Up-conversion luminescent material as well as preparation method and application thereof

Preparing nanoscale upconversion luminescent materials through a hydrothermal reaction method solves the problems of reduced high-temperature luminous efficiency and large particle size in the existing technology, achieves high purity and reverse thermal quenching performance of the material, and expands its application scope.

CN118725863AActive Publication Date: 2024-10-01CHINA UNIV OF PETROLEUM (BEIJING)
View PDF 3 Cites 0 Cited by

Patent Information

Application Number
CN202410760214.2
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Filing Date
2024-06-13
Publication Date
2024-10-01
Estimated Expiration
2044-06-13

AI Technical Summary

Technical Problem

The luminous efficiency of existing upconversion luminescent materials decreases under high temperature conditions, and the particle size is large and unevenly distributed, which limits their promotion in industrial production and high-temperature applications.

Method used

Up-conversion luminescent materials are prepared using a hydrothermal reaction method. The ytterbium salt, ammonium molybdate tetrahydrate and rare earth metal salt solutions are stirred, hydrothermal reacted, dried and calcined. The reaction temperature is controlled at 130-180°C and the time is 1.5- In 2.5 hours, the upconversion luminescent material of nanoscale particles was obtained.

Benefits of technology

It achieves uniform distribution of nanoscale particles, high degree of crystallization and reverse thermal quenching performance of up-conversion luminescent materials, reduces energy consumption and costs, and expands its application scope in fields such as biomedicine, information encryption and solar cells.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN118725863A_ABST
    Figure CN118725863A_ABST
Patent Text Reader

Abstract

The invention relates to the field of nanometer material synthesis, and discloses an up-conversion luminescent material and a preparation method and application thereof.The preparation method of the up-conversion luminescent material comprises the steps that 1, a ytterbium salt solution, an ammonium molybdate tetrahydrate solution and a rare earth metal salt solution are stirred for the first time, and an intermediate I is obtained; the rare earth metal salt in the rare earth metal salt solution is selected from at least one of erbium salt, holmium salt, praseodymium salt and europium salt; (2) carrying out hydrothermal reaction on the intermediate I in a hydrothermal reaction kettle to obtain an intermediate II; and (3) sequentially drying and calcining the intermediate II to obtain the up-conversion luminescent material. The average particle size of the up-conversion luminescent material prepared by the method provided by the invention is nanoscale, and the up-conversion luminescent material is good in crystallization degree and reverse heat quenching performance.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The present invention relates to the field of nano material synthesis, and in particular to up-conversion luminescent materials and preparation methods and applications thereof. Background Art

[0002] Upconversion luminescent materials are anti-Stokes luminescent materials, which absorb two or more long-wave low-energy photons and emit short-wave high-energy photons. They can absorb near-infrared light and emit visible light. Compared with traditional luminescent materials, upconversion luminescent materials have the advantages of long fluorescence lifetime, rich emission energy levels, and narrow emission spectrum lines. They are widely used in temperature sensors, biomedical probes, information encryption and anti-counterfeiting, solar cells, 3D imaging and other fields.

[0003] The up-conversion luminescent material is composed of a base material, a sensitizer and an activator. The base material can be fluoride, oxide, bromide, etc., and the sensitizer and activator are mostly rare earth ions.

[0004] At present, the preparation of upconversion luminescent materials mostly requires reactions under high temperature conditions, high energy consumption, and large particle size. In addition, the luminescence efficiency of upconversion luminescent materials is low, and there are problems such as thermal quenching and concentration quenching, which largely limit their practical application and make it difficult to promote industrial production.

[0005] CN105778911A discloses a rare earth doped photoluminescent material with YbMoO4 as the matrix, which is a rare earth Er doped YbMoO4 photoluminescent material obtained by reacting erbium nitrate, ytterbium nitrate and ammonium heptamolybdate. The preparation method of the above-mentioned luminescent material is mainly to dissolve erbium nitrate and ytterbium nitrate in ethanol to obtain solution A according to the molar ratio of erbium nitrate: ytterbium nitrate: ammonium heptamolybdate of 0-7:0-7:1, dissolve ammonium heptamolybdate in deionized water to obtain solution B, adjust the pH value of solution B to 7.0 with 1M NaOH solution, then slowly pour it into solution A and stir for 1 hour, dry it at 100°C for 12 hours, put it into a muffle furnace and heat it to 500-800°C at a rate of 8°C / min, and cool it with the furnace after 2 hours to obtain a rare earth doped photoluminescent material with YbMoO4 as the matrix. The method of the present invention is simple, easy to operate, and low in cost. The prepared rare earth doped photoluminescent material has high luminescence efficiency and excellent optical temperature sensing characteristics. However, the method requires high energy consumption, long reaction time, and incomplete reaction. The prepared particle size is large and unevenly distributed. As the temperature increases, the luminescence efficiency continues to decrease, which greatly limits the application of up-conversion luminescent materials in high temperature areas.

