtain a tetraethyl orthosilicate dispersion, wherein the volume ratio of ethanol to water was 4:6. The obtained tetraethyl orthosilicate dispersion was then added to 10 g of polymer nanosphere emulsion, and then 0.5 g of diethanolamine was added for catalytic hydrolysis. After reacting for 5 h at room temperature, silica nanoparticles generated by the hydrolysis reaction grew in situ on the surface of the polymer nanospheres to obtain 12.5 g of a composite nanofluid expellant.
[0109] Example 5
[0110] This embodiment provides a composite nanofluid repellent, which is prepared according to the following steps:
[0111] (1) Dissolve 0.3 g of Span 80 and 0.1 g of NP-10 in 40 mL of white oil and stir at 350 r / min for 30 min to obtain an emulsified oil phase;
[0112] (2) dissolving 7 g of acrylamide, 0.15 g of N,N-methylene acrylamide, and 0.14 g of potassium persulfate in 15 mL of deionized water to obtain an aqueous phase;
[0113] (3) At a stirring speed of 350 r / min, the aqueous phase was dripped into the emulsified oil phase to obtain a stable emulsion. After adjusting the HLB value to 5 using NH4OH, stirring was continued for 30 min to form a stable emulsion. The temperature was then raised to 75°C. Under the protection of N2, acrylamide and N,N-methylene acrylamide were polymerized for 4 h to adjust the HLB value of the emulsion system to 11, thereby obtaining a water-in-oil emulsion-like polymer nanosphere emulsion.
[0114] (4) First, 1 g of tetraethyl orthosilicate was added to a mixed solvent of 2 g of ethanol and water to obtain tetraethyl orthosilicate in which the volume ratio of ethanol to water was 1:1. The tetraethyl orthosilicate dispersion was then added to 10 g of polymer nanosphere emulsion. Then, 0.5 g of diethanolamine was added for catalytic hydrolysis. After reacting for 5 h at room temperature, the silica nanoparticles generated by hydrolysis were in situ grown on the surface of the polymer nanospheres to obtain 12 g of a composite nanofluid expellant.
[0115] Example 6
[0116] This embodiment provides a composite nanofluid repellent, which is prepared according to the following steps:
[0117] (1) Dissolve 0.3 g of Span 80 and 0.1 g of Tween 80 in 40 mL of white oil and stir at a speed of 350 r / min for 30 min to obtain an emulsified oil phase;
[0118] (2) dissolving 7 g of acrylamide, 0.15 g of N,N-methylene acrylamide, and 0.14 g of potassium persulfate in 15 mL of deionized water to obtain an aqueous phase;
[0119] (3) At a stirring speed of 350 r / min, the aqueous phase was dripped into the emulsified oil phase to obtain a stable emulsion. After adjusting the HLB value to 5 using NH4OH, stirring was continued for 30 min to form a stable emulsion. The temperature was then raised to 65°C. Under the protection of N2, acrylamide and N,N-methylene acrylamide were polymerized for 6 h. The HLB value of the emulsion system was adjusted to 10 to obtain a water-in-oil emulsion-like polymer nanosphere emulsion.
[0120] (4) First, 1 g of tetraethyl orthosilicate was dispersed in a mixed solvent of 4 g of ethanol and water to obtain a tetraethyl orthosilicate dispersion, wherein the volume ratio of ethanol to water was 3:7. The tetraethyl orthosilicate dispersion was then added to 10 g of a polymer nanosphere emulsion, and then 0.5 g of diethanolamine was added for catalytic hydrolysis. After reacting for 5 h at room temperature, silica nanoparticles generated by the hydrolysis reaction grew in situ on the surface of the polymer nanospheres to obtain 12.5 g of a composite nanofluid expellant.
[0121] Example 7
[0122] This embodiment provides a composite nanofluid repellent, which is prepared according to the following steps:
[0123] (1) Dissolve 0.3 g of Span 80 and 0.1 g of Tween 80 in 40 mL of white oil and stir at a speed of 350 r / min for 30 min to obtain an emulsified oil phase;
[0124] (2) dissolving 7 g of acrylamide, 0.15 g of N,N-methylene acrylamide, and 0.14 g of potassium persulfate in 15 mL of deionized water to obtain an aqueous phase;
[0125] (3) At a stirring speed of 350 r / min, the aqueous phase was dripped into the emulsified oil phase to obtain a stable emulsion. After adjusting the HLB value to 5 using NH4OH, stirring was continued for 30 min to form a stable emulsion. The temperature was then raised to 65°C and reacted for 6 h under N2 protection to adjust the HLB value of the emulsion system to 11 to obtain an oil-in-water emulsion-like polymer nanosphere emulsion.
