Environment-friendly soil stabilizer and preparation method thereof

By using environmentally friendly soil solidifiers such as gelatin, sodium alginate and cellulose, and using physical adsorption and mechanical fixation for soil solidification, the problem of pollution risks of existing soil solidifiers has been solved, and efficient and environmentally friendly soil solidification has been achieved. effectiveness and low-cost production.

CN118725870APending Publication Date: 2024-10-01CHINA MCC5 GROUP CORP LTD
View PDF 0 Cites 1 Cited by

Patent Information

Application Number
CN202410651649.3
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Filing Date
2024-05-24
Publication Date
2024-10-01

AI Technical Summary

Technical Problem

Existing soil solidifiers contain chemical substances, which lead to higher risks of soil pollution and poor environmental protection.

Method used

This environmentally friendly soil solidifier uses gelatin, sodium alginate and cellulose as the main raw materials. It solidifies the soil through physical adsorption and mechanical fixation. The preparation method is simple, the cost is low, the raw materials are safe and can be naturally decomposed.

Benefits of technology

It achieves good soil solidification effect and is environmentally friendly and safe, reduces production and use costs, avoids soil pollution, and is suitable for re-cultivation needs in temporary access roads and other scenarios.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure BDA0004856542820000051
    Figure BDA0004856542820000051
  • Figure BDA0004856542820000061
    Figure BDA0004856542820000061
  • Figure BDA0004856542820000071
    Figure BDA0004856542820000071
Patent Text Reader

Abstract

The invention provides an environment-friendly soil stabilizer and a preparation method thereof, and relates to the technical field of soil engineering materials. The environment-friendly soil stabilizer is prepared from the following raw materials in percentage by weight: 80-95% of gelatin, 4-19% of sodium alginate and 1-5% of cellulose. The preparation method comprises the following steps: mixing the gelatin, the sodium alginate and the cellulose in proportion, then adding water, and uniformly stirring to obtain the soil stabilizer. The raw materials of the soil stabilizer only comprise gelatin, sodium alginate and cellulose, the raw materials are common and low in cost, the preparation method is simple, large machines and strict environments are not needed, the manufacturing cost is low, the curing effect is good, and compared with a traditional soil stabilizer, the cost of the whole production and use link is reduced. In addition, the raw material components are safe and free of pollution components such as heavy metal, and the curing principle is based on physical adsorption and mechanical fixed connection of soil and the curing agent, so that the whole curing process has small influence on the environment, and remarkable environmental protection safety is achieved.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The present application belongs to the technical field of soil engineering materials, and specifically relates to an environmentally friendly soil solidifier and a preparation method thereof. Background Art

[0002] Soil stabilizer is a hydraulic cementing material composed of a variety of inorganic and organic materials, mainly used to improve the physical properties and engineering performance of soil. It can fill the pores between soil particles and transform loose soil into dense cementitious materials, thereby greatly improving the strength and durability of soil. Soil stabilizer is widely used in rural access roads and temporary site hardening. It has the advantages of fast forming, rapid reclamation and less soil abandonment.

[0003] The main types and action mechanisms of commonly used soil stabilizers are as follows:

[0004] (1) Inorganic curing agent: After the inorganic curing agent is mixed with water or aqueous solution, a hydration reaction occurs to generate gel products such as hydrated calcium silicate, hydrated calcium sulfate, and hydrated calcium aluminate. This product part continues to harden to form a skeleton structure, thereby improving the strength of the soil.

[0005] (2) Organic curing agents: Electrostatic effect is a major mechanism for the stabilization of soils cured by organic curing agents, especially cationic organic curing agents for stabilizing clay. This is because the surface of clay minerals is usually negatively charged. Polycations are easily adsorbed on the surface and edges of clay minerals, changing the water absorption near the surface of clay minerals and forming large and stable flocculent particles.

[0006] (3) Ionic solidifier: Ionic solidifiers mainly strengthen soil through strong ion exchange and surfactant hydrophobicity. After the solidifier solution is mixed with the soil, it can quickly ionize, release a large number of anions and cations, and exchange ions with cations near the surface of soil particles, thereby reducing the thickness of the double layer and causing the thickness of the bound water film on the surface of soil particles to become thinner.

