Vanadium slag oxygen-enriched flash roasting transformation method
Through mechanical activation of vanadium slag and oxygen-rich flash roasting technology, the problems of high energy consumption, low efficiency and low vanadium conversion rate in the vanadium slag roasting process are solved, and the rapid and efficient oxidation transformation of vanadium slag and high vanadium leaching rate are achieved, which has the advantages of Economic and environmentally friendly advantages.
Patent Information
- Application Number
- CN202410960199.6
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Filing Date
- 2024-07-17
- Publication Date
- 2024-10-01
AI Technical Summary
The existing vanadium slag roasting process has problems such as high energy consumption, low efficiency, high consumption of auxiliary materials, and low vanadium conversion rate, making it difficult to meet the needs of clean and efficient production.
The method of mechanical activation of vanadium slag and oxygen-rich flash roasting is adopted, and oxygen-rich flash roasting is carried out for 3s-15s through injection feeding. Mechanical activation is used to increase the exposed area and surface energy of vanadium slag powder, and combined with oxygen-rich injection to achieve rapid Oxidative transformation avoids balling and improves roasting efficiency.
It significantly improves the oxidation transformation efficiency of vanadium slag, shortens the roasting time, increases the vanadium leaching rate, reduces the consumption of auxiliary materials and wastewater treatment costs, and achieves cost-effective vanadium extraction.
Smart Images

Figure CN118726744A_ABST
Abstract
Description
Technical Field
[0001] The present application relates to the field of vanadium slag roasting, and in particular to a method for transforming vanadium slag into oxygen-enriched flash roasting. Background Art
[0002] Vanadium is a rare metal with a high melting point. As an important strategic resource, it is widely used in the three fields of steel metallurgy, titanium alloy and chemical industry. Vanadium-titanium magnetite is currently the most important and most economical vanadium resource. The concentrate of vanadium-titanium magnetite is processed by blast furnace-converter to produce vanadium slag, which can enrich vanadium.
[0003] The main chemical components of vanadium slag include: V2O5, V2O3, Cr2O3, FeO, Fe2O3, TiO2, etc. The main phase compositions include spinel phase, silicate phase and quartz phase, of which the spinel phase accounts for about 40%. Most of the vanadium exists in spinel in the form of trivalent vanadium, usually forming complex spinels FeO·V2O3 and MnO·V2O3 with elements such as iron and manganese. The rest is composed of fayalite, pyroxene phase, silicate phase and a small amount of free metallic iron tightly wrapping the spinel, forming a complex inclusion phase system.
[0004] Oxidation roasting is the most critical link in the process chain of vanadium extraction from vanadium slag. Its purpose is to destroy the lattice constraints of vanadium slag under high temperature and make low-cost insoluble vanadium (V 3+ ) is oxidized to high-valent soluble vanadium (V 5+ ). The mainstream oxidation roasting process can be divided into sodium roasting and calcium roasting according to different additives. The sodium roasting process has strong adaptability to raw materials and is the most widely used and most mature process for vanadium slag extraction at home and abroad. However, this process consumes a lot of sodium salt and has relatively strict requirements on the content of SiO2 and CaO in the vanadium slag raw materials; during the roasting process, the material is easy to agglomerate, stick to the furnace, and form rings, and tailings need to be added for dilution, resulting in reduced efficiency of the roasting equipment. Compared with sodium roasting, calcium roasting has the advantages of strong raw material adaptability, relatively cheap calcification agents, and easy treatment of leached slag and wastewater after roasting acid leaching. However, the vanadium leaching rate of this process is low, generally below 80%; the addition of a large amount of calcium-containing compounds during the roasting process not only greatly increases the consumption of sulfuric acid in the acid leaching process, but also causes the vanadium extraction tailings to contain high S, which deteriorates the recycling performance of the vanadium extraction tailings.
[0005] Whether it is sodium roasting or calcium roasting process, industrial production mainly uses rotary kiln as roasting production equipment. The material and hot air in the rotary kiln move in reverse, and the vanadium slag moves from the end of the kiln to the head of the kiln, through the process of low temperature to high temperature and then to low temperature. The vanadium slag stays in the kiln for about 4h-6h. Since the vanadium slag contains more silicon-containing low-melting-point substances, increasing the reaction temperature is prone to ring formation. Therefore, from a thermodynamic point of view, it is difficult to increase the vanadium extraction rate by increasing the temperature.