[0126] (4) Dispersing 1 g of tetraethyl orthosilicate in a mixed solvent of 4 g of ethanol and water to obtain a tetraethyl orthosilicate dispersion, wherein the volume ratio of ethanol to water is 4:6, and then adding the tetraethyl orthosilicate dispersion to 20 g of polymer nanosphere emulsion, and then adding 1 g of diethanolamine for catalytic hydrolysis. After reacting for 5 h at room temperature, the silica nanoparticles generated by the hydrolysis reaction grow in situ on the surface of the polymer nanospheres to obtain 14 g of a composite nanofluid expellant.
[0127] Example 8
[0128] This embodiment provides a composite nanofluid repellent, which is prepared according to the following steps:
[0129] (1) 0.3 g of Span 80 and 0.1 g of Tween 80 were dissolved in 40 mL of cyclohexane and stirred at a speed of 350 r / min for 30 min to obtain an emulsified oil phase;
[0130] (2) dissolving 7 g of acrylamide, 0.15 g of N,N-methylene acrylamide, and 0.14 g of potassium persulfate in 15 mL of deionized water to obtain an aqueous phase;
[0131] (3) At a stirring speed of 350 r / min, the aqueous phase was dripped into the emulsified oil phase to obtain a stable emulsion. After adjusting the HLB value to 5 using NH4OH, stirring was continued for 30 min to form a stable emulsion. The temperature was then raised to 65°C. Under the protection of N2, acrylamide and N,N-methylene acrylamide were polymerized for 6 h. The HLB value of the emulsion system was then adjusted to 14 to obtain a water-in-oil emulsion-like polymer nanosphere emulsion.
[0132] (4) First, 1 g of tetraethyl orthosilicate was added to a mixed solvent of 3 g of ethanol and water to obtain a tetraethyl orthosilicate dispersion, wherein the volume ratio of ethanol to water was 5:5. The obtained tetraethyl orthosilicate dispersion was then added to 10 g of polymer nanosphere emulsion, and then 1 g of diethanolamine was added for catalytic hydrolysis. After reacting for 5 h at room temperature, silica nanoparticles generated by the hydrolysis reaction grew in situ on the surface of the polymer nanospheres to obtain 13 g of a composite nanofluid expellant.
[0133] Example 9
[0134] This embodiment provides a composite nanofluid repellent, which is prepared according to the following steps:
[0135] (1) Dissolve 0.3 g of Span 80 and 0.1 g of OP-10 in 45 mL of white oil and stir at 350 r / min for 30 min to obtain an emulsified oil phase;
[0136] (2) dissolving 7.5 g of acrylamide, 0.18 g of N,N-methylene acrylamide, and 0.18 g of potassium persulfate in 18 mL of deionized water to obtain an aqueous phase;
[0137] (3) At a stirring speed of 350 r / min, the water phase was dripped into the emulsified oil phase to obtain a stable emulsion, and the HLB value was adjusted to 5 with NH4OH, and the stirring was continued for 30 min to form a stable emulsion, and then the temperature was raised to 70°C, and acrylamide and N,N-methylene acrylamide were polymerized for 6 h under N2 protection to adjust the HLB value of the emulsion system to 13, thereby obtaining a water-in-oil emulsion-like polymer nanosphere emulsion;
[0138] (4) First, 1 g of tetraethyl orthosilicate was added to a mixed solvent of 4 g of ethanol and water to obtain a tetraethyl orthosilicate dispersion, wherein the volume ratio of ethanol to water was 4:6. The obtained tetraethyl orthosilicate dispersion was then added to 10 g of polymer nanosphere emulsion, and then 0.75 g of diethanolamine was added for catalytic hydrolysis. After reacting at room temperature for 5 h, the silica nanoparticles generated by the hydrolysis reaction grew in situ on the surface of the polymer microspheres to obtain 13.25 g of a composite nanofluid expellant.
