Terbium-gadolinium nanocrystal, terbium-gadolinium nanocrystal compound wrapped by diphenyl phosphinoxyl benzoic acid compound ligand, and preparation method and application of terbium-gadolinium nanocrystal compound
By combining diphenylphosphineoxybenzoic acid compounds with terbium-gadolinium nanocrystals, the problem of high driving voltage and unbalanced carrier transport of rare earth luminescent materials in electroluminescent devices is solved, and high luminescence at low driving voltage is achieved. Luminous performance improves the overall performance of electroluminescent devices.
Patent Information
- Application Number
- CN202410748189.6
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Filing Date
- 2024-06-11
- Publication Date
- 2024-10-01
AI Technical Summary
Rare earth luminescent materials have problems with high driving voltage requirements and unbalanced carrier transport in electroluminescent devices driven directly by electric fields, which limits their application in high-resolution display devices.
Diphenylphosphineoxybenzoic acid compounds are used as ligands to combine with terbium-gadolinium nanocrystals. By enhancing carrier transmission and recombination to form excitons, the threshold voltage of the electroluminescent device is reduced, and the luminous brightness, current efficiency and Power efficiency.
It achieves balanced carrier transport and recombination at low driving voltage under the action of an electric field, and significantly improves the luminescence properties of rare earth element nanocrystals, including reducing threshold voltage, improving brightness, current efficiency, power efficiency and external quantum efficiency.
Smart Images

Figure BDA0004887041370000021 
Figure BDA0004887041370000031 
Figure BDA0004887041370000032
Abstract
Description
Technical Field
[0001] The present invention belongs to the technical field of organic-inorganic hybrid rare earth luminescent nanomaterials, and specifically relates to a diphenylphosphinobenzoic acid compound ligand coated NaGd (1-x) Synthesis and application of organic-inorganic hybrid rare earth luminescent nanoparticles of F4:xTb. Background Art
[0002] Rare earth (RE) resources are abundant in China, and rare earths include 17 elements, including lanthanides, scandium and yttrium. Materials containing rare earth elements have obvious absorption and emission bands and high color purity because the electrons in the 4f orbital of rare earth ions are well protected by the fully filled 5s and 5p subshells, which are protected from active interaction with the external environment. The main influence of surrounding ions on the internal orbital promotes the transition of electrons in the 4f orbital. This makes the materials containing rare earth elements play an important role in the application of technologies such as light-emitting diodes, cathode rays, near-infrared emission materials and plasma displays. In the development of rare earth materials, rare earth functionalized mesoporous nanostructured materials have attracted special attention in many fields due to their excellent structural characteristics and unique luminescence properties, such as fluorescent immunoassays, biological probes, lasers, optical amplification, light conversion molecular devices (LCMDs) and organic light-emitting diodes (OLEDs). However, the ff transition of rare earth ions is symmetry forbidden, so it is difficult to produce effective luminescence emission by direct excitation, which limits its practical application in the field of optical devices. Rare earth doping is an important way to improve the performance of optoelectronic functional materials. Organic-inorganic hybrid materials containing rare earth elements have attracted great attention in recent years. They can advantageously combine the different properties of organic and inorganic components in one material to achieve a composite dual-phase structure of organic and inorganic materials, integrating the advantages of both organic and inorganic materials, thereby showing significant characteristics in optical, magnetic and electrical properties.
[0003] Electroluminescent materials and devices for high-resolution display are gaining more and more attention. Currently, the more mainstream organic electroluminescent quantum dots and perovskites have shown very good advantages, especially recently, they have made certain breakthroughs in narrow-band emission and other aspects. However, compared with rare earth luminescent materials, the color purity of rare earth luminescent materials obviously has incomparable advantages, but rare earth materials still have bottlenecks in their processing performance, especially in the application of high-resolution display devices. In the past quite a long period of time, the research on materials based on rare earth luminescent nanocrystals has made great progress. Through effective ligand stabilization, rare earth luminescent nanocrystals of different sizes, different sizes, and different luminescent properties can be synthesized, and the color, efficiency, and life of their luminescence can be controlled and regulated, which will lay the foundation for the application of such rare earth luminescent materials in high-resolution display devices. However, there is an intrinsic bottleneck in the application of such materials in electroluminescent devices directly driven by electric fields. Rare earth fluorides or some other rare earth matrices are not conductive themselves, resulting in the need for a very high driving voltage in the electric field. At the same time, the transmission and recombination of carriers are also unbalanced, which will reduce its luminescent performance. Summary of the invention
[0004] In order to solve the above problems, the present invention provides a terbium-gadolinium nanocrystal and a terbium-gadolinium nanocrystal compound encapsulated by a diphenylphosphinobenzoic acid compound ligand, both of which have good optical properties and can realize electroluminescence under the action of an electric field, thereby preparing an electroluminescent device as a light-emitting layer material. The ligand of the terbium-gadolinium nanocrystal compound encapsulated by the diphenylphosphinobenzoic acid compound ligand can enhance carrier transport, and compound to form excitons, transfer energy to the nanocrystal, and the nanocrystal emits a narrow-band emission characteristic of rare earth elements terbium and gadolinium, thereby reducing the threshold voltage of the electroluminescent device, improving the luminous brightness, current efficiency, power efficiency and external quantum efficiency, and realizing the improvement of the comprehensive luminescent performance of the electroluminescent device using the rare earth element compound as the light-emitting layer material.
[0005] The purpose of the present invention is to:
[0006] 1. Provide a terbium-gadolinium nanocrystal, comprising a terbium-gadolinium nanocrystal coordinated with an unsaturated fatty acid and a ligand-free terbium-gadolinium nanocrystal,
[0007] After terbium salt, gadolinium salt and unsaturated fatty acid react in a solvent, alkali metal hydroxide and fluoride are added to react to prepare terbium gadolinium nanocrystal coordinated with unsaturated fatty acid, wherein the unsaturated fatty acid is selected from 10 One or more of the above unsaturated fatty acids, preferably containing C 14 -C 24 One or more of the monounsaturated fatty acids, more preferably oleic acid (OA).
[0008] The unsaturated fatty acid ligand is removed from the terbium-gadolinium nanocrystal coordinated with the unsaturated fatty acid to obtain the ligand-free terbium-gadolinium nanocrystal.
[0009] The terbium-gadolinium nanocrystals include MGd coordinated with unsaturated fatty acids. (1-x) F4:xTb, denoted as MGd (1-x) F4:xTb@unsaturated fatty acids, also includes ligand-free terbium-gadolinium nanocrystals, denoted as MGd (1-x) F4:xTb, wherein M is an alkali metal element, x is 0.1-0.9, preferably 0.3-0.5, more preferably 0.4. The alkali metal element is preferably Na and / or potassium, more preferably Na.
[0010] 2. Provide a method for preparing the terbium-gadolinium nanocrystals, wherein the method comprises reacting terbium salt, gadolinium salt and unsaturated fatty acid in a solvent, and then adding alkali metal hydroxide and fluoride to react to prepare the terbium-gadolinium nanocrystals. The method specifically comprises the following steps:
[0011] Step A. adding terbium salt, gadolinium salt and unsaturated fatty acid into a solvent, mixing evenly, heating for reaction, and obtaining a first reaction solution;
[0012] Step B. adding an alkali metal hydroxide and a fluoride to the first reaction solution to react and obtain a second reaction solution;
[0013] Step C: post-treating the second reaction solution to obtain terbium-gadolinium nanocrystals.
[0014] 3. Provide a diphenylphosphinobenzoic acid compound, which is represented by formula (1):
[0015]
[0016] Wherein, R0 is selected from hydrogen or a nitrogen-containing group, preferably hydrogen, carbazole, tert-butylcarbazole, dimethylacridinyl or diphenylacridinyl.
[0017] Preferably, the diphenylphosphinobenzoic acid compound is one of the following compounds:
[0018]
[0019] More preferably, the diphenylphosphinobenzoic acid compound is one of Compound 1 to Compound 4.
[0020] 4. Provide a method for preparing the diphenylphosphinobenzoic acid compound. The method specifically comprises the following steps:
[0021] Step 1. reacting halogenated toluene with magnesium to obtain a Grignard reagent, adding diphenylphosphine halide to react, and after oxidation, post-treating to obtain a diphenylphosphinoyltoluene compound;
[0022] Optionally, carry out step 2. add a diphenylphosphinooxytoluene compound and a nitrogen-containing compound to solvent I, carry out a catalytic reaction in the presence of a catalyst, and perform post-treatment to obtain a diphenylphosphinooxytoluene compound having a nitrogen heterocyclic substituent.
[0023] In step 2, the diphenylphosphinoyltoluene compound is:
[0024]
[0025] Wherein, R1 is a bromine substituent or a chlorine substituent.
[0026] Step 3. Add a diphenylphosphinooxytoluene compound or a nitrogen heterocyclic substituted diphenylphosphinooxytoluene compound to solvent II, add potassium permanganate, heat to react, and post-treat to obtain a diphenylphosphinooxybenzoic acid compound.
[0027] 5. Provide a terbium-gadolinium nanocrystalline compound encapsulated by a diphenylphosphinobenzoic acid compound ligand.
[0028] The terbium-gadolinium nanocrystalline compound wrapped by the diphenylphosphinobenzoic acid compound ligand is MGd coordinated with the diphenylphosphinobenzoic acid compound. (1-x) F4:xTb, denoted as MGd (1-x) F4:xTb@Ligand, wherein M is an alkali metal element, x is 0.1-0.9, preferably 0.3-0.5, more preferably 0.4. The alkali metal element is preferably Na and / or potassium, more preferably Na.
[0029] The terbium-gadolinium nanocrystal compound coated with a diphenylphosphinobenzoic acid compound ligand is obtained by reacting terbium-gadolinium nanocrystals without ligand coating with a diphenylphosphinobenzoic acid compound.
[0030] 6. Provide a method for preparing the terbium-gadolinium nanocrystalline compound encapsulated by the diphenylphosphinobenzoic acid compound ligand, the method specifically comprising the following steps:
[0031] Step a. Add the dispersion of the terbium-gadolinium nanocrystals coordinated with unsaturated fatty acids to a nitrosoboric acid tetrafluoroborate (NOBF4) solution, perform ultrasonic treatment, then add solvent a, perform ultrasonic treatment again, centrifuge and wash to obtain terbium-gadolinium nanocrystals without ligand coating.
[0032] Step b. adding the terbium-gadolinium nanocrystals without ligand coating to a diphenylphosphinobenzoic acid compound solution, subjecting to ultrasonic treatment, and repeating centrifugation, washing, and centrifugation to obtain the terbium-gadolinium nanocrystals compound coated with the diphenylphosphinobenzoic acid compound ligand.
[0033] 7. Provide an electroluminescent device, which includes an anode conductive layer, a hole injection layer, a hole transport layer, a light-emitting layer, a hole blocking layer, an electron transport layer, an electron injection layer and a cathode conductive layer.
[0034] The raw materials for preparing the light-emitting layer include one or more of the terbium gadolinium nanocrystals described in the first aspect, the terbium gadolinium nanocrystals without ligand coating obtained in the sixth aspect, and the terbium gadolinium nanocrystals coated with diphenylphosphinobenzoic acid compound ligands described in the fifth aspect, preferably include one or more of the terbium gadolinium nanocrystals coated with diphenylphosphinobenzoic acid compound ligands described in the fifth aspect, and more preferably include one or more of the terbium gadolinium nanocrystals coated with compounds 1 to 4.