[0007] However, the above traditional soil stabilizers contain a lot of chemical substances, which will continue to remain in the soil, causing the content of pollutants such as heavy metals in the soil to exceed the standard, causing soil pollution and poor environmental protection. Summary of the invention

[0008] In view of the poor environmental protection of existing soil solidifiers and the potential pollution risks they may bring to the soil, the present invention provides an environmentally friendly soil solidifier and a preparation method thereof, which solidifies the soil by physical adsorption and mechanical fixation, and has the advantages of good solidification effect and green environmental protection.

[0009] The purpose of the present invention is achieved through the following technical solutions:

[0010] On the one hand, the present application provides an environmentally friendly soil solidifier, which is made of the following raw materials in weight percentage: 80-95% gelatin, 4-19% sodium alginate and 1-5% cellulose.

[0011] On the other hand, the present application also provides a method for preparing an environmentally friendly soil solidifier, comprising the following steps: mixing gelatin, sodium alginate and cellulose in proportion, then adding water and stirring evenly to obtain the soil solidifier.

[0012] In this application, the working principle of each raw material is:

[0013] Gelatin: Under the action of water and temperature, gelatin molecules will form a network structure. In this process, different molecules will interact with each other and form hydrogen bonds, van der Waals forces and other forces, thereby sticking other objects together. Gelatin solution will form a layer of jelly on the surface of two objects. These jelly-like substances can combine the two objects and generate adhesion, so that the two objects are firmly bonded together.

[0014] Sodium alginate: Among the curing agents, the viscosity of sodium alginate is particularly critical. It contains a large amount of -COO-, which can exhibit polyanionic behavior in aqueous solution and has a certain degree of adhesion. This adhesion helps to bind soil particles tightly together, thereby improving the strength and stability of the soil.

[0015] Sodium alginate also has obvious pH sensitivity. Under acidic conditions, -COO- is converted into -COOH, the degree of ionization is reduced, the hydrophilicity of sodium alginate is reduced, and the molecular chain shrinks. When the pH value increases, the -COOH group continues to dissociate, the hydrophilicity of sodium alginate increases, and the molecular chain stretches. This characteristic makes sodium alginate have different curing effects under different pH environments, which can be adjusted according to specific needs.

[0016] Cellulose: When cellulose is combined with gelatin to prepare a composite film, strong hydrogen bonding occurs between the hydroxyl groups of cellulose and the amino and amide groups of gelatin molecules, which helps to form a stable supramolecular structure. This composite form of cellulose and gelatin can improve the toughness and mechanical properties of the solidified soil.

[0017] Beneficial effects of the present invention:

[0018] 1. The raw materials of the soil solidifier of the present application are only gelatin, sodium alginate and cellulose. All three raw materials are common and low-cost. The preparation method is simple, does not require large-scale machinery and strict environment, has low manufacturing cost and good solidification effect. Compared with traditional soil solidifiers, it reduces the cost of the entire production and use links.

[0019] 2. Most importantly, the raw material components of the curing agent of this application are safe, without heavy metals and other ingredients. The curing principle is based on the physical adsorption and mechanical bonding between the curing agent and the soil, so the entire curing process has little impact on the environment. In addition, the raw materials of this application have less residual chemical substances and can be gradually decomposed under natural conditions, which will not cause long-term pollution to the soil and has significant environmental safety. Especially for temporary access roads that need to be recultivated in the future, it has more practical value and practical significance. DETAILED DESCRIPTION

[0020] The following non-limiting examples serve to illustrate the invention.

[0021] Embodiment 1:

[0022] An environmentally friendly soil stabilizer is prepared by the following method:

[0023] S1: Weigh 1000 g of raw materials, and weigh the solid raw materials according to the following mass ratio: 80% industrial grade gelatin, 19% industrial grade sodium alginate (99% active ingredient), and 1% hydroxypropyl methylcellulose;

[0024] S2: The above solid raw materials are fully mixed, and then water of 15 times (i.e. 15 L) of the total mass of the solid raw materials is added, and the soil solidifying agent (liquid) of this embodiment is obtained after stirring for 3 hours.

[0025] Test the curing effect of the soil curing agent in this application on the soil:

[0026] S1. Take 10kg of dry soil and mix it with soil at a ratio of 3% (i.e. 900g of soil stabilizer);

[0027] S2. The mixing method is: add dry soil into a mixer, then add soil solidifier, take it out after stirring for 5 minutes (it is in a soft mud state at this time), put it into a 150mm*150mm*150mm cubic iron mold, and compact it with a 100kg weight for 24 hours.