[0139] Example 10
[0140] This embodiment provides a composite nanofluid repellent, which is prepared according to the following steps:
[0141] (1) Dissolve 0.3 g of Span 80 and 0.1 g of OP-10 in 45 mL of white oil and stir at 350 r / min for 30 min to obtain an emulsified oil phase;
[0142] (2) dissolving 7.5 g of acrylamide, 0.18 g of N,N-methylene acrylamide, and 0.18 g of potassium persulfate in 18 mL of deionized water to obtain an aqueous phase;
[0143] (3) At a stirring speed of 350 r / min, the aqueous phase was dripped into the emulsified oil phase to obtain a stable emulsion. After adjusting the HLB value to 5 using NH4OH, stirring was continued for 30 min to form a stable emulsion. The temperature was then raised to 70°C. Under the protection of N2, acrylamide and N,N-methylene acrylamide were polymerized for 6 h. The HLB value of the emulsion system was then adjusted to 15 to obtain a water-in-oil emulsion-like polymer nanosphere emulsion.
[0144] (4) First, 1 g of tetraethyl orthosilicate was added to a mixed solvent of 3 g of ethanol and water to obtain a tetraethyl orthosilicate dispersion, wherein the volume ratio of ethanol to water was 5:5. The obtained tetraethyl orthosilicate dispersion was then added to 10 g of polymer nanosphere emulsion, and then 0.75 g of diethanolamine was added for catalytic hydrolysis. After reacting at room temperature for 6 h, the silica nanoparticles generated by the hydrolysis reaction grew in situ on the surface of the polymer nanospheres to obtain 12.25 g of a composite nanofluid expellant.
[0145] Embodiment 11
[0146] This embodiment provides a composite nanofluid repellent, which is prepared according to the following steps:
[0147] (1) Dissolve 0.4 g of Span and 0.13 g of NP-10 in 45 mL of white oil and stir at 350 r / min for 30 min to obtain an emulsified oil phase;
[0148] (2) dissolving 7.5 g of acrylamide, 0.18 g of N,N-methylene acrylamide, and 0.18 g of potassium persulfate in 18 mL of deionized water to obtain an aqueous phase;
[0149] (3) At a stirring speed of 350 r / min, the aqueous phase was dripped into the emulsified oil phase to obtain a stable emulsion. After adjusting the HLB value to 5 using NH4OH, stirring was continued for 30 min to form a stable emulsion. The temperature was then raised to 75°C. Under the protection of N2, acrylamide and N,N-methylene acrylamide were polymerized for 6 h to adjust the HLB value of the emulsion system to 12, thereby obtaining an oil-in-water emulsion-like polymer nanosphere emulsion.
[0150] (4) First, 1 g of tetraethyl orthosilicate was added to a mixed solvent of 2 g of ethanol and water to obtain a tetraethyl orthosilicate dispersion, wherein the volume ratio of ethanol to water was 4:6. The obtained tetraethyl orthosilicate dispersion was then added to 10 g of a polymer nanosphere emulsion, and then 3 g of ammonia water (mass concentration of 25%) was added for catalytic hydrolysis. After reacting at room temperature for 6 h, the silica nanoparticles generated by the hydrolysis reaction grew in situ on the surface of the polymer nanospheres to obtain 12.5 g of a composite nanofluid expellant.
[0151] Example 12
[0152] This embodiment provides a composite nanofluid repellent, which is prepared according to the following steps:
[0153] (1) Dissolve 0.3 g of Span 80 and 0.1 g of Tween 80 in 40 mL of white oil and stir at a speed of 350 r / min for 30 min to obtain an emulsified oil phase;
[0154] (2) dissolving 7 g of acrylamide, 0.15 g of N,N-methylene acrylamide, and 0.14 g of potassium persulfate in 15 mL of deionized water to obtain an aqueous phase;
[0155] (3) At a stirring speed of 350 r / min, the aqueous phase was dripped into the emulsified oil phase to obtain a stable emulsion. After adjusting the HLB value to 5 using NH4OH, stirring was continued for 30 min to form a stable emulsion. The temperature was then raised to 65°C. Under the protection of N2, acrylamide and N,N-methylene acrylamide were polymerized for 6 h. The HLB value of the emulsion system was then adjusted to 14 to obtain a water-in-oil emulsion-like polymer nanosphere emulsion.