[0035] 8. Provide a method for preparing the electroluminescent device. The method specifically comprises the following steps:
[0036] 1. preparing a conductive anode layer;
[0037] 2. preparing a hole injection layer;
[0038] 3. Preparation of hole transport layer;
[0039] 4. preparing a light-emitting layer;
[0040] 5. preparing a hole blocking layer;
[0041] 6. Preparation of electron transport layer;
[0042] 7. preparing an electron injection layer;
[0043] 8. Prepare a cathode conductive layer, encapsulate, and obtain an organic-inorganic hybrid rare earth luminescent nanoparticle electroluminescent device.
[0044] The present invention has the following beneficial effects:
[0045] (1) The rare earth nanoparticles MGd provided by the present invention (1-x) F4:xTb, the synthesis route is easy to achieve, the preparation method is simple, and it can synthesize ultra-small nanoparticles.
[0046] (2) The diphenylphosphinobenzoic acid compound provided by the present invention forms a complex with terbium-gadolinium nanocrystals, which can enhance the luminescence performance of terbium-gadolinium nanocrystals. The diphenylphosphinobenzoic acid compound is used as a ligand, and its triplet energy level is close to that of the lanthanide ion Tb. 3+ The energy transition of energy levels, the ligand molecule plays a sensitizing role.
[0047] (3) The diphenylphosphinobenzoic acid compounds provided by the present invention can integrate the excellent photoelectric properties of the diphenylphosphinobenzoic acid compounds and the special luminescent properties of rare earth nanocrystals through a ligand engineering strategy. On the one hand, the luminescence of the rare earth nanocrystals can be sensitized by the ligands, and on the other hand, the functions of the ligands themselves can be added to the rare earth nanocrystals, so that such an organic-inorganic composite system has the possibility of realizing electroluminescence under the action of an electric field.
[0048] (4) The diphenylphosphinobenzoic acid compounds provided by the present invention have ligands that inject and transfer carriers, recombine to form excitons, and then transfer energy to nanocrystals, which emit narrow-band emission with rare earth characteristics.
[0049] (5) The electroluminescent device prepared by the organic-inorganic composite system formed by the diphenylphosphinobenzoic acid compound coated with terbium gadolinium nanocrystals provided by the present invention achieves a low driving voltage in the electric field, balanced carrier transmission and recombination, and enhanced luminescence performance.
[0050] (6) The terbium-gadolinium nanocrystals and ligand-free terbium-gadolinium nanocrystals provided by the present invention can be used as guest materials for the light-emitting layer of an electroluminescent device, and realize the electroluminescence of rare earth element nanocrystals with stable luminescent properties.
[0051] (7) The terbium-gadolinium nanocrystal compound encapsulated by the diphenylphosphinobenzoic acid compound ligand provided by the present invention is used as a luminescent guest material, which improves the luminescent properties of the terbium-gadolinium nanocrystal to varying degrees, such as reducing the threshold voltage, improving the brightness, current efficiency, power efficiency, external quantum efficiency, etc., and significantly improves the luminescent properties of the rare earth element nanocrystal. BRIEF DESCRIPTION OF THE DRAWINGS
[0052] Figure 1 The cyclic voltammetry spectra of compounds 1-5 in Examples 3-7 of the present invention are shown;
[0053] Figure 2 It shows that NaGd in Examples 3-7 of the present invention 0.6 F4: UV-visible absorption spectrum of 0.4Tb@Ligand nanoparticles;
[0054] Figure 3 It shows that NaGd in Examples 3-7 of the present invention 0.6 F4: Photoluminescence spectrum of 0.4Tb@Ligand nanoparticles;
[0055] Figure 4 The voltage-current density relationship curves of the electroluminescent devices prepared in Examples 1-7 of the present invention are shown;
[0056] Figure 5The voltage-brightness relationship curves of the electroluminescent devices prepared in Examples 1-7 of the present invention are shown;
[0057] Figure 6 The brightness-current efficiency relationship curves of the electroluminescent devices prepared in Examples 1-7 of the present invention are shown;
[0058] Figure 7 The brightness-power efficiency relationship curves of the electroluminescent devices prepared in Examples 1-7 of the present invention are shown;
[0059] Figure 8 The relationship curves between brightness and external quantum efficiency of the electroluminescent devices prepared in Examples 1-7 of the present invention are shown;
[0060] Fig. 9 The electroluminescence spectra of the electroluminescent devices prepared in Examples 1-7 of the present invention are shown. DETAILED DESCRIPTION
[0061] The present invention is described in detail below through specific implementation modes, and the characteristics and advantages of the present invention will become clearer and more specific with these descriptions.
[0062] The first aspect of the present invention provides a terbium-gadolinium nanocrystal, which includes terbium-gadolinium nanocrystal coordinated with unsaturated fatty acid and ligand-free terbium-gadolinium nanocrystal.
[0063] Terbium salt, gadolinium salt and unsaturated fatty acid react in a solvent, and then alkali metal hydroxide and fluoride are added to react to prepare terbium gadolinium nanocrystals coordinated with unsaturated fatty acid. The unsaturated fatty acid is selected from 10 One or more of the above unsaturated fatty acids, preferably containing C 14 -C 24 One or more of the monounsaturated fatty acids, more preferably oleic acid (OA).
[0064] The unsaturated fatty acid ligand is removed from the terbium-gadolinium nanocrystal coordinated with the unsaturated fatty acid to obtain the ligand-free terbium-gadolinium nanocrystal.
[0065] In the terbium-gadolinium nanocrystals, the ratio of the molar number of the alkali metal element to the total molar number of the terbium element and the gadolinium element is (0.6-1.4):1, preferably (0.8-1.2):1, and more preferably 1:1.
[0066] In the terbium-gadolinium nanocrystals, the molar ratio of terbium element (Tb) to gadolinium element (Gd) is (0.1-0.9):(0.1-0.9), preferably (0.3-0.5):(0.5-0.7), and more preferably 0.4:0.6.
[0067] Preferably, the terbium-gadolinium nanocrystal is MGd coordinated with an unsaturated fatty acid.(1-x) F4:xTb, denoted as MGd (1-x) F4: xTb@unsaturated fatty acid, wherein M is an alkali metal element, x is 0.1-0.9, preferably 0.3-0.5, more preferably 0.4. The alkali metal element is preferably Na and / or potassium, more preferably Na.
[0068] The second aspect of the present invention provides a method for preparing the terbium-gadolinium nanocrystals. The method comprises reacting terbium salt, gadolinium salt and unsaturated fatty acid in a solvent, and then adding alkali metal hydroxide and fluoride to react to obtain terbium-gadolinium nanocrystals coordinated with unsaturated fatty acid.
[0069] The method specifically comprises the following steps:
[0070] Step A: adding terbium salt, gadolinium salt and unsaturated fatty acid into a solvent, mixing them evenly, and heating them for reaction to obtain a first reaction solution.
[0071] The terbium salt is preferably selected from one or more of terbium chloride, terbium nitrate and terbium bromide, more preferably terbium chloride.
[0072] The gadolinium salt is preferably selected from one or more of gadolinium chloride, gadolinium nitrate and gadolinium bromide, more preferably gadolinium chloride.
[0073] The solvent is selected from one or more olefin solvents, preferably having a carbon number of C 16 -C 24 One or more of the olefin solvents, more preferably octadecene.
[0074] The molar volume ratio of the terbium salt to the solvent is 0.4:(8-22) mL, preferably 0.4:(10-20) mL, and more preferably 0.4:(12-18) mL.
[0075] The molar ratio of terbium salt to gadolinium salt is (0.1-0.9):(0.1-0.9), preferably (0.3-0.5):(0.5-0.7), and more preferably 0.4:0.6. The molar amount of terbium salt is calculated based on the molar amount of terbium therein, and the molar amount of gadolinium salt is calculated based on the molar amount of gadolinium therein.
[0076] The reaction temperature is 125-155° C., preferably 130-150° C., more preferably 135-145° C. The reaction time is 2-4 h, preferably 2.5-3.5 h.
[0077] After the reaction is completed, the mixture is cooled to 20-30° C. to obtain a first reaction solution.
[0078] Step B: adding alkali metal hydroxide and fluoride to the first reaction solution to react and obtain a second reaction solution.
[0079] The fluoride is selected from one or more inorganic ion fluorides, preferably NH4F.
[0080] Preferably, the solution containing alkali metal hydroxide and fluoride is added dropwise to the first reaction solution at 20-30° C. In the solution containing alkali metal hydroxide and fluoride, solvent A is one or more of alcohol solvents, preferably one or more of methanol, propanol, isopropanol and butanol, more preferably methanol. The reaction is carried out at 20-30° C. for 8-12 hours.
[0081] The molar ratio of the terbium salt to the alkali metal hydroxide is 0.4:(0.8-1.5), preferably 0.4:(1-1.2), and more preferably 0.4: 1. The molar amount of the alkali metal hydroxide is based on the molar amount of the alkali metal element therein.
[0082] The molar ratio of the alkali metal hydroxide to the fluoride is 1:(2-6), preferably 1:(3-5), and more preferably 1: 4. The molar amount of the fluoride is calculated based on the molar amount of the fluorine element therein.
[0083] After the reaction is completed, the solvent A is removed and the reaction is heated again. The reaction temperature is 225-255° C., preferably 230-250° C., more preferably 235-245° C. The reaction time is 2-4 h, preferably 2.5-3.5 h.
[0084] Step C: post-treating the second reaction solution to obtain terbium-gadolinium nanocrystals coordinated with unsaturated fatty acids.
[0085] The post-treatment is to wait for the second reaction liquid to cool to room temperature, add a precipitation solvent to precipitate the product, centrifuge and wash to obtain terbium-gadolinium nanocrystals coordinated with unsaturated fatty acids.
[0086] Step D: adding the dispersion of the terbium-gadolinium nanocrystals coordinated with unsaturated fatty acids to a nitrosoboric acid tetrafluoroborate (NOBF4) solution, ultrasonically treating it, then adding solvent a, ultrasonically treating it again, centrifuging and washing it, to obtain ligand-free terbium-gadolinium nanocrystals.
[0087] In the dispersion of the terbium-gadolinium nanocrystals, the solvent 1-1 is one or more alkane solvents, preferably one or more alkane solvents with a carbon number of C5-C8, and more preferably n-hexane. The mass volume ratio of the terbium-gadolinium nanocrystals to the solvent 1-1 is 50 mg:(0.6-2.1) mL, preferably 50 mg:(0.8-1.8) mL, and more preferably 50 mg:(1-1.5) mL.
[0088] In the nitroso tetrafluoroborate (NOBF4) solution, solvent 1-2 is one or more of amide solvents, preferably N,N-dimethylformamide and / or N,N-dimethylacetamide. The concentration of the nitroso tetrafluoroborate (NOBF4) solution is 0.06-0.18 mol / mL, preferably 0.08-0.15 mol / mL, and more preferably 0.1 mol / mL.
[0089] The mass molar ratio of the terbium gadolinium nanocrystals to nitrous tetrafluoroborate is (30-70) mg:0.1 mmol, preferably (40-60) mg:0.1 mmol, and more preferably 50 mg:0.1 mmol.
[0090] The third aspect of the present invention also provides a diphenylphosphinobenzoic acid compound, which is represented by formula (1):
[0091]
[0092] Wherein, R0 is selected from hydrogen or a nitrogen-containing group, preferably hydrogen, carbazole, tert-butylcarbazole, dimethylacridinyl or diphenylacridinyl.
[0093] Preferably, the diphenylphosphinobenzoic acid compound is one of the following compounds:
[0094]
[0095]
[0096] More preferably, the diphenylphosphinobenzoic acid compound is one of Compound 1 to Compound 4.