[0006] Patent CN100582257C discloses a method for roasting high calcium vanadium slag in a fluidized equipment. In this method, vanadium slag with a CaO / V2O5 weight ratio in the range of 0.5-0.7 is added to the fluidized equipment for fluidized roasting. The roasting time is 30min-150min. The roasted clinker obtained is leached with sulfuric acid to further produce vanadium products. Compared with traditional rotary kiln and multi-chamber furnace roasting, this method has high production efficiency and large equipment capacity. However, this technology has not broken through the scope of calcification roasting. The weight ratio of CaO / V2O5 in its raw materials is 0.5-0.7. Therefore, the micro-area encapsulation of the powder has not been solved, resulting in a low leaching rate of vanadium in roasted sand, less than 88%; Patent CN112267028B discloses a method and application for extracting vanadium and chromium from vanadium slag. This method adds 0.5%-2% of a promoter and mixes it with vanadium slag for grinding. The powder is roasted in two stages to obtain a roasted product. The roasted product is acid-leached in two stages, coupled with hydrolysis to precipitate vanadium, which greatly reduces the consumption of leaching agents and wastewater treatment costs, and has a good treatment effect. This method adds a small amount of promoter to catalytically enhance the transformation effect of vanadium slag, but the addition of promoters such as FeCl3 places high requirements on the equipment for roasting, flue gas treatment and wet extraction of roasted products, and needs to consider Cl - Open circuit problem.
[0007] The existing vanadium slag roasting and transformation process cannot meet the development trend of clean and efficient production. Therefore, it is urgent to develop a vanadium slag roasting transformation method that is energy-saving, environmentally friendly, and economically efficient.
[0008] In view of this, the present invention is proposed. Summary of the invention
[0009] The purpose of the present application is to provide a method for transformation of oxygen-enriched flash roasting of vanadium slag to solve the above-mentioned problems.
[0010] To achieve the above objectives, the present application provides a method for transformation of vanadium slag by oxygen-enriched flash roasting, comprising: Mechanically activating the vanadium slag to obtain vanadium slag powder; The vanadium slag powder is fed by oxygen-enriched injection, and oxygen-enriched flash roasting is performed to obtain a transformation product and roasting flue gas; The roasting flue gas is subjected to dust collection to obtain a fine particle transformation product; The time for the oxygen-enriched flash roasting of the vanadium slag powder is 3s-15s.
[0011] Optionally, the method for transformation of vanadium slag by oxygen-enriched flash roasting satisfies at least one of the following conditions: A. The mechanical activation is dry grinding, which includes one or more of a rod mill, a ball mill, a vertical mill, and a fan mill; B. The particle size of the vanadium slag powder is -0.15mm, accounting for 100%, and the particle size of -0.074mm, accounting for 85%-98%.
[0012] Optionally, the particle size of the vanadium slag powder is 25 μm-48 μm, accounting for 50%-80%.
[0013] Optionally, the method for transformation of vanadium slag by oxygen-enriched flash roasting satisfies at least one of the following conditions: A. The volume concentration of oxygen in the oxygen-enriched oxygen is 25%-60%; B. The oxygen excess coefficient during the oxygen-enriched flash roasting process is 1.05-1.3; C. The maximum temperature of the vanadium slag powder during the oxygen-enriched flash roasting is 800°C-900°C.
[0014] Optionally, the oxygen-enriched flash roasting is carried out in a flash roasting furnace.
[0015] Optionally, the flash roasting furnace comprises an injection port, which is a spiral injection port and is divided into a powder channel, a central air channel and an external air channel; The fine-particle vanadium slag powder enters the injection port through the powder channel, is dispersed by the central wind in the central wind channel, and is supplemented by the external wind in the external wind channel, and is injected into the flash roasting furnace in an atomized and dispersed state.
[0016] Optionally, the method for transformation of vanadium slag by oxygen-enriched flash roasting satisfies at least one of the following conditions: A. The flash roasting furnace includes a ship-shaped furnace body, a discharge furnace bottom, a heating system, a flue gas dust collection system and a smoke exhaust system. The heating system includes a heating method of hot air and / or a combustion gun; B. During the oxygen-enriched flash roasting, the temperature of the high temperature zone of the flash roasting furnace is 800°C-1050°C, and the residence time of the vanadium slag powder in the high temperature zone is 3s-10s.
[0017] Optionally, the temperature of the high temperature zone in the flash roasting furnace is 900°C-1000°C.