[0156] (4) First, 1 g of tetraethyl orthosilicate was added to a mixed solvent of 3 g of ethanol and water to obtain a tetraethyl orthosilicate dispersion, wherein the volume ratio of ethanol to water was 5:5. The obtained tetraethyl orthosilicate dispersion was then added to 10 g of polymer nanosphere emulsion, and then 2 g of diethanolamine was added for catalytic hydrolysis. After reacting for 6 h at room temperature, the silica nanoparticles generated by the hydrolysis reaction grew in situ on the surface of the polymer microspheres to obtain 13 g of a composite nanofluid expellant.
[0157] Example 13
[0158] The difference between this embodiment and embodiment 1 is that in step (1), the amount of white oil used is 47.5 mL; in step (2), the amount of acrylamide used is 5 g, the amount of N,N-methylene acrylamide used is 0.4 g, the amount of potassium persulfate used is 0.1 g, and the amount of deionized water used is 12.5 mL.
[0159] Embodiment 14
[0160] The difference between this embodiment and embodiment 1 is that in step (1), the amount of white oil used is 37.5 mL; in step (2), the amount of acrylamide used is 8 g, the amount of N,N-methylene acrylamide used is 0.1 g, the amount of potassium persulfate used is 0.1 g, and the amount of deionized water used is 18 mL.
[0161] Embodiment 15
[0162] The difference between this embodiment and embodiment 1 is that in step (1), the amount of white oil used is 25 mL.
[0163] Example 16
[0164] The difference between this embodiment and embodiment 1 is that in step (1), the amount of white oil used is 60 mL.
[0165] Embodiment 17
[0166] The difference between this embodiment and embodiment 1 is that in step (2), the amount of acrylamide used is 4 g and the amount of N,N-methylene acrylamide used is 0.5 g.
[0167] Embodiment 18
[0168] The difference between this embodiment and embodiment 1 is that in step (2), the amount of acrylamide used is 10 g and the amount of N,N-methylene acrylamide used is 0.1 g.
[0169] Embodiment 19
[0170] The difference between this embodiment and embodiment 1 is that in step (2), the amount of deionized water is 10 mL.
[0171] Embodiment 20
[0172] The difference between this embodiment and embodiment 1 is that in step (2), the amount of deionized water is 20 mL.
[0173] Test Example 1
[0174] The composite nanofluid repellent provided in the examples was subjected to the following tests, and the results are shown in Table 1 below.
[0175] (1) Interfacial tension test: According to SY / T 5370-2018 “Surface and interfacial tension determination method”, the interfacial tension between the oil displacement agent aqueous solution and the formation crude oil was tested. The test equipment used was German dataphysis SVT20N, the test temperature was 60°C, and the rotation speed was 6000 r / min.
[0176] (2) Wettability test: According to SY / T 5153-2017, the wettability of the composite nano-displacement agent on the reservoir rock was tested.
[0177] (3) The oil-infiltration performance of composite nano-displacement agents with different concentrations was evaluated using an oil-infiltration bottle.
[0178] (4) The particle size of the composite nanoparticles in the composite nano-expulsion agent was tested using a scanning electron microscope.
[0179] (5) Referring to the national energy industry standard NB / T 14003.1-2015 “Shale gas fracturing fluid Part 1: Slick water performance indicators and evaluation methods”, the viscosity and drag reduction performance of composite nano-displacement agents with different concentrations were evaluated.
[0180] Table 1
[0181] serial number Average particle size of polymer nanoparticles (nm) <![CDATA[Average particle size (nm) of SiO2-coated polymer nanoparticles]]> Example 1 50 58 Example 2 43 55 Example 3 34 60 Example 4 52 59 Example 5 54 60 Example 6 51 56 Example 7 52 60 Example 8 48 55 Example 9 30 39 Example 10 31 30 Embodiment 11 43 58 Example 12 42 55 Example 13 36 48 Embodiment 14 41 58 Embodiment 15 700 720 Example 16 930 943 Embodiment 17 430 442 Embodiment 18 690 710 Embodiment 19 500 510 Embodiment 20 800 814
[0182] Test Example 2
[0183] (2.1) The composite nanofluid displacement agent provided in Example 1 was prepared into aqueous solutions with mass concentrations of 0.05%, 0.1%, 0.2%, and 0.3%, respectively, and its wettability, interfacial tension, imbibition oil recovery efficiency, viscosity, and drag reduction rate were tested. The results are shown in Table 2.