[0028] S3. Take out the soil from the mold and place it in a dry constant temperature container (controlled temperature 15°C). Sprinkle water on the surface to keep it moist for the first 3 days, and then place it until 28 days.

[0029] S4. Perform compressive strength test.

[0030] Embodiment 2:

[0031] The preparation method and testing method of this embodiment are basically the same as those of Example 1, except that the mass ratio of the raw materials of each component described in Preparation Method S1 is specifically 80% industrial grade gelatin, 14% industrial grade sodium alginate (99% active ingredient), and 6% hydroxypropyl methylcellulose.

[0032] Embodiment 3:

[0033] The preparation method and testing method of this embodiment are basically the same as those of Example 1, except that the mass ratio of the raw materials of each component described in Preparation Method S1 is specifically 80% industrial grade gelatin, 9% industrial grade sodium alginate (99% active ingredient), and 11% hydroxypropyl methylcellulose.

[0034] Embodiment 4:

[0035] The preparation method and testing method of this embodiment are basically the same as those of Example 1, except that the mass ratio of the raw materials of each component in the preparation method S1 is specifically 80% industrial grade gelatin, 4% industrial grade sodium alginate (99% active ingredient), and 16% hydroxypropyl methylcellulose.

[0036] Embodiment 5:

[0037] The preparation method and testing method of this embodiment are basically the same as those of Example 1, except that the mass ratio of the raw materials of each component described in Preparation Method S1 is specifically 85% industrial grade gelatin, 14% industrial grade sodium alginate (99% active ingredient), and 1% hydroxypropyl methylcellulose.

[0038] Embodiment 6:

[0039] The preparation method and testing method of this embodiment are basically the same as those of Example 1, except that the mass ratio of the raw materials of each component described in Preparation Method S1 is specifically 85% industrial grade gelatin, 9% industrial grade sodium alginate (99% active ingredient), and 6% hydroxypropyl methylcellulose.

[0040] Embodiment 7:

[0041] The preparation method and testing method of this embodiment are basically the same as those of Example 1, except that the mass ratio of the raw materials of each component described in Preparation Method S1 is specifically 85% industrial grade gelatin, 4% industrial grade sodium alginate (99% active ingredient), and 11% hydroxypropyl methylcellulose.

[0042] Embodiment 8:

[0043] The preparation method and testing method of this embodiment are basically the same as those of Example 1, except that the mass ratio of the raw materials of each component described in Preparation Method S1 is specifically 90% industrial grade gelatin, 9% industrial grade sodium alginate (99% active ingredient), and 1% hydroxypropyl methylcellulose.

[0044] Embodiment 9:

[0045] The preparation method and testing method of this embodiment are basically the same as those of Example 1, except that the mass ratio of the raw materials of each component described in Preparation Method S1 is specifically 90% industrial grade gelatin, 4% industrial grade sodium alginate (99% active ingredient), and 6% hydroxypropyl methylcellulose.

[0046] Embodiment 10:

[0047] The preparation method and testing method of this embodiment are basically the same as those of Example 1, except that the mass ratio of the raw materials of each component in the preparation method S1 is specifically 95% industrial grade gelatin, 4% industrial grade sodium alginate (99% active ingredient), and 1% hydroxypropyl methylcellulose.

[0048] Embodiment 11:

[0049] The preparation method and testing method of this embodiment are basically the same as those of Example 1, except that the mass ratio of the raw materials of each component in the preparation method S1 is specifically 90% industrial grade gelatin, 8% industrial grade sodium alginate (99% active ingredient), and 2% hydroxypropyl methylcellulose.

[0050] Embodiment 12:

[0051] The preparation method and testing method of this embodiment are basically the same as those of Example 1, except that the mass ratio of the raw materials of each component described in Preparation Method S1 is specifically 90% industrial grade gelatin, 7% industrial grade sodium alginate (99% active ingredient), and 3% hydroxypropyl methylcellulose.

[0052] Embodiment 13:

[0053] The preparation method and testing method of this embodiment are basically the same as those of Example 1, except that the mass ratio of the raw materials of each component in the preparation method S1 is specifically 90% industrial grade gelatin, 6% industrial grade sodium alginate (99% active ingredient), and 4% hydroxypropyl methylcellulose.

[0054] Embodiment 14:

[0055] The preparation method and testing method of this embodiment are basically the same as those of Example 1, except that the mass ratio of the raw materials of each component described in Preparation Method S1 is specifically 90% industrial grade gelatin, 5% industrial grade sodium alginate (99% active ingredient), and 5% hydroxypropyl methylcellulose.