[0006] Therefore, it is of great significance to develop a new upconversion luminescent material. Summary of the invention

[0007] The purpose of the present invention is to provide an up-conversion luminescent material with nanometer average particle size, good crystallinity and reverse thermal quenching performance.

[0008] In order to achieve the above object, the first aspect of the present invention provides a method for preparing an upconversion luminescent material, the method comprising:

[0009] (1) performing a first stirring on an ytterbium salt solution, an ammonium molybdate tetrahydrate solution and a rare earth metal salt solution to obtain an intermediate I; the rare earth metal salt in the rare earth metal salt solution is selected from at least one of an erbium salt, a holmium salt, a praseodymium salt and a europium salt;

[0010] (2) subjecting the intermediate I to a hydrothermal reaction in a hydrothermal reactor to obtain an intermediate II; the conditions of the hydrothermal reaction include: a temperature of 130-180° C. and a time of 1.5-2.5 h;

[0011] (3) subjecting the intermediate II to drying and calcining treatments in sequence to obtain the up-conversion luminescent material;

[0012] In step (1), in the mixed solution at the start of the first stirring, Yb 3+ The concentration of is 0.2-0.32 mol / L, the concentration of ammonium molybdate tetrahydrate is 0.15-0.22 mol / L, and the concentration of rare earth metal ions is 0.004-0.02 mol / L.

[0013] The second aspect of the present invention provides an up-conversion luminescent material prepared by the method described in the first aspect.

[0014] The third aspect of the present invention provides the use of the up-conversion luminescent material described in the second aspect in biomedical diagnosis, information encryption storage or solar cells.

[0015] The technical solution provided by the present invention has at least the following advantages compared with the prior art:

[0016] (1) The up-conversion luminescent material provided by the present invention has good crystallinity, high purity, easy to control morphology and reverse thermal quenching performance.

[0017] (2) The present invention adopts a hydrothermal reaction method to prepare up-conversion luminescent materials, which has a simple preparation process, low reaction temperature, short reaction time, low energy consumption, sufficient reaction, low material synthesis cost, and no need to use organic solvents, which is more environmentally friendly.

[0018] (3) The upconversion luminescent material particles provided by the present invention have an average particle size of nanometers, a small particle size, and a uniform size distribution of the nanomaterials, and can be used in the field of nanomaterials, thus expanding the application scope of upconversion luminescent materials. BRIEF DESCRIPTION OF THE DRAWINGS

[0019] Figure 1 is a scanning electron microscope image of the up-conversion luminescent material S1;

[0020] Figure 2 It is the X-ray diffraction spectra of up-conversion luminescent materials S1, S2, S3, S4, DS1, DS2 and DS3, the left part represents the X-ray diffraction spectra of S1, S2, S3, S4, and the right part represents the X-ray diffraction spectra of DS1, DS2 and DS3;

[0021] Figure 3 It is the up-conversion luminescence spectrum of up-conversion luminescent material S1 at different temperatures under 980nm laser excitation;

[0022] Figure 4 It is the up-conversion luminescence spectrum of the up-conversion luminescent material S2 at different temperatures under 980nm laser excitation;

[0023] Figure 5 It is the up-conversion luminescence spectrum of up-conversion luminescent material S3 at different temperatures under 980nm laser excitation;

[0024] Figure 6 It is the up-conversion luminescence spectrum of up-conversion luminescent material S4 at different temperatures under 980nm laser excitation;

[0025] Figure 7 This is the up-conversion luminescence spectrum of the up-conversion luminescent material DS1 under 980nm laser excitation;

[0026] Figure 8 This is the up-conversion luminescence spectrum of the up-conversion luminescent material DS2 under 980nm laser excitation;

[0027] Fig. 9 This is the upconversion luminescence spectrum of the upconversion luminescent material DS3 at different temperatures under 980nm laser excitation. DETAILED DESCRIPTION

[0028] The endpoints and any values ​​of the ranges disclosed in this article are not limited to the precise ranges or values, and these ranges or values ​​should be understood to include values ​​close to these ranges or values. For numerical ranges, the endpoint values ​​of each range, the endpoint values ​​of each range and the individual point values, and the individual point values ​​can be combined with each other to obtain one or more new numerical ranges, which should be considered as specifically disclosed in this article.