[0097] The diphenylphosphinobenzoic acid compounds provided by the present invention can be used as ligands to react with the ligand-free terbium gadolinium nanocrystals to form terbium gadolinium nanocrystal particles wrapped with diphenylphosphinobenzoic acid compound ligands, thereby comprehensively improving the luminescence performance thereof. The threshold voltage of the electroluminescent device prepared by using the diphenylphosphinobenzoic acid compound as a luminescent layer material is significantly reduced, and the brightness, current efficiency, power efficiency and external quantum efficiency can be significantly improved.
[0098] The fourth aspect of the present invention also provides a method for preparing the diphenylphosphinobenzoic acid compound. The method specifically comprises the following steps:
[0099] Step 1. reacting halogenated toluene with magnesium to obtain a Grignard reagent, and then adding diphenylphosphine halide to react, and after oxidation, post-treatment is performed to obtain a diphenylphosphinooxytoluene compound.
[0100] Step 1 is carried out under anhydrous and oxygen-free conditions, such as under an argon atmosphere.
[0101] The halogenated toluene is:
[0102]
[0103] Wherein, X1 and X2 are each independently selected from hydrogen, a bromine substituent, an iodine substituent or a chlorine substituent, preferably selected from hydrogen, a bromine substituent or an iodine substituent.
[0104] Preferably, the halogenated toluene is 2-bromotoluene or 5-bromo-2-iodotoluene.
[0105] The molar ratio of the halogenated toluene to magnesium is 10:(7-18), preferably 10:(9-15), and more preferably 10:(11-13).
[0106] The halogenated toluene reacts with magnesium in an ether solvent, and the ether solvent is selected from one or more of aliphatic ethers having a carbon number of C1-C8, preferably one or more of methyl ether, ethyl ether, tetrahydrofuran, isopropyl ether and dimethyl ether, and more preferably ethyl ether. The molar volume ratio of the halogenated toluene to the ether solvent is 10mmol:(5-15mL), preferably 10mmol:(7-13mL), and more preferably 10mmol:(9-11mL). The Grignard reagent is cooled to -5 to 5°C, and diphenylphosphine halide is added dropwise. The diphenylphosphine halide is selected from one or more of diphenylphosphine chloride, diphenylphosphine bromide and diphenylphosphine iodide, and is preferably diphenylphosphine chloride. The molar ratio of the halogenated toluene to diphenylphosphine halide is 10:(7-18), preferably 10:(9-15), and more preferably 10:(11-13).
[0107] After the reaction is completed, water and dichloromethane are added for extraction, and the organic layer is obtained by merging. The oxidation is to add an oxidant to the organic layer. The oxidant is one or more of peroxides, preferably one or more of peroxyacids and hydrogen peroxide, more preferably hydrogen peroxide. The molar ratio of the oxidant to the halogenated toluene is (30-60):10, preferably (35-55):10, and more preferably (40-50):10.
[0108] After the oxidation reaction is completed, water and dichloromethane are added for extraction, and the organic layers are combined, dried, and purified by column chromatography to obtain diphenylphosphinoyltoluene compounds.
[0109] The diphenylphosphinoyl toluene compound is:
[0110]
[0111] Wherein, R1 is hydrogen, bromine substituent or chlorine substituent.
[0112] Optionally, carry out step 2. add a diphenylphosphinooxytoluene compound and a nitrogen-containing compound to solvent I, carry out a catalytic reaction in the presence of a catalyst, and perform post-treatment to obtain a diphenylphosphinooxytoluene compound having a nitrogen heterocyclic substituent.
[0113] Step 2 is carried out under anhydrous and oxygen-free conditions, such as under an argon atmosphere.
[0114] In step 2, the diphenylphosphinoyltoluene compound is:
[0115]
[0116] Wherein, R1 is a bromine substituent or a chlorine substituent.
[0117] The nitrogen-containing compound is selected from one or more of carbazole compounds and acridine compounds, preferably one or more of carbazole, 3,6-di-tert-butylcarbazole, 9,9-dimethylacridine and 9,10-dihydro-9,9-diphenylacridine, more preferably one or more of carbazole, 3,6-di-tert-butylcarbazole and 9,9-dimethylacridine.
[0118] The molar ratio of the nitrogen-containing compound to the diphenylphosphinoyltoluene compound is (10-48):10, preferably (11-40):10, and more preferably (12-32):10.
[0119] The solvent I is selected from one or more of aliphatic heterocyclic solvents and aromatic hydrocarbon solvents, preferably one or more of 1,3-dimethyl-2-imidazolidinone, N-methylpyrrolidone, imidazolidinyl urea, 2-pyrrolidone, toluene and xylene, more preferably 1,3-dimethyl-2-imidazolidinone or toluene. The volume molar ratio of the solvent I to the diphenylphosphinoyltoluene compound is (6-112) mL:10 mmol, preferably (8-107) mL:10 mmol, and more preferably (10-102) mL:10 mmol.
[0120] The reaction is carried out under alkaline conditions. An alkaline substance is added to the reaction solution, selected from one or more of carbonate, hydroxide, sodium alcoholate and potassium alcoholate, preferably one or more of carbonate, sodium alcoholate and potassium alcoholate. The molar ratio of the alkaline substance to the diphenylphosphinooxytoluene compound is (16-32):10, preferably (18-28):10, and more preferably (20-32):10.
[0121] The catalyst is a copper catalyst or a palladium catalyst. The copper catalyst is selected from one or more cuprous catalysts, preferably one or more cuprous halides, more preferably cuprous iodide. The palladium catalyst is selected from one or more palladium salts, palladium complexes and palladium carbon.
[0122] The molar ratio of the copper catalyst to the diphenylphosphinothiotoluene compound is (0.2-1.0):5, preferably (0.3-0.8):5, and more preferably (0.4-0.6):5.
[0123] The molar ratio of the palladium catalyst to the diphenylphosphinoyltoluene compound is (0.2-1.0):10, preferably (0.3-0.8):10, and more preferably (0.4-0.6):10.
[0124] The reaction temperature is 80-200° C., preferably 85-195° C., more preferably 90-190° C. The reaction time is 4-16 h, preferably 5-14 h, more preferably 6-12 h.
[0125] Step 3. Add a diphenylphosphinooxytoluene compound or a nitrogen heterocyclic substituted diphenylphosphinooxytoluene compound to solvent II, add potassium permanganate, heat to react, and post-treat to obtain a diphenylphosphinooxybenzoic acid compound.
[0126] The solvent II is selected from one or more of water and pyridine solvents, preferably selected from one or more of water, pyridine and alkyl pyridine, and more preferably a mixed solvent of water and pyridine, wherein the volume ratio of water to pyridine is 10:(20-30), preferably 10:25.
[0127] The molar ratio of potassium permanganate to diphenylphosphinooxytoluene compounds or nitrogen heterocyclic substituted diphenylphosphinooxytoluene compounds is (12-40):5, preferably (16-35):5, and more preferably (20-30):5.
[0128] The reaction temperature is 85-115° C., preferably 90-110° C., more preferably 95-105° C. The reaction time is 4-8 h, preferably 5-6 h.
[0129] After the reaction is completed, the product is treated with hydrochloric acid and purified by column chromatography to obtain a diphenylphosphinobenzoic acid compound.
[0130] The fifth aspect of the present invention provides a terbium-gadolinium nanocrystalline compound encapsulated by a diphenylphosphinobenzoic acid compound ligand.
[0131] The terbium-gadolinium nanocrystal compound wrapped by the diphenylphosphinobenzoic acid compound ligand is a terbium-gadolinium nanocrystal (MGd) coordinated with the diphenylphosphinobenzoic acid compound. (1-x) F4:xTb), denoted as MGd (1-x) F4:xTb@Ligand, wherein M is an alkali metal element, x is 0.1-0.9, preferably 0.3-0.5, more preferably 0.4. The alkali metal element is preferably Na and / or K, more preferably Na.
[0132] The terbium-gadolinium nanocrystal compound coated with a diphenylphosphinobenzoic acid compound ligand is obtained by reacting terbium-gadolinium nanocrystals without ligand coating with a diphenylphosphinobenzoic acid compound.
[0133] The sixth aspect of the present invention provides a method for preparing the terbium-gadolinium nanocrystalline compound encapsulated by the diphenylphosphinobenzoic acid compound ligand, the method specifically comprising the following steps:
[0134] Step a. Add the dispersion of the terbium-gadolinium nanocrystals coordinated with unsaturated fatty acids to a nitrosoboric acid tetrafluoroborate (NOBF4) solution, perform ultrasonic treatment, then add solvent a, perform ultrasonic treatment again, centrifuge and wash to obtain terbium-gadolinium nanocrystals without ligand coating.
[0135] In the dispersion of the terbium-gadolinium nanocrystals, the solvent 1-1 is one or more alkane solvents, preferably one or more alkane solvents with a carbon number of C5-C8, and more preferably n-hexane. The mass volume ratio of the terbium-gadolinium nanocrystals to the solvent 1-1 is 50 mg:(0.6-2.1) mL, preferably 50 mg:(0.8-1.8) mL, and more preferably 50 mg:(1-1.5) mL.
[0136] In the nitroso tetrafluoroborate (NOBF4) solution, solvent 1-2 is one or more of amide solvents, preferably N,N-dimethylformamide and / or N,N-dimethylacetamide. The concentration of the nitroso tetrafluoroborate (NOBF4) solution is 0.06-0.18 mol / mL, preferably 0.08-0.15 mol / mL, and more preferably 0.1 mol / mL.
[0137] The mass molar ratio of the terbium gadolinium nanocrystals to nitrous tetrafluoroborate is (30-70) mg:0.1 mmol, preferably (40-60) mg:0.1 mmol, and more preferably 50 mg:0.1 mmol.
[0138] Step b. adding the terbium-gadolinium nanocrystals without ligand coating to a diphenylphosphinobenzoic acid compound solution, subjecting to ultrasonic treatment, and repeating centrifugation, washing, and centrifugation to obtain the terbium-gadolinium nanocrystals compound coated with the diphenylphosphinobenzoic acid compound ligand.
[0139] The diphenylphosphinobenzoic acid compound solution is further added with an alkaline substance selected from one or more hydroxides, preferably one or more alkali metal hydroxides, more preferably potassium hydroxide and / or sodium hydroxide, and the solvent is selected from one or more alcohol solvents, ether solvents and ester solvents, preferably one or more alcohol solvents with a carbon number of C1-C5, more preferably ethanol. The molar ratio of the diphenylphosphinobenzoic acid compound to the alkaline substance is 1:(1-2), preferably 1:(1-1.5), more preferably 1:1. The molar volume ratio of the diphenylphosphinobenzoic acid compound to the solvent is 1mmol:(30-55)mL, preferably 1mmol:(35-50)mL, more preferably 1mmol:(40-45)mL.
[0140] The molar ratio of the terbium gadolinium nanocrystals without ligand coating to the diphenylphosphinobenzoic acid compound is 1:(30-70), preferably 1:(40-60), and more preferably 1:50.
[0141] The seventh aspect of the present invention also provides an electroluminescent device, which includes a light-emitting layer, and also includes an anode conductive layer, a hole injection layer, a hole transport layer, a hole blocking layer, an electron transport layer, an electron injection layer and a cathode conductive layer.
[0142] The raw materials for preparing the light-emitting layer include one or more of the terbium gadolinium nanocrystals described in the first aspect and the terbium gadolinium nanocrystals wrapped with diphenylphosphinobenzoic acid compound ligands described in the fifth aspect, preferably include one or more of the terbium gadolinium nanocrystals wrapped with diphenylphosphinobenzoic acid compound ligands described in the fifth aspect, and more preferably include one or more of the terbium gadolinium nanocrystals wrapped with compounds 1 to 4.