[0184] Table 2
[0185] Concentration (wt%) Interfacial tension (mN / m) Wetting angle (°) Imbibition recovery rate (%) Viscosity(mPs) Drag reduction rate (%) 0 16.42 92 1.5 1.0 / 0.05 2 81 4.6 3.8 58 0.1 0.6 70 7.8 6.3 66 0.2 0.2 56 8.9 7.6 72 0.3 0.01 38 12.8 13 77
[0186] (2.2) The composite nanofluid displacement agent provided in Example 2 was prepared into aqueous solutions with mass concentrations of 0.05%, 0.1%, 0.2% and 0.3%, respectively, and its wettability, interfacial tension, imbibition oil recovery efficiency, viscosity and drag reduction rate were tested. The results are shown in Table 3.
[0187] Table 3
[0188] Concentration (wt%) Interfacial tension (mN / m) Wetting angle (°) Imbibition recovery rate (%) Viscosity(mPs) Drag reduction rate (%) 0 16.73 93 1.3 1.0 / 0.05 3 84 4.2 3.6 55 0.1 0.8 71 7.7 6.0 62 0.2 0.3 59 8.6 7.2 73 0.3 0.07 42 11.5 12 74
[0189] (2.3) The composite nanofluid displacement agent provided in Example 3 was prepared into aqueous solutions with mass concentrations of 0.05%, 0.1%, 0.2% and 0.3%, respectively, and its wettability, interfacial tension, imbibition oil recovery efficiency, viscosity and drag reduction rate were tested. The results are shown in Table 4.
[0190] Table 4
[0191] Concentration (wt%) Interfacial tension (mN / m) Wetting angle (°) Imbibition recovery rate (%) Viscosity(mPs) Drag reduction rate (%) 0 16.73 93 1.2 1.0 / 0.05 5 88 4.0 3.3 52 0.1 1 76 6.8 5.2 60 0.2 0.7 62 8.1 6.4 71 0.3 0.09 47 10.4 10 75
[0192] (2.4) The composite nanofluid displacement agent provided in Example 5 was prepared into aqueous solutions with mass concentrations of 0.05%, 0.1%, 0.2% and 0.3%, respectively, and its wettability, interfacial tension, imbibition oil recovery efficiency, viscosity and drag reduction rate were tested. The results are shown in Table 5.
[0193] Table 5
[0194]
[0195]
[0196] (2.5) The composite nanofluid displacement agent provided in Example 8 was prepared into aqueous solutions with mass concentrations of 0.05%, 0.1%, 0.2% and 0.3%, respectively, and its wettability, interfacial tension, imbibition oil recovery efficiency, viscosity and drag reduction rate were tested. The results are shown in Table 6.
[0197] Table 6
[0198] Concentration (wt%) Interfacial tension (mN / m) Wetting angle (°) Imbibition recovery rate (%) Viscosity(mPs) Drag reduction rate (%) 0 16.73 93 1.4 1.0 / 0.05 2 85 5.3 3.3 50 0.1 1 72 6.8 5.2 64 0.2 0.3 64 7.3 7.5 73 0.3 0.02 37 11.2 11.3 76
[0199] (2.6) The composite nanofluid displacement agent provided in Example 12 was prepared into aqueous solutions with mass concentrations of 0.05%, 0.1%, 0.2% and 0.3%, respectively, and its wettability, interfacial tension, imbibition oil recovery efficiency, viscosity and drag reduction rate were tested. The results are shown in Table 7.