[0029] As mentioned above, the first aspect of the present invention provides a method for preparing an upconversion luminescent material, the method comprising:

[0030] (1) performing a first stirring on an ytterbium salt solution, an ammonium molybdate tetrahydrate solution and a rare earth metal salt solution to obtain an intermediate I; the rare earth metal salt in the rare earth metal salt solution is selected from at least one of an erbium salt, a holmium salt, a praseodymium salt and a europium salt;

[0031] (2) subjecting the intermediate I to a hydrothermal reaction in a hydrothermal reactor to obtain an intermediate II; the conditions of the hydrothermal reaction include: a temperature of 130-180° C. and a time of 1.5-2.5 h;

[0032] (3) subjecting the intermediate II to drying and calcining treatments in sequence to obtain the up-conversion luminescent material;

[0033] In step (1), in the mixed solution at the start of the first stirring, Yb 3+ The concentration of is 0.2-0.32 mol / L, the concentration of ammonium molybdate tetrahydrate is 0.15-0.22 mol / L, and the concentration of rare earth metal ions is 0.004-0.02 mol / L.

[0034] It should be noted that in the present invention, there is no special requirement for the ytterbium salt and the rare earth metal salt, as long as the Yb 3+ and the rare earth metal ion. Exemplarily, the ytterbium salt is ytterbium nitrate, and the rare earth metal salt is selected from at least one of erbium nitrate, holmium nitrate, praseodymium nitrate and europium nitrate.

[0035] Preferably, in step (1), the Yb in the ytterbium salt solution is 3+ The molar ratio of the amount of ammonium molybdate tetrahydrate in the ammonium molybdate tetrahydrate solution calculated on a dry basis is 1:0.7-0.9 mol.

[0036] Preferably, in step (1), Yb in the ytterbium salt solution is 3+ The total molar amount of rare earth metal ions in the rare earth metal salt solution is taken as the reference, and the Yb in the ytterbium salt solution is 3+ The dosage of is 92-98 mol %, and the dosage of the rare earth metal ions in the rare earth metal salt solution is 2-8 mol %. The inventors of the present invention have found that in this preferred case, the up-conversion luminescent material provided by the present invention has better reverse thermal quenching performance.

[0037] Preferably, in step (2), the conditions of the hydrothermal reaction include: a temperature of 130-150° C. The inventors of the present invention have found that in this preferred case, the up-conversion luminescent material provided by the present invention has a better degree of crystallinity.

[0038] Preferably, in step (1), the Yb in the ytterbium salt solution is 3+ The concentration is 0.5-0.7mol / L.

[0039] Preferably, in step (1), the concentration of the ammonium molybdate tetrahydrate solution is 0.25-0.35 mol / L.

[0040] Preferably, in step (1), the concentration of rare earth metal ions in the rare earth metal salt solution is 0.5-3.5 mol / L. The inventors of the present invention have found that in this preferred case, the up-conversion luminescent material provided by the present invention has better reverse thermal quenching performance.

[0041] Preferably, in step (1), the first stirring conditions include: temperature of 10-30°C and time of 1.5-2.5h. The inventors of the present invention have found that in this preferred case, the particle size of the upconversion luminescent material provided by the present invention is smaller and the reverse thermal quenching performance is better.

[0042] It should be noted that in step (2), the method further includes, before the drying treatment, washing the intermediate II at least once, centrifuging and the like, and then drying the obtained precipitate. The present invention has no special requirements for the washing and the centrifuging, and any method known in the art can be used. Exemplarily, the present invention uses deionized water for washing and a centrifuge for centrifugation, and the centrifugation conditions at least include: a centrifuge speed of 6000-7000rpm and a centrifugation time of 6-10min.

[0043] Preferably, in step (3), the drying conditions include: temperature of 70-90° C. and time of 3-5 h.

[0044] Preferably, in step (3), the calcination treatment conditions include: temperature of 810-900° C. and time of 1.5-2.5 h.