[0143] The eighth aspect of the present invention provides a method for preparing the electroluminescent device. The method specifically comprises the following steps:
[0144] 1. preparing a conductive anode layer;
[0145] The conductive anode layer is prepared on the substrate layer. The conductive anode layer is selected from tin oxide conductive glass (ITO), transparent conductive polymers such as polyaniline, and semi-transparent metals such as Au, preferably ITO or semi-transparent metals, and more preferably ITO.
[0146] Preferably, the glass or plastic substrate cleaned with deionized water is placed in a vacuum evaporator with a vacuum degree of 1×10 - 6 mbar, the evaporation rate is set to 0.1-0.3 nm / s, and the evaporation material is indium tin oxide (ITO) on the glass or plastic substrate, and the thickness of the anode conductive layer is 1-100 nm;
[0147] Preferably, the following hole injection layer, hole transport layer and light emitting layer are prepared by spin coating, and the following hole blocking layer, electron transport layer, electron injection layer and cathode conductive layer are prepared by vacuum evaporation.
[0148] 2. preparing a hole injection layer;
[0149] The hole injection layer is spin-coated on the anode conductive layer, and the spin-coating thickness is 40-60nm, preferably 45-55nm, and more preferably 40nm;
[0150] The hole injection layer material is poly(3,4-ethylenedioxythiophene):poly(styrenesulfonic acid) (PEDOT:PSS), and the volume ratio of poly(3,4-ethylenedioxythiophene):poly(styrenesulfonic acid) (PEDOT:PSS) to deionized water is 1:1, and it is spin-coated on a pre-cleaned ITO glass substrate at 2000-2500 rpm, and then dried at 105-120° C. for 15-30 minutes.
[0151] 3. Preparation of hole transport layer;
[0152] The hole transport layer is spin-coated on the hole injection layer, and the spin-coating thickness is 10-30 nm, preferably 15-25 nm, and more preferably 20 nm.
[0153] The hole transport layer material is selected from polyvinyl carbazole (PVK).
[0154] 4. preparing a light-emitting layer;
[0155] The light-emitting layer is spin-coated on the hole transport layer, and the spin-coating thickness is 15-35 nm, preferably 20-30 nm, and more preferably 25 nm.
[0156] The light-emitting layer material is a mixture of one or more of the terbium-gadolinium nanocrystals described in the first aspect, the terbium-gadolinium nanocrystals without ligand coating obtained in the sixth aspect, and the terbium-gadolinium nanocrystals coated with diphenylphosphinobenzoic acid compound ligands described in the fifth aspect and a host material.
[0157] The main material is selected from one or more of 9,9'-(1,3-phenyl)di-9H-carbazole (mCP), bis-4(N-carbazolylphenyl)phenylphosphine oxide (BCPO), 4,4-bis(9-carbazole)biphenyl (CBP), 4,4'-bis(9H-carbazole-9-yl)-2,2'-dimethylbiphenyl (CDBP), (4-(9H-carbazole-9-yl)-2-methylphenyl)diphenylphosphine oxide (CPPOM), 9-(4-tert-butylphenyl)-3,6-bis(triphenylsilyl)-9h-carbazole (CzSi), bis[2-((oxy)diphenylphosphino)phenyl]ether (DPEPO) and polyvinylcarbazole (PVK), preferably 9,9'-(1,3-phenyl)di-9H-carbazole (mCP). The mass fraction of the column material is 40%-80%.
[0158] 5. preparing a hole blocking layer;
[0159] The hole blocking layer is evaporated on the light-emitting layer, and the evaporated thickness is 4-20 nm, preferably 8-12 nm, and more preferably 10 nm.
[0160] The hole blocking layer material is bis[2-((oxy)diphenylphosphino)phenyl]ether (DPEPO).
[0161] 6. Preparation of electron transport layer;
[0162] The electron transport layer is evaporated on the hole blocking layer, and the evaporated thickness is 30-55 nm, preferably 35-45 nm, and more preferably 40 nm.
[0163] The electron transport layer material is 3,3'-[5'-[3-(3-pyridyl)phenyl][1,1':3',1"-terphenyl]-3,3"-diyl]bipyridine (TmPyPB).
[0164] 7. preparing an electron injection layer;
[0165] The electron injection layer is evaporated on the electron transport layer, and the evaporated thickness is 1-10 nm, preferably 1-5 nm, and more preferably 1 nm.
[0166] The electron injection layer material is LiF.
[0167] 8. Prepare a cathode conductive layer, encapsulate, and obtain an organic-inorganic hybrid rare earth luminescent nanoparticle electroluminescent device.
[0168] The cathode conductive layer is deposited on the electron injection layer, and the deposition thickness is 80-120 nm, preferably 90-110 nm, and more preferably 100 nm. The cathode conductive layer is made of metal aluminum.
[0169] Example
[0170] Example 1
[0171] GdCl3·6H2O (0.6mmol), TbCl3·6H2O (0.4mmol), 6mL oleic acid, 15mL 1-octadecene were mixed together and heated to 140°C for 3h, then cooled to room temperature, 10mL of NaOH and NH4F methanol solution (containing 1mmol NaOH, 4mmol NH4F) were added dropwise thereto, and reacted at room temperature for 12h. The reaction mixture was then heated at 70°C to remove methanol, then placed under a gentle argon flow, heated to 240°C for 45min, then cooled to room temperature, ethanol was added to precipitate the product, centrifuged, and washed with ethanol to obtain terbium gadolinium crystal nanoparticles (NaGd 0.6 F4: 0.4Tb@OA nanoparticles).
[0172] NaGd 0.6 F4: a mixture of 0.4Tb@OA nanoparticles and mCP (where NaGd 0.6 F4: 0.4Tb@OA nanoparticles (mass fraction 30%) are used as the light-emitting layer material to prepare an electroluminescent device, and the process is as follows:
[0173] 1. Place the glass substrate cleaned with deionized water into a vacuum evaporator with a vacuum degree of 1×10 -6 mbar, the evaporation rate is set to 0.1-0.3 nm / s, such as 0.1 nm / s, and the evaporation material on the glass substrate is indium tin oxide (ITO) with a thickness of 1-100 nm, such as 100 nm of the anode conductive layer.
[0174] 2. Spin-coat the hole injection layer material PEDOT:PSS on the anode conductive layer. The volume ratio of PEDOT:PSS to deionized water is 1:1. Spin-coat on the pre-cleaned ITO glass substrate at 2000 rpm and then dry at 120°C for 15 minutes to obtain a hole injection layer with a thickness of 40 nm.
[0175] 3. Spin-coat the hole transport layer material polyvinyl carbazole (PVK) on the hole injection layer to obtain a hole transport layer with a thickness of 20 nm.
[0176] 4. Spin coating the light-emitting layer material on the hole transport layer: NaGd 0.6 F4: a mixture of 0.4Tb@OA nanoparticles and mCP, in which NaGd 0.6 F4: The mass fraction of 0.4Tb@OA nanoparticles is 30%, and a light-emitting layer with a thickness of 25 nm is obtained.
[0177] 5. The hole blocking layer material DPEPO is evaporated on the light-emitting layer to obtain a hole blocking layer with a thickness of 10 nm.
[0178] 6. The electron transport layer material TmPyPB is evaporated on the hole blocking layer to obtain an electron transport layer with a thickness of 40 nm.
[0179] 7. The electron injection layer material LiF is evaporated on the electron transport layer to obtain an electron injection layer with a thickness of 1 nm.
[0180] 8. A cathode conductive layer whose material is aluminum and whose thickness is 100 nm is evaporated on the electron injection layer to obtain an electroluminescent device.
[0181] The structure of the electroluminescent device in this embodiment is: ITO / PEDOT:PSS (40nm) / PVK (20nm) / mCP:NaGd 0.6 F4:0.4Tb@OA(30%)(25nm) / DPEPO(10nm) / TmPyPB(40nm) / LiF(1nm) / Al(100nm).
[0182] The current density of the electroluminescent device is tested to show the changing trend of the current density with the change of voltage. The voltage-current density relationship curve is as follows: Figure 4 As shown, the threshold voltage of the device is 6.4V.
[0183] The brightness of the electroluminescent device is tested to show the change trend of voltage. The voltage-brightness relationship curve is as follows: Figure 5 As shown in Figure 2, the maximum brightness of the device can reach 1.956 cd·m -2 .
[0184] The current efficiency of the electroluminescent device is tested to show the trend of change with brightness. The brightness-current efficiency relationship curve is as follows: Figure 6 As shown in the figure, the device has a brightness of 0.8522 cd·m -2 When the current efficiency reaches the maximum value of 0.78545cd·A -1 .
[0185] The power efficiency of the electroluminescent device is tested to see how it changes with brightness. The brightness-power efficiency relationship curve is as follows: Figure 7 As shown in the figure, the device has a brightness of 0.8522 cd·m -2 When the power efficiency reaches the maximum value of 0.41105lm·W -1 .
[0186] The change trend of the external quantum efficiency of the electroluminescent device to the change of current density is tested. The relationship curve between brightness and external quantum efficiency is as follows: Figure 8 As shown in the figure, the device has a brightness of 0.8522 cd·m-2 When , the maximum external quantum efficiency of 0.47127% is obtained.
[0187] The electroluminescence spectrum of the electroluminescent device is shown in FIG. Fig. 9 As shown by Fig. 9 It can be seen that the electroluminescence peak of the device is at 544nm.
[0188] Example 2
[0189] At room temperature, 1 mL of the terbium-gadolinium nanocrystal particles (NaGd 0.6 The dispersion of F4:0.4Tb@OA nanoparticles in n-hexane (50 mg / mL) was mixed with 1 mL NOBF4 in N,N-dimethylformamide (0.1 mmol / mL), and the surface oleic acid ligands were removed by ultrasonic treatment for 30 min. Then, 1 mL toluene was added, ultrasonic treatment was performed for 30 min, and centrifugation was performed to further purify the mixture. An appropriate amount of toluene and n-hexane mixed solution was added, ultrasonic treatment was performed, centrifugation was performed, and the mixture was dispersed with ethanol to obtain NaGd without ligand coating. 0.6 F4: 0.4Tb nanoparticles.
[0190] Ligand-free NaGd 0.6 F4: A mixture of 0.4Tb nanoparticles and mCP (without ligand NaGd 0.6 F4: 0.4Tb nanoparticles (mass fraction is 60%) are used as the light-emitting layer material to prepare an electroluminescent device, and the process is as follows:
[0191] 1. Place the glass substrate cleaned with deionized water into a vacuum evaporator with a vacuum degree of 1×10 -6 mbar, the evaporation rate is set to 0.1-0.3 nm / s, such as 0.1 nm / s, and the evaporation material on the glass substrate is indium tin oxide (ITO), and the thickness is 1-100 nm, such as 100 nm of the anode conductive layer;
[0192] 2. Spin-coat the hole injection layer material PEDOT:PSS on the anode conductive layer. The volume ratio of PEDOT:PSS to deionized water is 1:1. Spin-coat it on the pre-cleaned ITO glass substrate at 2000 rpm and then dry it at 120°C for 15 minutes. A hole injection layer with a thickness of 40 nm is obtained.