[0200] Table 7
[0201] Concentration (wt%) Interfacial tension (mN / m) Wetting angle (°) Imbibition recovery rate (%) Viscosity(mPs) Drag reduction rate (%) 0 16.76 95 1.5 1.0 / 0.05 5 87 4.8 3.4 47 0.1 2 77 5.7 5.6 56 0.2 0.6 68 6.8 6.7 69 0.3 0.05 48 9.5 10.1 71
[0202] (2.7) The composite nanofluid displacement agents provided in Examples 4, 6-7, 9-11, and 13-20 were respectively prepared into aqueous solutions with a mass concentration of 0.1%, and the wettability, interfacial tension, imbibition oil recovery efficiency, viscosity, and drag reduction rate were tested. The results are shown in Table 8.
[0203] Table 8
[0204]
[0205]
[0206] As can be seen from Table 1, through Examples 4 and 5, it can be seen that only changing the mass and ratio of the mixed solvent of ethanol and water has little effect on the average particle size (nm) of the polymer nanoparticles and the average particle size (nm) of the SiO2-coated polymer nanoparticles; through Examples 6 and 7, it can be seen that changing the mass of diethanolamine has little effect on the average particle size (nm) of the polymer nanoparticles and the average particle size (nm) of the SiO2-coated polymer nanoparticles; through Examples 7 and 8, it can be seen that only changing the type of the oil phase, after replacing the white oil with cyclohexane, the average particle size (nm) of the polymer nanoparticles and the average particle size (nm) of the SiO2-coated polymer nanoparticles are slightly reduced; through Examples 3, 9, 10, and 11, it can be seen that after increasing the amount of acrylamide The average particle size (nm) of polymer nanoparticles and the average particle size (nm) of SiO2-coated polymer nanoparticles are slightly reduced; through Examples 15 and 16, it can be obtained that the mass ratio of water to oil phase and acrylamide to oil phase that is too large or too small will cause the average particle size (nm) of polymer nanoparticles and the average particle size (nm) of SiO2-coated polymer nanoparticles to increase, and agglomeration will occur; the data of Examples 17-20 show that the mass ratio of acrylamide to N,N-methylene acrylamide is (10-16):(0.2-0.8), and the mass ratio of water in the aqueous phase to the oil phase is (25-36):(75-95), which is more conducive to the preparation of polymer nanoparticles with smaller particle sizes and SiO2-coated polymer nanoparticles.
[0207] In Experimental Example 2, Tables 2 to 7 show that for composite nanofluid displacement agents prepared in different proportions, the aqueous solution meets the following conditions: the greater the concentration, the smaller the interfacial tension and wetting angle, and the greater the imbibition recovery rate, viscosity and drag reduction rate. Table 8 shows that at the same concentration, the larger the average particle size of the polymer nanoparticles, the greater the interfacial tension and wetting angle; on the contrary, the larger the average particle size of the polymer nanoparticles, the smaller the imbibition recovery rate, viscosity and drag reduction rate.
[0208] From the above description, it can be seen that the above-mentioned embodiments of the present invention achieve the following technical effects: Based on the above-mentioned experimental data, it can be concluded that the composite nanofluid displacement agent provided by the present application is a composite of polymer nano-microspheres and silica nano-particles, and has the properties of both organic and inorganic nano-materials, and can be used for shale oil reservoir fracturing. It not only has good drag reduction effect and sand carrying capacity, and has little damage to the reservoir, but also has excellent wettability reversal and imbibition oil displacement function, can effectively penetrate into the rock, replace the crude oil inside the pore throat, and also has good temperature and salt resistance.
[0209] The above description is only a preferred embodiment of the present invention and is not intended to limit the present invention. For those skilled in the art, the present invention may have various modifications and variations. Any modification, equivalent replacement, improvement, etc. made within the spirit and principle of the present invention shall be included in the protection scope of the present invention.
Claims
1. A composite nanofluid repellent, characterized in that: The composite nanofluid repellent is an emulsion dispersed with composite nanospheres, the emulsion comprises an aqueous phase and an oil phase, the oil phase is dispersed in the aqueous phase in the form of droplets; the composite nanospheres comprise polymer nanospheres and silicon dioxide nanoparticles in situ grown on the surface of the polymer nanospheres.
2. The composite nanofluid repellent according to claim 1, characterized in that: The polymer nanospheres are copolymers of acrylamide and N,N-methylene acrylamide; Preferably, the mass ratio of the acrylamide to the N,N-methylene acrylamide is (10-16):(0.2-0.8).