[0045] More preferably, in step (3), the calcination treatment conditions include: a temperature of 810-850° C. The inventors of the present invention have found that in this preferred case, the particle size of the up-conversion luminescent material provided by the present invention is smaller and the degree of crystallinity is higher.

[0046] As mentioned above, the second aspect of the present invention provides an up-conversion luminescent material prepared by the method described in the first aspect.

[0047] Preferably, the average particle size of the up-conversion luminescent material particles is 40 nm-210 nm.

[0048] As mentioned above, the third aspect of the present invention provides the use of the up-conversion luminescent material described in the second aspect in biomedical diagnosis, information encryption storage or solar cells.

[0049] The present invention will be described in detail below by way of examples. In the following examples, unless otherwise specified, the instruments, reagents, materials, etc. involved are all conventional instruments, reagents, materials, etc., which can be obtained through regular commercial channels. Among them, unless otherwise specified, the reagents used are all commercially available analytically pure products.

[0050] Ytterbium salt: Ytterbium (III) nitrate pentahydrate, purchased from Adamas Beta (Shanghai) Chemical Reagent Co., Ltd., analytical grade;

[0051] Ammonium molybdate tetrahydrate: purchased from Adamas Beta (Shanghai) Chemical Reagent Co., Ltd., analytical grade;

[0052] Rare earth metal salts: Erbium nitrate, purchased from Adamas Beta (Shanghai) Chemical Reagent Co., Ltd., analytical grade;

[0053] Hydrothermal reactor: 50 mL, model CYKH-50ML, purchased from Xi'an Changyi Instrument Equipment Company.

[0054] Example 1

[0055] (1) stirring an ytterbium salt solution, an ammonium molybdate tetrahydrate solution and a rare earth metal salt solution to obtain an intermediate I;

[0056] (2) subjecting the intermediate I to a hydrothermal reaction in a hydrothermal reactor to obtain an intermediate II;

[0057] (3) The intermediate II was washed with deionized water and then centrifuged (the centrifuge speed was 6750 rpm and the centrifugation time was 7 min). The above operation was repeated 3 times, and the obtained precipitate was dried and calcined in turn to obtain the upconversion luminescent material S1.

[0058] The specific raw material dosage and concentration and process parameters of Example 1 are shown in Table 1. Unless otherwise specified, the remaining examples are carried out using the same process as Example 1, except that the raw material concentrations and dosages and process parameters used are different, see Table 1 for details.

[0059] Table 1

[0060] Example 1 Example 2 Step (1) <![CDATA[The concentration of Yb in ytterbium salt solution (mol / L)]]> 3+ > 0.6 0.5 Amount of ytterbium salt solution / mL 7.84 8.1 Concentration of ammonium molybdate tetrahydrate solution (mol / L) 0.3 0.32 Dosage of ammonium molybdate tetrahydrate solution / mL 12 10 Concentration of rare earth ions in rare earth metal salt solution (mol / L) 0.6 0.7 Amount of rare earth metal salt solution / mL 0.16 0.4 First stirring Temperature / ℃ 25 30 Time / h 2 1.5 Step (2) Hydrothermal reaction Temperature / ℃ 140 130 Time / h 2 2.5 Step (3) Drying Temperature / ℃ 85 75 Time / h 3.5 4 Calcination treatment Temperature / ℃ 830 820 Time / h 1.5 2 name S1 S2

[0061] Example 3

[0062] This example is carried out in a similar manner to that of Example 1, except that in this example, the concentration of the ammonium molybdate tetrahydrate solution is adjusted to 0.35 mol / L, and the volume used remains unchanged, to obtain the up-conversion luminescent material S3.

[0063] Example 4

[0064] This embodiment is carried out using a method similar to that of Embodiment 1, except that the temperature of the hydrothermal reaction in step (2) of this embodiment is adjusted to 170° C. to obtain the up-conversion luminescent material S4.

[0065] Comparative Example 1

[0066] Step (1) is the same as in Example 1;

[0067] Step (2): react the intermediate I in a beaker in a water bath at 80°C for 2 h to obtain the intermediate II;

[0068] Step (3) is the same as in Example 1 to obtain the up-conversion luminescent material DS1.

[0069] Comparative Example 2

[0070] This comparative example is carried out in a similar manner to Example 1, except that the concentration of rare earth ions in the rare earth metal salt solution in this comparative example is adjusted to 3.2 mol / L, and the volume dosage remains unchanged, to obtain the up-conversion luminescent material DS2.