[0193] 3. Spin-coating a hole transport layer material, polyvinyl carbazole (PVK), on the hole injection layer to obtain a hole transport layer with a thickness of 20 nm;
[0194] 4. Spin coating the light-emitting layer material on the hole transport layer: ligand-free NaGd 0.6 F4: A mixture of 0.4Tb nanoparticles and mCP, without ligand NaGd 0.6F4: The mass fraction of 0.4Tb nanoparticles is 60%, and a light-emitting layer with a thickness of 25nm is obtained;
[0195] 5. Evaporating a hole blocking layer material DPEPO on the light-emitting layer to obtain a hole blocking layer with a thickness of 10 nm;
[0196] 6. Evaporating the electron transport layer material TmPyPB on the hole blocking layer to obtain an electron transport layer with a thickness of 40 nm;
[0197] 7. Vapor depositing LiF, an electron injection layer material, on the electron transport layer to obtain an electron injection layer with a thickness of 1 nm;
[0198] 8. A cathode conductive layer whose material is aluminum and whose thickness is 100 nm is evaporated on the electron injection layer to obtain an electroluminescent device.
[0199] The structure of the electroluminescent device in this embodiment is: ITO / PEDOT:PSS (40nm) / PVK (20nm) / mCP:NaGd 0.6 F4:0.4Tb(60%)(25nm) / DPEPO(10nm) / TmPyPB(40nm) / LiF(1nm) / Al(100nm).
[0200] The current density of the electroluminescent device is tested to show the changing trend of the current density with the change of voltage. The voltage-current density relationship curve is as follows: Figure 4 As shown, the threshold voltage of the device is 7.6V.
[0201] The brightness of the electroluminescent device is tested to show the change trend of voltage. The voltage-brightness relationship curve is as follows: Figure 5 As shown in Figure 2, the maximum brightness of the device can reach 8.414 cd·m -2 .
[0202] The current efficiency of the electroluminescent device is tested to show the trend of change with brightness. The brightness-current efficiency relationship curve is as follows: Figure 6 As shown, the device has a brightness of 1.495 cd·m -2 When the current efficiency reaches the maximum value of 0.14853cd·A -1 .
[0203] The power efficiency of the electroluminescent device is tested to see how it changes with brightness. The brightness-power efficiency relationship curve is as follows: Figure 7 As shown in the figure, the device has a brightness of 1.495 cd·m -2 When the power efficiency reaches the maximum value of 0.0583lm·W -1 .
[0204] The change trend of the external quantum efficiency of the electroluminescent device to the change of current density is tested. The relationship curve between brightness and external quantum efficiency is as follows: Figure 8 As shown in the figure, the device has a brightness of 1.495 cd·m -2 When , the maximum external quantum efficiency of 0.07738% was obtained.
[0205] The electroluminescence spectrum of the electroluminescent device is shown in FIG. Fig. 9 As shown by Fig. 9 It can be seen that the electroluminescence peaks of the device are at 488nm, 544nm, 584nm, and 620nm.
[0206] Example 3
[0207] Under anhydrous and oxygen-free conditions, 2-bromotoluene (1.19 ml, about 10 mmol) was prepared into a Grignard reagent with a magnesium stick (0.27 g, about 11 mmol) in 10 mL of ether, and reacted at 40°C for 1 h. The mixture was cooled to 0°C, and diphenylphosphine chloride (1.98 ml, about 11 mmol) was added dropwise. The reaction was continued for 12 h at a reaction temperature of 0°C. The mixture was extracted with water and dichloromethane, and the organic layers were combined. The mixture was oxidized with H2O2 (30 wt% hydrogen peroxide solution containing about 40 mmol H2O2), and then extracted with water and dichloromethane. The organic layers were combined, dried, and purified by column chromatography with petroleum ether and ethyl acetate as the eluent to obtain precursor 1.
[0208]
[0209] Precursor 1 (1.46 g, about 5 mmol) was added to a mixed solution of pyridine (25 ml) and water (10 ml), and potassium permanganate (3.16 g, about 20 mmol) was added four times, reacted at 100°C for 5 hours, treated with aqueous hydrochloric acid, and purified by column chromatography. The eluent was a mixed solvent of dichloromethane and methanol to obtain compound 1 (TPPOA).
[0210]
[0211] Compound 1 was analyzed by hydrogen nuclear magnetic resonance spectrum, and the test data were: 1 H NMR (TMS, DMSO-d6, 400MHz): δ = 13.086 (s, 1H), 7.857 (q, J1 = 7.2Hz, J2 = 3.6Hz, 1H),7.697(t,J=7.2Hz,1H),7.624(t,J=7.2Hz,1H),7.587-7.477ppm(m,11H).
[0212] The electrochemical properties of compound 1 were tested, and the cyclic voltammetry curve was obtained as follows: Figure 1As shown. Glassy carbon was used as the working electrode, platinum wire as the comparison electrode, and Ag / AgCl as the reference electrode. By cyclic voltammetry, the HOMO energy level of compound 1 was measured to be -6.508 eV, and the LUMO energy level was -3.192 eV.
[0213] Compound 1 (0.0468 mol) and sodium hydroxide (0.0468 mol) were added to 2 mL of ethanol solution and ultrasonicated until the solution was clear. 0.6 F4: 0.4Tb nanoparticles mixed (ligand-free NaGd 0.6 The molar ratio of F4:0.4Tb nanoparticles to compound 1 was 1:50), ultrasonicated for 2 h, then centrifuged, the supernatant was removed, and the precipitate was washed three times with ethanol to obtain NaGd 0.6 F4:0.4Tb@TPPOA nanoparticles.
[0214] NaGd 0.6 F4:0.4Tb@TPPOA nanoparticles were tested for UV-visible light absorption spectrum, and the spectrum is shown in the figure below. Figure 2 As shown, there is an absorption peak at 274nm.
[0215] NaGd 0.6 F4: 0.4Tb@TPPOA nanoparticles were tested for photoluminescence spectrum, and its spectrum is shown in the figure below. Figure 3 As shown, there are emission peaks at 488nm, 543nm, 584nm, and 620nm.
[0216] NaGd 0.6 F4: a mixture of 0.4Tb@TPPOA nanoparticles and mCP (where NaGd 0.6 F4: 0.4Tb@TPPOA nanoparticles (mass fraction is 20%) are used as the light-emitting layer material to prepare an electroluminescent device, and the process is as follows:
[0217] 1. Place the glass substrate cleaned with deionized water into a vacuum evaporator with a vacuum degree of 1×10 -6 mbar, the evaporation rate is set to 0.1-0.3nm / s, such as 0.1nm / s, and the evaporation material on the glass substrate is indium tin oxide (ITO), and the thickness is 1-100nm, such as 100nm of the anode conductive layer (the thickness of the anode conductive layer is);
[0218] 2. Spin-coat the hole injection layer material PEDOT:PSS on the anode conductive layer. The volume ratio of PEDOT:PSS to deionized water is 1:1. Spin-coat it on the pre-cleaned ITO glass substrate at 2000 rpm and then dry it at 120°C for 15 minutes. A hole injection layer with a thickness of 40 nm is obtained.
[0219] 3. Spin-coating a hole transport layer material, polyvinyl carbazole (PVK), on the hole injection layer to obtain a hole transport layer with a thickness of 20 nm;
[0220] 4. Spin coating the light-emitting layer material on the hole transport layer: NaGd 0.6 F4: a mixture of 0.4Tb@TPPOA nanoparticles and mCP, in which NaGd 0.6 F4: The mass fraction of 0.4Tb@TPPOA nanoparticles is 20%, and a light-emitting layer with a thickness of 25 nm is obtained;
[0221] 5. Evaporating a hole blocking layer material DPEPO on the light-emitting layer to obtain a hole blocking layer with a thickness of 10 nm;
[0222] 6. Evaporating the electron transport layer material TmPyPB on the hole blocking layer to obtain an electron transport layer with a thickness of 40 nm;
[0223] 7. Vapor depositing LiF, an electron injection layer material, on the electron transport layer to obtain an electron injection layer with a thickness of 1 nm;
[0224] 8. A cathode conductive layer whose material is aluminum and whose thickness is 100 nm is evaporated on the electron injection layer to obtain an electroluminescent device.
[0225] The structure of the electroluminescent device in this embodiment is: ITO / PEDOT:PSS (40nm) / PVK (20nm) / mCP:NaGd 0.6 F4:0.4Tb@TPPOA(20%)(25nm) / DPEPO(10nm) / TmPyPB(40nm) / LiF(1nm) / Al(100nm).
[0226] The current density of the electroluminescent device was tested to determine the variation trend of the current density with the voltage. The voltage-current density relationship curve is shown in FIG. Figure 4 As shown, the threshold voltage of the device is 5.3V.
[0227] The brightness of the electroluminescent device is tested to see how it changes with voltage. The voltage-brightness relationship curve is as follows: Figure 5 As shown in Figure 2, the maximum brightness of the device can reach 13.07 cd·m -2 .
[0228] The current efficiency of the electroluminescent device was tested to determine the variation trend of the current efficiency with the change of brightness. The brightness-current efficiency relationship curve is shown in FIG. Figure 6 As shown, the device has a brightness of 1.347 cd·m -2 When the current efficiency reaches the maximum value of 0.85371cd·A -1 .
[0229] The power efficiency of the electroluminescent device was tested to see how it changes with brightness. The brightness-power efficiency relationship curve is shown in Figure 7 As shown in the figure, the device has a brightness of 1.347 cd·m -2 When the power efficiency reaches the maximum value of 0.50578lm·W -1 .
[0230] The change trend of the external quantum efficiency of the electroluminescent device to the change of current density is tested, and the relationship curve between brightness and external quantum efficiency is as follows: Figure 8 As shown in the figure, the device has a brightness of 1.347 cd·m -2 When , the maximum external quantum efficiency of 0.53784% was obtained.
[0231] The electroluminescence spectrum of the electroluminescent device is shown in FIG. Fig. 9 As shown by Fig. 9 It can be seen that the electroluminescence peaks of the device are at 488nm, 544nm, 584nm, and 620nm.
[0232] Example 4
[0233] Under anhydrous and oxygen-free conditions, 5-bromo-2-iodotoluene (2.96 g, about 10 mmol) was prepared into a Grignard reagent with a magnesium stick (0.27 g, about 11 mmol) in 10 mL of ether, and reacted at 40°C for 1 h. The mixture was cooled to 0°C, and diphenylphosphine chloride (1.98 ml, about 11 mmol) was added dropwise. The mixture was reacted for 12 h, extracted with water and dichloromethane, and the organic layers were combined. The mixture was oxidized with H2O2 (30 wt% aqueous hydrogen peroxide solution, containing about 40 mmol of H2O2), and then extracted with water and dichloromethane. The organic layers were combined, dried, and purified by column chromatography with petroleum ether and ethyl acetate as eluents to obtain precursor 2.
[0234]
[0235] Under anhydrous and oxygen-free conditions, precursor 2 (1.856 g, about 5 mmol) was mixed with carbazole (2.508 g, about 15 mmol), cuprous iodide (0.095 g, about 0.5 mmol), and potassium carbonate (2.073 g, about 15 mmol) in 1,3-dimethyl-2-imidazolidinone (50 ml), and the mixture was heated to 190 ° C and stirred for 12 hours. It was naturally cooled to room temperature and poured into water. An appropriate amount of dichloromethane was added to extract the collected organic layer and dried with anhydrous sodium sulfate, and the solvent in the organic layer was removed in vacuo, and purified by column chromatography, with dichloromethane and ethyl acetate as the eluent to obtain precursor 3.
[0236]
[0237] Precursor 3 (2.28 g, about 5 mmol) was added to a mixed solution of pyridine (25 ml) and water (10 ml), and then potassium permanganate (3.16 g, about 20 mmol) was added in four portions. The mixture was reacted at 100 °C for 5 h. After the reaction, 6 mmol / mL hydrochloric acid was added and purified by column chromatography with dichloromethane and methanol as the eluent to obtain compound 2 (CzPPOA).