3. The composite nanofluid repellent according to claim 2, characterized in that: The mass ratio of water in the water phase to the oil phase is (25-36):(75-95).
4. The composite nanofluid repellent according to any one of claims 1 to 3, characterized in that: The D50 of the composite nano-microspheres is 30 to 60 nm; The mass concentration of the composite nano-microspheres is 20% to 30%; Preferably, the emulsion further comprises an emulsifier, and the emulsifier is selected from at least one of Span 80, Span 60, OP-10, NP-10 or Tween 80; Preferably, the oil phase is selected from at least one of cyclohexane, white oil or liquid paraffin.
5. A method for preparing a composite nanofluid repellent, characterized in that: The preparation method comprises: Step S1, dissolving a polymerizable monomer and an initiator in water to obtain an aqueous phase, wherein the polymerizable monomer is a water-soluble monomer; Step S2, mixing the water phase and the oil phase to obtain a mixed solution, heating the mixed solution, so that the polymerizable monomer undergoes a polymerization reaction under the action of the initiator to form polymer nanospheres, and obtaining a polymer nanosphere emulsion; Step S3, adding tetraethyl orthosilicate to the polymer nanosphere emulsion for hydrolysis reaction, and the silicon dioxide nanoparticles generated by the hydrolysis reaction grow in situ on the surface of the polymer nanosphere to obtain the composite nanofluid repellent.
6. The preparation method according to claim 5, characterized in that: In step S1, the polymerization monomers include a first comonomer and a second comonomer, the first comonomer is acrylamide, the second comonomer is N,N-methylene acrylamide, and the initiator is a persulfate, preferably potassium persulfate; Preferably, the mass ratio of the acrylamide, the N,N-methylene acrylamide and the potassium persulfate is (10-16):(0.2-0.8):(0.2-0.8).
7. The preparation method according to claim 5, characterized in that: In the step S2, an emulsifier is dispersed in the oil phase, and the mass ratio of the emulsifier to the oil phase is (0.5-1): (75-95); Preferably, the emulsifier is selected from at least one of Span 80, Span 60, OP-10, NP-10 or Tween 80; Preferably, the oil phase is selected from at least one of cyclohexane, white oil or liquid paraffin.
8. The preparation method according to claim 5, characterized in that: The step S2 comprises: first adjusting the HLB value of the mixed solution to 3-6, and then heating the mixed solution to carry out the polymerization reaction; Preferably, the polymerization reaction is carried out at a temperature of 50 to 80°C for a time of 2 to 6 hours, and preferably the polymerization reaction is carried out under the protection of an inert gas; Preferably, the mass ratio of water in the aqueous phase to the oil phase is (25-36): (75-95); Preferably, the mass ratio of the acrylamide to the oil phase is (10-16): (75-95); Preferably, the step S2 further comprises: after the polymerization reaction is completed, adjusting the HLB value of the system to 10-15 to obtain the polymer nanosphere emulsion.
9. The preparation method according to any one of claims 5 to 8, characterized in that: The step S3 comprises: first dispersing the tetraethyl orthosilicate in a mixed solvent of ethanol and water to obtain a dispersion of the tetraethyl orthosilicate, and then adding the dispersion of the tetraethyl orthosilicate to the polymer nanosphere emulsion; Preferably, in the mixed solvent, the volume ratio of ethanol to water is (3-5): (5-7); Preferably, the mass ratio of tetraethyl orthosilicate to the mixed solvent is 1:(2-4); Preferably, the mass ratio of tetraethyl orthosilicate dispersion to the polymer nanosphere emulsion is (3-5):10; Preferably, the hydrolysis reaction is carried out under the action of a catalyst, and the catalyst is preferably selected from at least one of diethanolamine and ammonia water, and the mass concentration of the ammonia water is preferably 20-30%; Preferably, the mass ratio of the catalyst to the tetraethyl orthosilicate is (2-30):(5-10); Preferably, the temperature of the hydrolysis reaction is 10-40° C. and the time is 4-6 hours.
10. The composite nanofluid displacement agent according to any one of claims 1 to 4 or the composite nanofluid displacement agent obtained according to the preparation method according to any one of claims 5 to 9 is used as an imbibition oil displacement agent or to displace slick water in a tight reservoir.