[0071] Comparative Example 3

[0072] This comparative example was carried out in a similar manner to Example 1, except that in this comparative example, Yb 3+ The concentration was adjusted to 4 mol / L, and the volume remained unchanged to obtain the upconversion luminescent material DS3.

[0073] Test Case

[0074] The present invention exemplarily selects the up-conversion luminescent material S1 obtained in the above example and uses a scanning electron microscope to test its morphology. The results are shown in FIG. Figure 1 .

[0075] The up-conversion luminescent materials S1, S2, S3, S4, DS1, DS2 and DS3 obtained in the above examples were analyzed by X-ray diffraction for phase composition. Figure 2 . Figure 2 The left part is the X-ray diffraction spectrum of S1, S2, S3, and S4, and the right part is the X-ray diffraction spectrum of DS1, DS2, and DS3.

[0076] The up-conversion luminescent material obtained in the above example was optically tested using a fluorescence spectrophotometer under the following test conditions: at a temperature of 37°C to 397°C and excited by a 980nm laser. The temperature-dependent up-conversion luminescent spectrum of the up-conversion luminescent material provided by the present invention under 980nm excitation is shown in Figure 3 , Figure 4 , Figure 5 , Figure 6 , Figure 7 , Figure 8 and Fig. 9 .

[0077] from Figure 1 It can be seen that the average particle size of the up-conversion luminescent material prepared by the method provided by the present invention is 117 nm, and the shape is blocky.

[0078] from Figure 2 It can be seen that the up-conversion luminescent materials S1, S2, S3 and S4 provided by the present invention have a high degree of crystallinity and no impurities are present. By comparing the up-conversion luminescent materials with the standard cards, it can be seen that the up-conversion luminescent materials S1, S2, S3, S4 and DS2 have a high degree of crystallinity, the DS3 material has a low degree of crystallinity, and DS1 has no diffraction peak.

[0079] from Figure 3 It can be seen that the upconversion luminescent material S2 has green light emission peaks at wavelengths of 524nm and 559nm, mainly due to the erbium ions in the luminescent center. 2 H 11 / 2 → 4 I 15 / 2 and 4 S 3 / 2 → 4 I 15 / 2 It can also be seen from the figure that the temperature rising from 37℃ to 377℃ does not affect the luminescence intensity of the conversion luminescent material S2. It has the highest emission intensity at 377℃, and its luminescence intensity increases with the increase of temperature, indicating that the material has great application potential in high temperature areas.

[0080] from Figure 4 It can be seen that the up-conversion luminescent material S2 has a green light emission peak at a wavelength of 450nm to 700nm, which is mainly due to the erbium ion in the luminescent center. 2 H 11 / 2 → 4 I 15 / 2 , 4 S 3 / 2 → 4 I 15 / 2 and 4 F 9 / 2 → 4 I 15 / 2 It can also be seen from the figure that the temperature increasing from 37°C to 377°C does not affect the luminescence intensity of the conversion luminescent material S2. It has the highest emission intensity at 377°C, and its luminescence intensity continues to increase with the increase of temperature, indicating that the material has great application potential in high temperature areas.

[0081] from Figure 5 It can be seen that the up-conversion luminescent material S3 has a green light emission peak at a wavelength of 450nm to 700nm, which is mainly due to the erbium ion in the luminescent center.2 H 11 / 2 → 4 I 15 / 2 , 4 S 3 / 2 → 4 I 15 / 2 and 4 F 9 / 2 → 4 I 15 / 2 It can also be seen from the figure that the temperature rising from 37℃ to 377℃ does not affect the luminescence intensity of the conversion luminescent material S3. It has the highest emission intensity at 377℃, and its luminescence intensity increases with the increase of temperature, indicating that the material has great application potential in high temperature areas.

[0082] from Figure 6 It can be seen that the upconversion luminescent material S4 has green light emission peaks at wavelengths of 524nm and 559nm, mainly due to the erbium ions in the luminescent center. 2 H 11 / 2 → 4 I 15 / 2 and 4 S 3 / 2 → 4 I 15 / 2 It can also be seen from the figure that the highest emission intensity is at 277℃, indicating that the material has great application potential in high temperature areas.

[0083] from Figure 7 It can be seen that the emission peak of the up-conversion luminescent material DS1 is not detected, indicating that the up-conversion luminescent material prepared without adopting the method provided by the present invention does not have luminescent performance.