[0238]
[0239] Compound 2 was analyzed by hydrogen nuclear magnetic resonance spectrum, and the test data were: 1 H NMR (TMS, DMSO-d6, 400MHz): δ = 13.398 (s, 1H), 8.273 (d, J = 7.6Hz, 2H), 8.100 (t, J = 2.4Hz, 1H), 7.994 (d, J = 8.4Hz, 1H), 7.814 (q,J1=8.4Hz, J2=13.2Hz,1H),7.705-7.658(m,4H),7.632-7.649(m,8H),7.484(t,J=7.6Hz,2H),7.349ppm(t,J=7.2Hz,2H).
[0240] The electrochemical properties of compound 2 were tested, and the cyclic voltammetry curve was as follows: Figure 1 As shown. Glassy carbon was used as the working electrode, platinum wire as the comparison electrode, and Ag / AgCl as the reference electrode. By cyclic voltammetry, the HOMO energy level of compound 2 was measured to be -6.186 eV, and the LUMO energy level was -3.278 eV.
[0241] 0.0468 mol of compound 2 and 0.0468 mol of sodium hydroxide were added to 2 mL of ethanol solution and ultrasonicated until the solution was clear. 0.6 F4: 0.4Tb nanoparticles mixed (NaGd 0.6 The molar ratio of F4:0.4Tb nanoparticles to compound 2 was 1:50), ultrasonicated for 2 h, then centrifuged, the supernatant was removed, and the precipitate was washed three times with ethanol to obtain NaGd 0.6 F4: 0.4Tb@CzPPOA nanoparticles.
[0242] Testing NaGd 0.6 F4: UV-visible absorption spectrum of 0.4Tb@CzPPOA nanoparticles, such as Figure 2 As shown, there are absorption peaks at 293nm and 339nm.
[0243] Testing NaGd 0.6F4: Photoluminescence spectrum of 0.4Tb@CzPPOA nanoparticles, such as Figure 3 As shown, there are emission peaks at 489nm, 544nm, 585nm, and 620nm.
[0244] NaGd 0.6 F4: a mixture of 0.4Tb@CzPPOA nanoparticles and mCP (where NaGd 0.6 F4: 0.4Tb@CzPPOA nanoparticles (mass fraction is 25%) are used as the light-emitting layer material to prepare an electroluminescent device, and the process is as follows:
[0245] 1. Place the glass substrate cleaned with deionized water into a vacuum evaporator with a vacuum degree of 1×10 -6 mbar, the evaporation rate is set to 0.1-0.3 nm / s, such as 0.1 nm / s, and the evaporation material on the glass substrate is indium tin oxide (ITO), and the thickness is 1-100 nm, such as 100 nm of the anode conductive layer;
[0246] 2. Spin-coat the hole injection layer material PEDOT:PSS on the anode conductive layer. The volume ratio of PEDOT:PSS to deionized water is 1:1. Spin-coat it on the pre-cleaned ITO glass substrate at 2000 rpm and then dry it at 120°C for 15 minutes. A hole injection layer with a thickness of 40 nm is obtained.
[0247] 3. Spin-coating a hole transport layer material, polyvinyl carbazole (PVK), on the hole injection layer to obtain a hole transport layer with a thickness of 20 nm;
[0248] 4. Spin coating the light-emitting layer material on the hole transport layer: NaGd 0.6 F4: a mixture of 0.4Tb@CzPPOA nanoparticles and mCP, in which NaGd 0.6 F4: The mass fraction of 0.4Tb@CzPPOA nanoparticles is 25%, and the thickness of the light-emitting layer is 25 nm;
[0249] 5. Evaporating a hole blocking layer material DPEPO on the light-emitting layer to obtain a hole blocking layer with a thickness of 10 nm;
[0250] 6. Evaporating the electron transport layer material TmPyPB on the hole blocking layer to obtain an electron transport layer with a thickness of 40 nm;
[0251] 7. Vapor depositing LiF, an electron injection layer material, on the electron transport layer to obtain an electron injection layer with a thickness of 1 nm;
[0252] 8. A cathode conductive layer whose material is aluminum and whose thickness is 100 nm is evaporated on the electron injection layer to obtain an electroluminescent device.
[0253] The structure of the electroluminescent device in this embodiment is: ITO / PEDOT:PSS (40nm) / PVK (20nm) / mCP:NaGd 0.6 F4:0.4Tb@CzPPOA(25%)(25nm) / DPEPO(10nm) / TmPyPB(40nm) / LiF(1nm) / Al(100nm).
[0254] The current density of the electroluminescent device is tested to show the changing trend of the current density with the change of voltage. The voltage-current density relationship curve is as follows: Figure 4 As shown, the threshold voltage of the device is 5.5V.
[0255] The brightness of the electroluminescent device is tested to show the change trend of voltage. The voltage-brightness relationship curve is as follows: Figure 5 As shown in Figure 2, the maximum brightness of the device can reach 33.51 cd·m -2 .
[0256] The current efficiency of the electroluminescent device is tested to show the trend of change with brightness. The brightness-current efficiency relationship curve is as follows: Figure 6 As shown in the figure, the device has a brightness of 0.9633 cd·m -2 When the current efficiency reaches the maximum value of 9.19179cd·A -1 .
[0257] The power efficiency of the electroluminescent device is tested to see how it changes with brightness. The brightness-power efficiency relationship curve is as follows: Figure 7 As shown in the figure, the device has a brightness of 0.9633 cd·m -2 When the power efficiency reaches the maximum value of 5.24768lm·W -1 .
[0258] The change trend of the external quantum efficiency of the electroluminescent device to the change of current density is tested. The relationship curve between brightness and external quantum efficiency is as follows: Figure 8 As shown in the figure, the device has a brightness of 0.9633 cd·m -2 When , the maximum external quantum efficiency of 5.46912% is obtained.
[0259] The electroluminescence spectrum of the electroluminescent device is shown in FIG. Fig. 9 As shown by Fig. 9 It can be seen that the electroluminescence peaks of the device are at 488nm, 544nm, 584nm, and 620nm.
[0260] Example 5
[0261] Under anhydrous and oxygen-free conditions, the precursor 2 (1.856 g, about 5 mmol) was mixed with tert-butyl carbazole (4.19 g, about 15 mmol), cuprous iodide (0.095 g, about 0.5 mmol), and potassium carbonate (2.073 g, about 15 mmol) in 1,3-dimethyl-2-imidazolidinone (50 ml), and the mixture was heated to 190 ° C and stirred for 12 hours. It was naturally cooled to room temperature and poured into water. The organic layer was collected by extraction with dichloromethane and dried with anhydrous sodium sulfate, and the solvent in the organic layer was removed by vacuum, and purified by column chromatography, with dichloromethane and ethyl acetate as the eluent to obtain the precursor 4.
[0262]
[0263] Precursor 4 (2.8 g, about 5 mmol) was added to a mixed solution of pyridine (25 ml) and water (10 ml), and potassium permanganate (3.16 g, about 20 mmol) was then added four times, and the mixture was reacted at 100°C for 5 h. After the reaction, hydrochloric acid (6 mmol / mL) was added, and the mixture was purified by column chromatography with dichloromethane and methanol as eluents to obtain compound 3 (tBCzPPOA).
[0264]
[0265] Compound 3 was analyzed by hydrogen nuclear magnetic resonance spectrum, and the test data were: 1 H NMR (TMS, DMSO-d6, 400MHz): δ = 13.352 (s, 1H), 8.320 (s, 2H), 8.073 (s, 1H), 7.973 (d, J = 6.8Hz, 1H), 7.786-7.492 (m, 15H), 1.412ppm (s, 18H).
[0266] The electrochemical properties of compound 3 were tested, and the cyclic voltammetry curve was as follows: Figure 1 As shown. Glassy carbon was used as the working electrode, platinum wire as the comparison electrode, and Ag / AgCl as the reference electrode. By cyclic voltammetry, the HOMO energy level of compound 1 was measured to be -6.058 eV, and the LUMO energy level was -3.236 eV.
[0267] 0.0468 mol of compound 3 and 0.0468 mol of sodium hydroxide were added to 2 mL of ethanol solution and ultrasonicated until the solution was clear. 0.6 F4: 0.4Tb nanoparticles mixed (ligand-free NaGd 0.6 The molar ratio of F4:0.4Tb nanoparticles to compound 3 was 1:50), ultrasonicated for 2 h, then centrifuged, the supernatant was removed, and the precipitate was washed three times with ethanol to obtain NaGd0.6 F4:0.4Tb@tBCzPPOA nanoparticles.
[0268] NaGd 0.6 F4:0.4Tb@tBCzPPOA nanoparticles were tested for UV-visible light absorption spectrum, and the spectrum is shown in the figure below. Figure 2 As shown, there are absorption peaks at 298nm and 345nm.
[0269] NaGd 0.6 F4:0.4Tb@tBCzPPOA nanoparticles were tested for photoluminescence spectrum, and its spectrum is shown in the figure below. Figure 3 As shown, there are emission peaks at 489nm, 544nm, 585nm, and 620nm.
[0270] NaGd 0.6 F4: a mixture of 0.4Tb@tBCzPPOA nanoparticles and mCP (where NaGd 0.6 F4: 0.4Tb@tBCzPPOA nanoparticles (mass fraction is 30%) are used as the light-emitting layer material to prepare an electroluminescent device, and the process is as follows:
[0271] 1. Place the glass substrate cleaned with deionized water into a vacuum evaporator with a vacuum degree of 1×10 -6 mbar, the evaporation rate is set to 0.1-0.3 nm / s, such as 0.1 nm / s, and indium tin oxide (ITO) is evaporated on the glass substrate to obtain an anode conductive layer with a thickness of 1-100 nm, such as 100 nm;
[0272] 2. Spin-coat the hole injection layer material PEDOT:PSS on the anode conductive layer. The volume ratio of PEDOT:PSS to deionized water is 1:1. Spin-coat it on the pre-cleaned ITO glass substrate at 2000 rpm and then dry it at 120°C for 15 minutes. A hole injection layer with a thickness of 40 nm is obtained.
[0273] 3. Spin-coating a hole transport layer material, polyvinyl carbazole (PVK), on the hole injection layer to obtain a hole transport layer with a thickness of 20 nm;
[0274] 4. Spin coating the light-emitting layer material on the hole transport layer: NaGd 0.6 F4: a mixture of 0.4Tb@tBCzPPOA nanoparticles and mCP, in which NaGd 0.6 F4: The mass fraction of 0.4Tb@tBCzPPOA nanoparticles is 30%, and a light-emitting layer with a thickness of 25 nm is obtained;
[0275] 5. Evaporating a hole blocking layer material DPEPO on the light-emitting layer to obtain a hole blocking layer with a thickness of 10 nm;
[0276] 6. Evaporating the electron transport layer material TmPyPB on the hole blocking layer to obtain an electron transport layer with a thickness of 40 nm;
[0277] 7. Vapor depositing LiF, an electron injection layer material, on the electron transport layer to obtain an electron injection layer with a thickness of 1 nm;
[0278] 8. A cathode conductive layer whose material is aluminum and whose thickness is 100 nm is evaporated on the electron injection layer to obtain an electroluminescent device.
[0279] The structure of the electroluminescent device in this embodiment is: ITO / PEDOT:PSS (40nm) / PVK (20nm) / mCP:NaGd 0.6 F4:0.4Tb@tBCzPPOA(30%)(25nm) / DPEPO(10nm) / TmPyPB(40nm) / LiF(1nm) / Al(100nm).
[0280] The current density of the electroluminescent device was tested to determine the variation trend of the current density with the voltage. The voltage-current density relationship curve is shown in FIG. Figure 4 As shown, the threshold voltage of the device is 5.0V.