[0056] The effects of different proportions of the curing agent on the properties of the cured soil were investigated, and the results are shown in Table 1.

[0057] Table 1

[0058]

[0059]

[0060] Through experimental groups 1, 5, 8, and 10, it can be concluded that with the increase in the amount of gelatin added, the compressive strength of the solidified soil first increases and then decreases, indicating that the amount of gelatin added is not the more the better, and it is appropriate to keep it at around 90%.

[0061] It can be concluded from experimental groups 1-4, 5-7, and 8-10 that the addition amount of sodium alginate is lower than the addition amount of cellulose, which will have a significant impact on the compressive strength of the solidified soil.

[0062] It can be concluded from experimental groups 8 and 11-14 that the overall effect is better when the addition amount of sodium alginate / cellulose is greater than 2.

[0063] Embodiment 15:

[0064] An environmentally friendly soil stabilizer is prepared by the following method:

[0065] S1: Weigh 1000 g of raw materials, and weigh the solid raw materials according to the following mass ratio: 90% industrial grade gelatin, 9% industrial grade sodium alginate (99% active ingredient), and 1% hydroxypropyl methylcellulose;

[0066] S2: The above solid raw materials are fully mixed, and then 15 times (i.e. 15 L) of water in an amount of the total mass of the solid raw materials is added, and the soil solidifying agent (liquid) of this embodiment is obtained after stirring for 0.5 hours.

[0067] Test the curing effect of the soil curing agent in this application on the soil:

[0068] S1: Take 10kg of dry soil and mix it with soil at a ratio of 3% (i.e. 900g of soil stabilizer);

[0069] S2: The mixing method is: add dry soil into a mixer, then add soil solidifier, take it out after stirring for 5 minutes (it is in a soft mud state at this time), put it into a 150mm*150mm*150mm cubic iron mold, and compact it with a 100kg weight for 24 hours.

[0070] S3: Take out the soil from the mold and place it in a dry constant temperature container (controlled at 15°C). Sprinkle water on the surface to keep it moist for the first 3 days, and then place it until 28 days.

[0071] S4: Perform compressive strength test.

[0072] Embodiment 16:

[0073] The preparation method of this embodiment is basically the same as that of Example 15, except that the stirring time in step S2 of the preparation method is specifically 1 h;

[0074] Embodiment 17:

[0075] The preparation method of this embodiment is basically the same as that of Example 15, except that the stirring time in step S2 of the preparation method is specifically 1.5 h;

[0076] Embodiment 18:

[0077] The preparation method of this embodiment is basically the same as that of Example 15, except that the stirring time in step S2 of the preparation method is specifically 2 hours;

[0078] Embodiment 19:

[0079] The preparation method of this embodiment is basically the same as that of Example 15, except that the stirring time in step S2 of the preparation method is specifically 2.5 h;

[0080] Embodiment 20:

[0081] The preparation method of this embodiment is basically the same as that of Example 15, except that the stirring time in step S2 of the preparation method is specifically 3.5 h;

[0082] Embodiment 21:

[0083] The preparation method of this embodiment is basically the same as that of Example 15, except that the stirring time in step S2 of the preparation method is specifically 4 hours;

[0084] The effect of stirring time on the compressive strength of soil stabilizer during the preparation of the stabilizer was investigated. The results are shown in Table 2.

[0085] Table 2

[0086]

[0087]

[0088] It can be seen from Table 2 that with the increase of stirring time, the raw materials are mixed more evenly and the compressive strength of the final product is higher. When the stirring time reaches 3h, further increasing the stirring time has no significant effect on the compressive strength of the product. Therefore, considering the cost and time, the best stirring time is 3h.

[0089] Embodiment 22:

[0090] An environmentally friendly soil stabilizer is prepared by the following method:

[0091] S1: Weigh 1000 g of raw materials, and weigh the solid raw materials according to the following mass ratio: 90% industrial grade gelatin, 9% industrial grade sodium alginate (99% active ingredient), and 1% hydroxypropyl methylcellulose;

[0092] S2: The above solid raw materials are fully mixed, and then water in an amount of 3 times (i.e. 3 L) of the total mass of the solid raw materials is added, and the soil solidifying agent (liquid) of this embodiment is obtained after stirring for 3 hours.