[0084] from Figure 8 It can be seen that the emission peak of the up-conversion luminescent material DS2 is not detected, indicating that the up-conversion luminescent material prepared without adopting the method provided by the present invention does not have luminescent properties.

[0085] from Fig. 9 It can be seen that the upconversion luminescent material DS3 has a green light emission peak at 450nm~700nm, which is mainly due to the erbium ion in the luminescent center. 2 H 11 / 2 → 4 I 15 / 2 and 4 S 3 / 2 → 4 I 15 / 2 It can also be seen from the figure that when the temperature rises from 37°C to 377°C, the highest emission intensity is at 37°C, and the luminescence intensity of the up-conversion luminescent material DS3 decreases with the increase of temperature.

[0086] The preferred embodiments of the present invention are described in detail above, but the present invention is not limited thereto. Within the technical concept of the present invention, the technical solution of the present invention can be subjected to a variety of simple modifications, including the combination of various technical features in any other suitable manner, and these simple modifications and combinations should also be regarded as the contents disclosed by the present invention and belong to the protection scope of the present invention.

Claims

1. A method for preparing an upconversion luminescent material, characterized in that: The method includes: (1) performing a first stirring on an ytterbium salt solution, an ammonium molybdate tetrahydrate solution and a rare earth metal salt solution to obtain an intermediate I; the rare earth metal salt in the rare earth metal salt solution is selected from at least one of an erbium salt, a holmium salt, a praseodymium salt and a europium salt; (2) subjecting the intermediate I to a hydrothermal reaction in a hydrothermal reactor to obtain an intermediate II; the conditions of the hydrothermal reaction include: a temperature of 130-180° C. and a time of 1.5-2.5 h; (3) subjecting the intermediate II to drying and calcining treatments in sequence to obtain the up-conversion luminescent material; In step (1), in the mixed solution at the start of the first stirring, Yb 3+ The concentration of is 0.2-0.32 mol / L, the concentration of ammonium molybdate tetrahydrate is 0.15-0.22 mol / L, and the concentration of rare earth metal ions is 0.004-0.02 mol / L.

2. The method according to claim 1, wherein: In step (1), the Yb in the ytterbium salt solution 3+ The molar ratio of the amount of ammonium molybdate tetrahydrate in the ammonium molybdate tetrahydrate solution calculated on a dry basis is 1:0.7-0.9 mol; And / or, in step (1), Yb in the ytterbium salt solution 3+ The total molar amount of rare earth metal ions in the rare earth metal salt solution is taken as the reference, and the Yb in the ytterbium salt solution is 3+ The amount of rare earth metal ions in the rare earth metal salt solution is 2-8 mol%; And / or, in step (2), the conditions of the hydrothermal reaction include: a temperature of 130-150°C.

3. The method according to claim 1 or 2, wherein: In step (1), the Yb in the ytterbium salt solution 3+ The concentration is 0.5-0.7mol / L.

4. The method according to claim 1 or 2, wherein: In step (1), the concentration of the ammonium molybdate tetrahydrate solution is 0.25-0.35 mol / L.

5. The method according to claim 1 or 2, wherein: In step (1), the concentration of rare earth metal ions in the rare earth metal salt solution is 0.5-3.5 mol / L.

6. The method according to claim 1 or 2, wherein: In step (1), the first stirring conditions include: temperature of 10-30° C. and time of 1.5-2.5 h.

7. The method according to claim 1 or 2, wherein: In step (3), the drying conditions include: temperature of 70-90°C and time of 3-5h; And / or, in step (3), the calcination treatment conditions include: temperature of 810-900° C. and time of 1.5-2.5 h.

8. An up-conversion luminescent material prepared by the method according to any one of claims 1 to 7.

9. The up-conversion luminescent material according to claim 8, wherein: The average particle size of the up-conversion luminescent material particles is 40nm-210nm.

10. Use of the up-conversion luminescent material according to claim 8 or 9 in biomedical diagnosis, information encryption storage or solar cells.

Citation Information

Patent Citations

  • Efficient and green up-conversion light-emitting compound film and preparation method thereof

    CN105295912A

  • Rare-earth doped photoluminescence material by using YbMoO4 as substrate and preparation method thereof

    CN105778911A

  • Efficient up-conversion luminescent nanometer material based on ytterbium molybdate substrate as well as preparation method and application thereof

    CN106010527A