[0281] The brightness of the electroluminescent device is tested to see how it changes with voltage. The voltage-brightness relationship curve is as follows: Figure 5 As shown in Figure 2, the maximum brightness of the device can reach 7.109 cd·m -2 .
[0282] The current efficiency of the electroluminescent device was tested to determine the variation trend of the current efficiency with the change of brightness. The brightness-current efficiency relationship curve is shown in FIG. Figure 6 As shown in the figure, the device has a brightness of 0.776 cd·m -2 When the current efficiency reaches the maximum value of 2.16972cd·A -1 .
[0283] The power efficiency of the electroluminescent device was tested to see how it changes with brightness. The brightness-power efficiency relationship curve is shown in Figure 7 As shown in the figure, the device has a brightness of 0.776 cd·m -2 When the power efficiency reaches the maximum value of 1.36259lm·W -1 .
[0284] The change trend of the external quantum efficiency of the electroluminescent device to the change of current density is tested, and the relationship curve between brightness and external quantum efficiency is as follows: Figure 8 As shown in the figure, the device has a brightness of 0.776 cd·m -2 When , the maximum external quantum efficiency of 1.08486% is obtained.
[0285] The electroluminescence spectrum of the electroluminescent device is shown in FIG. Fig. 9 As shown by Fig. 9 It can be seen that the electroluminescence peaks of the device are at 488nm, 544nm, 584nm, and 620nm.
[0286] Example 6
[0287] Under anhydrous and oxygen-free conditions, precursor 2 (3.7 g, about 10 mmol) was reacted in toluene (10 ml) with 9,9-dimethylacridine (2.5 g, about 12 mmol), tri(dibenzylideneacetone)dipalladium (0.36 g, about 0.4 mmol), tri-tert-butylphosphine (0.09 ml, about 0.04 mmol), and sodium tert-butoxide (1.9 g, about 20 mmol) at 90 °C for 6 h. The toluene solvent was distilled off, and the solid mixture was dissolved in dichloromethane and purified by column chromatography with dichloromethane and ethyl acetate as the eluent to obtain precursor 5.
[0288]
[0289] Precursor 5 (2.5 g, about 5 mmol) was added to a mixed solution of pyridine (25 ml) and water (10 ml), and then potassium permanganate (3.16 g, about 20 mmol) was added four times to react at 100 ° C for 5 h, and hydrochloric acid (6 mmol / mL) was added for treatment. It was purified by column chromatography with dichloromethane and methanol as the eluent to obtain compound 4 (DMACPPOA).
[0290]
[0291] Compound 4 was analyzed by hydrogen nuclear magnetic resonance spectrum, and the test data were: 1 H NMR (TMS, CDCl3, 400MHz): δ = 8.392 (s, 1H), 7.658-7.580 (m, 9H), 7.494 (s, 5H), 7.2 82(d,J=6.8Hz,2H),7.240-7.128(m,4H),7.035(d,J=7.6Hz,1H),1.486ppm(s,6H).
[0292] The electrochemical properties of compound 4 were tested, and the cyclic voltammetry curve was as follows: Figure 1 As shown. Glassy carbon was used as the working electrode, platinum wire as the comparison electrode, and Ag / AgCl as the reference electrode. By cyclic voltammetry, the HOMO energy level of compound 1 was measured to be -6.45 eV, and the LUMO energy level was -3.265 eV.
[0293] 0.0468 mol of compound 4 and 0.0468 mol of sodium hydroxide were added to 2 mL of ethanol and sonicated until the solution was clear. 0.6 F4: 0.4Tb nanoparticles mixed (ligand-free NaGd 0.6 The molar ratio of F4:0.4Tb nanoparticles to compound 4 was 1:50), ultrasonicated for 2 h, then centrifuged, the supernatant was removed, and the precipitate was washed three times with ethanol to obtain NaGd 0.6 F4:0.4Tb@DMACPPOA nanoparticles.
[0294] NaGd 0.6 F4:0.4Tb@DMACPPOA nanoparticles were tested for UV-visible light absorption spectrum, and the spectrum is shown in the figure below. Figure 2 As shown, there is an absorption peak at 303nm.
[0295] NaGd 0.6 F4: 0.4Tb@DMACPPOA nanoparticles were tested for photoluminescence spectrum, and its spectrum is shown in the figure below. Figure 3 As shown, there are emission peaks at 489nm, 544nm, 584nm, and 620nm.
[0296] NaGd 0.6 F4: a mixture of 0.4Tb@DMACPPOA nanoparticles and mCP (where NaGd 0.6 F4: 0.4Tb@DMACPPOA nanoparticles (mass fraction is 20%) are used as the light-emitting layer material to prepare an electroluminescent device, and the process is as follows:
[0297] 1. Place the glass substrate cleaned with deionized water into a vacuum evaporator with a vacuum degree of 1×10 -6 mbar, the evaporation rate is set to 0.1-0.3 nm / s, such as 0.1 nm / s, and indium tin oxide (ITO) is evaporated on the glass substrate to obtain an anode conductive layer with a thickness of 1-100 nm, such as 100 nm;
[0298] 2. Spin-coat the hole injection layer material PEDOT:PSS on the anode conductive layer. The volume ratio of PEDOT:PSS to deionized water is 1:1. Spin-coat it on the pre-cleaned ITO glass substrate at 2000 rpm and then dry it at 120°C for 15 minutes. A hole injection layer with a thickness of 40 nm is obtained.
[0299] 3. Spin-coating a hole transport layer material, polyvinyl carbazole (PVK), on the hole injection layer to obtain a hole transport layer with a thickness of 20 nm;
[0300] 4. Spin coating the light-emitting layer material on the hole transport layer: NaGd 0.6F4: a mixture of 0.4Tb@DMACPPOA nanoparticles and mCP, in which NaGd 0.6 F4: The mass fraction of 0.4Tb@DMACPPOA nanoparticles is 20%, and the thickness of the light-emitting layer is 25nm;
[0301] 5. Evaporating a hole blocking layer material DPEPO on the light-emitting layer to obtain a hole blocking layer with a thickness of 10 nm;
[0302] 6. Evaporating the electron transport layer material TmPyPB on the hole blocking layer to obtain an electron transport layer with a thickness of 40 nm;
[0303] 7. Vapor depositing LiF, an electron injection layer material, on the electron transport layer to obtain an electron injection layer with a thickness of 1 nm;
[0304] 8. A cathode conductive layer whose material is aluminum and whose thickness is 100 nm is evaporated on the electron injection layer to obtain an electroluminescent device.
[0305] The structure of the electroluminescent device in this embodiment is: ITO / PEDOT:PSS (40nm) / PVK (20nm) / mCP:NaGd 0.6 F4:0.4Tb@DMACPPOA(20%)(25nm) / DPEPO(10nm) / TmPyPB(40nm) / LiF(1nm) / Al(100nm).
[0306] The current density of the electroluminescent device was tested to determine the variation trend of the current density with the voltage. The voltage-current density relationship curve is shown in FIG. Figure 4 As shown, the threshold voltage of the device is 5.6V.
[0307] The brightness of the electroluminescent device is tested to see how it changes with voltage. The voltage-brightness relationship curve is as follows: Figure 5 As shown in Figure 2, the maximum brightness of the device can reach 8.729 cd·m -2 .
[0308] The current efficiency of the electroluminescent device was tested to determine the variation trend of the current efficiency with the change of brightness. The brightness-current efficiency relationship curve is shown in FIG. Figure 6 As shown in the figure, the device has a brightness of 1.969 cd·m -2 When the current efficiency reaches the maximum value of 1.07829cd·A -1 .
[0309] The power efficiency of the electroluminescent device was tested to see how it changes with brightness. The brightness-power efficiency relationship curve is shown in Figure 7 As shown in the figure, the device has a brightness of 1.969 cd·m -2When the power efficiency reaches the maximum value of 0.60461lm·W -1 .
[0310] The change trend of the external quantum efficiency of the electroluminescent device to the change of current density is tested, and the relationship curve between brightness and external quantum efficiency is as follows: Figure 8 As shown in the figure, the device has a brightness of 1.969 cd·m -2 When , the maximum external quantum efficiency of 0.53915% is obtained.
[0311] The electroluminescence spectrum of the electroluminescent device is shown in FIG. Fig. 9 As shown by Fig. 9 It can be seen that the electroluminescence peaks of the device are at 488nm, 544nm, 584nm, and 620nm.
[0312] Example 7
[0313] Under anhydrous and oxygen-free conditions, precursor 2 (3.7 g, about 10 mmol) was reacted in toluene (10 ml) with 9,10-dihydro-9,9-diphenylacridine (4 g, about 12 mmol), tri(dibenzylideneacetone)dipalladium (0.36 g, about 0.4 mmol), tri-tert-butylphosphine (0.09 ml, about 0.04 mmol), and sodium tert-butoxide (1.9 g, about 20 mmol) at 90 °C for 6 h. The toluene solvent was distilled off, and the solid mixture was dissolved in dichloromethane and purified by column chromatography with dichloromethane and ethyl acetate as eluents to obtain precursor 6.
[0314]
[0315] Precursor 6 (3.1 g, about 5 mmol) was added to a mixed solution of pyridine (25 ml) and water (10 ml), potassium permanganate (3.16 g, about 20 mmol) was added four times, reacted at 100 ° C for 5 h, treated with hydrochloric acid (6 mmol / mL), purified by column chromatography, eluents are dichloromethane and methanol, to obtain compound 5 (DPACPPOA).
[0316]
[0317] Compound 5 was analyzed by hydrogen nuclear magnetic resonance spectrum, and the test data were: 1H NMR (TMS, CDCl3, 400MHz): δ = 8.097 (s, 1H), 7.621-7.552 (m, 6H), 7.475 (t, J = 2Hz, 4H), 7.210 (d, J = 5.6Hz, 6H) ),7.106(t,J=7.6Hz,2H),7.028(q,J1=14Hz,J2=8Hz,1H),6.973-6.902(m,10H),6.572ppm(d,J=8.4Hz,2H).
[0318] The electrochemical properties of compound 5 were tested, and the cyclic voltammetry curve was as follows: Figure 1 As shown. Glassy carbon was used as the working electrode, platinum wire as the comparison electrode, and Ag / AgCl as the reference electrode. By cyclic voltammetry, the HOMO energy level of compound 1 was measured to be -5.932 eV, and the LUMO energy level was -3.303 eV.
[0319] 0.0468 mol of compound 5 and 0.0468 mol of sodium hydroxide were added to 2 mL of ethanol solution and ultrasonicated until the solution was clear. 0.6 F4: 0.4Tb nanoparticles mixed (NaGd 0.6 The molar ratio of F4:0.4Tb nanoparticles to compound 5 was 1:50), ultrasonicated for 2 h, then centrifuged, the supernatant was removed, and the precipitate was washed three times with ethanol to obtain NaGd 0.6 F4:0.4Tb@DPACPPOA nanoparticles.
[0320] NaGd 0.6 F4:0.4Tb@DPACPPOA nanoparticles were tested for UV-visible light absorption spectrum, and the spectrum is shown in the figure below. Figure 2 As shown, there is an absorption peak at 313nm.
[0321] NaGd 0.6 F4: 0.4Tb@DPACPPOA nanoparticles were tested for photoluminescence spectrum, and its spectrum is shown in the figure below. Figure 3 As shown, there are emission peaks at 489nm, 544nm, 585nm, and 620nm.