[0093] Test the curing effect of the soil curing agent in this application on the soil:

[0094] S1: Take 10kg of dry soil and mix it with soil at a ratio of 3% (i.e. 900g of soil stabilizer);

[0095] S2: The mixing method is: add dry soil into a mixer, then add soil solidifier, take it out after stirring for 5 minutes (it is in a soft mud state at this time), put it into a 150mm*150mm*150mm cubic iron mold, and compact it with a 100kg weight for 24 hours.

[0096] S3: Take out the soil from the mold and place it in a dry constant temperature container (controlled at 15°C). Sprinkle water on the surface to keep it moist for the first 3 days, and then place it until 28 days.

[0097] S4: Perform compressive strength test.

[0098] Embodiment 23:

[0099] The preparation method of this embodiment is basically the same as that of Example 22, except that the amount of water added in step S2 of the preparation method is different, specifically, 6 times (i.e., 6 L) of water is added to the total mass of the solid raw materials;

[0100] Embodiment 24:

[0101] The preparation method of this embodiment is basically the same as that of Example 22, except that the amount of water added in step S2 of the preparation method is different, specifically, 9 times (i.e., 9 L) of water is added to the total mass of the solid raw materials;

[0102] Embodiment 25:

[0103] The preparation method of this embodiment is basically the same as that of Example 22, except that the amount of water added in step S2 of the preparation method is different, specifically, 12 times (i.e., 12 L) of water is added to the total mass of the solid raw material;

[0104] Embodiment 26:

[0105] The preparation method of this embodiment is basically the same as that of Example 22, except that the amount of water added in step S2 of the preparation method is different, specifically, 18 times (i.e., 18 L) of water is added to the total mass of the solid raw materials;

[0106] Embodiment 27:

[0107] The preparation method of this embodiment is basically the same as that of Example 22, except that the amount of water added in step S2 of the preparation method is different, specifically, 21 times (i.e., 21 L) of water is added to the total mass of the solid raw materials;

[0108] The effect of the amount of water added in the preparation method on the compressive strength of the soil after subsequent soil solidification by the soil solidifier was investigated, and the results are shown in Table 3.

[0109] Table 3

[0110]

[0111] As can be seen from Table 3, the compressive strength of the mixture in experimental group 22 could not be determined because the mixture did not show sufficient fluidity after mixing and the test could not be carried out. The compressive strength of the mixture in experimental groups 8, 23-27 increased with the increase of water addition and finally reached equilibrium at 15 times the water addition.

[0112] The above basic examples of the present invention and their further optional examples can be freely combined to form multiple embodiments, all of which are embodiments that can be adopted and claimed for protection by the present invention. In the scheme of the present invention, each optional example can be arbitrarily combined with any other basic examples and optional examples.

[0113] The above description is only a preferred embodiment of the present invention and is not intended to limit the present invention. Any modifications, equivalent substitutions and improvements made within the spirit and principles of the present invention should be included in the protection scope of the present invention.

Claims

1. An environmentally friendly soil solidifier, characterized in that: The invention is prepared from the following raw materials in weight percentage: 80-95% gelatin, 4-19% sodium alginate and 1-5% cellulose.

2. An environmentally friendly soil solidifier according to claim 1, characterized in that: The gelatin is industrial gelatin.

3. The environmentally friendly soil solidifier according to claim 1, characterized in that: The sodium alginate is industrial grade and has an effective content of 99%.

4. The environmentally friendly soil solidifier according to claim 1, characterized in that: The cellulose is hydroxypropyl methylcellulose.

5. The environmentally friendly soil solidifier according to claim 1, characterized in that: The weight ratio of sodium alginate to cellulose is ≥2.

6. A method for preparing an environmentally friendly soil solidifying agent as claimed in any one of claims 1 to 5, characterized in that: The method comprises the following steps: mixing gelatin, sodium alginate and cellulose in proportion, and then adding water and stirring the mixture evenly to obtain the soil solidifying agent.

7. The method for preparing an environmentally friendly soil solidifying agent according to claim 6, characterized in that: The weight of the added water is 15-20 times that of the solid raw material.

8. The method for preparing an environmentally friendly soil solidifying agent according to claim 6, characterized in that: The stirring time is 3-5h.

Citation Information

Cited By

  • Preparation method of lignin-based dual-network hydrogel and application of lignin-based dual-network hydrogel in soil remediation of mining area

    CN121378800A