[0322] NaGd 0.6 F4: a mixture of 0.4Tb@DPACPPOA nanoparticles and mCP (where NaGd 0.6 F4: 0.4Tb@DPACPPOA nanoparticles (mass fraction is 10%) are used as the light-emitting layer material to prepare an electroluminescent device, and the process is as follows:
[0323] 1. Place the glass washed with deionized water into a vacuum evaporator with a vacuum degree of 1×10-6 mbar, the evaporation rate is set to 0.1-0.3 nm / s, such as 0.1 nm / s, and indium tin oxide (ITO) is evaporated on the glass substrate to obtain an anode conductive layer with a thickness of 1-100 nm, such as 100 nm;
[0324] 2. Spin-coat the hole injection layer material PEDOT:PSS on the anode conductive layer. The volume ratio of PEDOT:PSS to deionized water is 1:1. Spin-coat it on the pre-cleaned ITO glass substrate at 2000 rpm and then dry it at 120°C for 15 minutes. A hole injection layer with a thickness of 40 nm is obtained.
[0325] 3. Spin-coating a hole transport layer material, polyvinyl carbazole (PVK), on the hole injection layer to obtain a hole transport layer with a thickness of 20 nm;
[0326] 4. Spin coating the light-emitting layer material on the hole transport layer: NaGd 0.6 F4: a mixture of 0.4Tb@DPACPPOA nanoparticles and mCP, in which NaGd 0.6 F4: The mass fraction of 0.4Tb@DPACPPOA nanoparticles is 10%, and a light-emitting layer with a thickness of 25 nm is obtained;
[0327] 5. Evaporating a hole blocking layer material DPEPO on the light-emitting layer to obtain a hole blocking layer with a thickness of 10 nm;
[0328] 6. Evaporating the electron transport layer material TmPyPB on the hole blocking layer to obtain an electron transport layer with a thickness of 40 nm;
[0329] 7. Vapor depositing LiF, an electron injection layer material, on the electron transport layer to obtain an electron injection layer with a thickness of 1 nm;
[0330] 8. A cathode conductive layer whose material is aluminum and whose thickness is 100 nm is evaporated on the electron injection layer to obtain an electroluminescent device.
[0331] The structure of the electroluminescent device in this embodiment is: ITO / PEDOT:PSS (40nm) / PVK (20nm) / mCP:NaGd 0.6 F4:0.4Tb@DPACPPOA(10%)(25nm) / DPEPO(10nm) / TmPyPB(40nm) / LiF(1nm) / Al(100nm).
[0332] The current density of the electroluminescent device was tested to determine the variation trend of the current density with the voltage. The voltage-current density relationship curve is shown in FIG. Figure 4 As shown, the threshold voltage of the device is 5.9V.
[0333] The brightness of the electroluminescent device is tested to see how it changes with voltage. The voltage-brightness relationship curve is as follows: Figure 5 As shown in Figure 2, the maximum brightness of the device can reach 7.744 cd·m -2 .
[0334] The current efficiency of the electroluminescent device was tested to determine the variation trend of the current efficiency with the change of brightness. The brightness-current efficiency relationship curve is shown in FIG. Figure 6 As shown in the figure, the device has a brightness of 0.5258 cd·m -2 When the current efficiency reaches the maximum value of 0.66406cd·A -1 .
[0335] The power efficiency of the electroluminescent device was tested to see how it changes with brightness. The brightness-power efficiency relationship curve is shown in Figure 7 As shown in the figure, the device has a brightness of 0.5258 cd·m -2 When the power efficiency reaches the maximum value of 0.37912lm·W -1 .
[0336] The change trend of the external quantum efficiency of the electroluminescent device to the change of current density is tested, and the relationship curve between brightness and external quantum efficiency is as follows: Figure 8 As shown in the figure, the device has a brightness of 0.5258 cd·m -2 When , the maximum external quantum efficiency of 0.33203% is obtained.
[0337] The electroluminescence spectrum of the electroluminescent device is shown in FIG. Fig. 9 As shown by Fig. 9 It can be seen that the electroluminescence peaks of the device are at 488nm, 544nm, 584nm, and 620nm.
[0338] The present invention is described in detail above in conjunction with specific embodiments and / or exemplary examples and drawings, but these descriptions cannot be understood as limiting the present invention. Those skilled in the art understand that, without departing from the spirit and scope of the present invention, various equivalent substitutions, modifications or improvements may be made to the technical solutions and implementations of the present invention, all of which fall within the scope of the present invention. The scope of protection of the present invention shall be subject to the attached claims.
Claims
1. A terbium-gadolinium nanocrystal, comprising a terbium-gadolinium nanocrystal coordinated with an unsaturated fatty acid and a ligand-free terbium-gadolinium nanocrystal, After terbium salt, gadolinium salt and unsaturated fatty acid react in a solvent, alkali metal hydroxide and fluoride are added to react to prepare terbium gadolinium nanocrystal coordinated with unsaturated fatty acid, wherein the unsaturated fatty acid is selected from 10 One or more of the above unsaturated fatty acids, The unsaturated fatty acid ligand is removed from the terbium-gadolinium nanocrystal coordinated with the unsaturated fatty acid to obtain the ligand-free terbium-gadolinium nanocrystal.
2. A diphenylphosphinobenzoic acid compound, characterized in that: It is expressed by formula (1): Wherein, R0 is selected from hydrogen or a nitrogen-containing group, preferably hydrogen, carbazole, tert-butylcarbazole, dimethylacridinyl or diphenylacridinyl.
3. The diphenylphosphinobenzoic acid compound according to claim 2, wherein the diphenylphosphinobenzoic acid compound is one of the following compounds: More preferably, the diphenylphosphinobenzoic acid compound is one of Compound 1 to Compound 4.
4. A method for preparing a diphenylphosphinobenzoic acid compound, characterized in that: The method specifically comprises the following steps: Step 1. reacting halogenated toluene with magnesium to obtain a Grignard reagent, then adding diphenylphosphine halide to react, and after oxidation, post-treatment to obtain a diphenylphosphinoyltoluene compound. The halogenated toluene is: wherein X1 and X2 are each independently selected from hydrogen, a bromine substituent, an iodine substituent or a chlorine substituent, preferably selected from hydrogen, a bromine substituent or an iodine substituent, The diphenylphosphinoyl toluene compound is: wherein R1 is hydrogen, a bromine substituent or a chlorine substituent; Optionally, step 2 is performed: adding a diphenylphosphinooxytoluene compound and a nitrogen-containing compound to solvent I, catalyzing a reaction in the presence of a catalyst, and post-treating to obtain a nitrogen heterocyclic substituted diphenylphosphinooxytoluene compound. In step 2, the diphenylphosphinoyltoluene compound is: Wherein, R1 is a bromine substituent or a chlorine substituent, The nitrogen-containing compound is one or more selected from carbazole compounds and acridine compounds, preferably one or more selected from carbazole, 3,6-di-tert-butylcarbazole, 9,9-dimethylacridine and 9,10-dihydro-9,9-diphenylacridine, more preferably one or more selected from carbazole, 3,6-di-tert-butylcarbazole and 9,9-dimethylacridine; Step 3. Add a diphenylphosphinooxytoluene compound or a nitrogen heterocyclic substituted diphenylphosphinooxytoluene compound to solvent II, add potassium permanganate, heat to react, and post-treat to obtain a diphenylphosphinooxybenzoic acid compound.
5. The method for preparing diphenylphosphinobenzoic acid compounds according to claim 4, characterized in that: In step 1, The molar ratio of the halogenated toluene to magnesium is 10:(7-18), preferably 10:(9-15), more preferably 10:(11-13), The molar ratio of the diphenylphosphine halide to the halogenated toluene is 10:(7-18), preferably 10:(9-15), and more preferably 10:(11-13).
6. The method for preparing diphenylphosphinobenzoic acid compounds according to claim 4, characterized in that: In step 2, The molar ratio of the nitrogen-containing compound to the diphenylphosphinoyltoluene compound is (10-48):10, preferably (11-40):10, and more preferably (12-32):
10. The catalyst is a copper catalyst or a palladium catalyst.
7. A terbium-gadolinium nanocrystalline compound coated with a diphenylphosphinobenzoic acid compound ligand, characterized in that: The method is obtained by reacting terbium-gadolinium nanocrystals without ligand wrapping with the diphenylphosphinobenzoic acid compound according to claim 3.
8. A method for preparing a terbium-gadolinium nanocrystalline compound coated with a diphenylphosphinobenzoic acid compound ligand, characterized in that: The method specifically comprises the following steps: Step a. adding the dispersion of the terbium-gadolinium nanocrystals coordinated with unsaturated fatty acids to a nitrosoboric acid tetrafluoroborate (NOBF4) solution, ultrasonically treating it, then adding solvent a, ultrasonically treating it again, centrifuging it, washing it, and obtaining terbium-gadolinium nanocrystals without ligand coating; Step b. adding the terbium-gadolinium nanocrystals without ligand coating to a diphenylphosphinobenzoic acid compound solution, subjecting to ultrasonic treatment, and repeating centrifugation, washing, and centrifugation to obtain the terbium-gadolinium nanocrystals compound coated with the diphenylphosphinobenzoic acid compound ligand.
9. The method for preparing the terbium-gadolinium nanocrystalline compound coated with a diphenylphosphinobenzoic acid compound ligand according to claim 8, characterized in that: The diphenylphosphinobenzoic acid compound solution is further added with an alkaline substance selected from one or more hydroxides, and the solvent is selected from one or more alcohol solvents, ether solvents and ester solvents, preferably one or more alcohol solvents with a carbon number of C1-C5. The molar ratio of the terbium gadolinium nanocrystals without ligand coating to the diphenylphosphinobenzoic acid compound is 1:(30-70), preferably 1:(40-60), and more preferably 1:
50.
10. An electroluminescent device, characterized in that: It comprises a light-emitting layer, wherein the raw materials for preparing the light-emitting layer comprise one or more of the terbium gadolinium nanocrystals according to claim 1, the ligand-free terbium gadolinium nanocrystals and the terbium gadolinium nanocrystals wrapped with diphenylphosphinobenzoic acid compound ligands according to claim 2, preferably comprise one or more of the terbium gadolinium nanocrystals wrapped with diphenylphosphinobenzoic acid compound ligands according to claim 2, and more preferably comprise one or more of the terbium gadolinium nanocrystals wrapped with compounds 1 to 4. The electroluminescent device further comprises an anode conductive layer, a hole injection layer, a hole transport layer, a hole blocking layer, an electron transport layer, an electron injection layer and a cathode conductive layer. The hole injection layer material is poly(3,4-ethylenedioxythiophene):poly(styrene sulfonic acid), The hole transport layer material is selected from polyvinyl carbazole, The raw materials for preparing the light-emitting layer also include a host material, and the host material is selected from one or more of 9,9'-(1,3-phenyl)di-9H-carbazole (mCP), bis-4(N-carbazolylphenyl)phenylphosphine oxide (BCPO), 4,4-bis(9-carbazole)biphenyl (CBP), 4,4'-bis(9H-carbazole-9-yl)-2,2'-dimethylbiphenyl (CDBP), (4-(9H-carbazole-9-yl)-2-methylphenyl)diphenylphosphine oxide (CPPOM), 9-(4-tert-butylphenyl)-3,6-bis(triphenylsilyl)-9h-carbazole (CzSi), bis[2-((oxy)diphenylphosphino)phenyl]ether (DPEPO) and polyvinylcarbazole (PVK). The hole blocking layer material is bis[2-((oxy)diphenylphosphino)phenyl]ether, The electron transport layer material is 3,3'-[5'-[3-(3-pyridyl)phenyl][1,1':3',1"-terphenyl]-3,3"-diyl]bipyridine, The electron injection layer material is LiF.