[0018] Optionally, the dust collection includes dry dust collection, and the dry dust collection includes one or more of sedimentation bin dust collection, cyclone dust collection and bag dust collection.
[0019] Optionally, the dust collection also produces dust collection tail gas, which is sprayed with alkali solution before being discharged in compliance with emission standards.
[0020] Compared with the prior art, the beneficial effects of this application include: The method for oxygen-enriched flash roasting transformation of vanadium slag provided in the present application obtains vanadium slag powder through mechanical activation, which, on the one hand, significantly increases the exposed area of vanadium spinel in the vanadium slag, which is beneficial to mineral separation and enrichment of valuable metal elements; on the other hand, it increases the surface energy of the particles, greatly improving the kinetic conditions of the roasting reaction; the vanadium slag powder is then treated by oxygen-enriched flash roasting, the contact area between the vanadium slag powder and oxygen is large, the gas-solid reaction is sufficient, and the oxidation transformation of the vanadium slag can be achieved within seconds, which greatly shortens the roasting time and improves the roasting efficiency, while effectively avoiding the balling and ringing phenomenon caused by the long roasting time and the melting and solidification of low-melting-point materials in the existing rotary kiln roasting process; no auxiliary materials are added during the roasting process, and the reaction performance of the vanadium slag particles is improved through mechanical activation, and then the vanadium slag powder is directly oxygen-enriched flash roasted without adding any auxiliary materials, and the oxidation transformation of the vanadium slag is completed instantly and efficiently, which solves the problems of large additive consumption, long roasting time, poor heat and mass transfer effect, and low vanadium conversion rate in the existing oxidation roasting process to the greatest extent, has high economic and environmental value, and has broad application prospects. BRIEF DESCRIPTION OF THE DRAWINGS
[0021] In order to more clearly illustrate the technical solutions of the embodiments of the present application, the drawings required for use in the embodiments will be briefly introduced below. It should be understood that the following drawings only show certain embodiments of the present application and therefore should not be regarded as limiting the scope of the present application.
[0022] Figure 1 is a front view of an injection port in a flash roasting furnace; Figure 2 A view of the injection port in the flash roasting furnace; Figure 3 This is a schematic flow chart of the method for transformation of oxygen-enriched flash roasting of vanadium slag provided in Example 1.
[0023] Description of main component symbols: 1-inlet of central wind channel; 2-inlet of powder channel; 3-inlet of external wind channel; 4-external wind channel outlet; 5-exit of powder channel; 6-spiral guide cone; 7-exit of central wind channel. DETAILED DESCRIPTION
[0024] As used herein: "Prepared from" is synonymous with "comprising." As used herein, the terms "comprising," "including," "having," "containing," or any other variation thereof, are intended to cover a non-exclusive inclusion. For example, a composition, process, method, article, or apparatus that comprises the listed elements is not necessarily limited to only those elements but may include other elements not expressly listed or inherent to such composition, process, method, article, or apparatus.
[0025] The conjunction "consisting of excludes any unspecified element, step, or component. If used in a claim, this phrase renders the claim closed-ended so that it does not include materials other than those described, except for conventional impurities associated therewith. When the phrase "consisting of" appears in a clause of the body of a claim rather than immediately following the subject matter, it limits only the elements described in that clause; other elements are not excluded from the claim as a whole.
[0026] When an amount, concentration, or other value or parameter is expressed as a range, a preferred range, or a range defined by a series of upper preferred values and lower preferred values, this should be understood as specifically disclosing all ranges formed by any pairing of any range upper limit or preferred value with any range lower limit or preferred value, regardless of whether the range is disclosed separately. For example, when a range of "1 to 5" is disclosed, the described range should be interpreted as including ranges "1 to 4", "1 to 3", "1 to 2", "1 to 2 and 4 to 5", "1 to 3 and 5", etc. When a numerical range is described in this article, unless otherwise stated, the range is intended to include its end values and all integers and fractions within the range.
[0027] In these examples, parts and percentages are by mass unless otherwise indicated.
[0028] "Parts by mass" refers to the basic unit of measurement for expressing the mass ratio of multiple components. 1 part can represent any unit mass, such as 1g or 2.689g. If the mass parts of component A are a parts and the mass parts of component B are b parts, then the ratio of the mass of component A to the mass of component B is a:b. Alternatively, it means that the mass of component A is aK and the mass of component B is bK (K is an arbitrary number, indicating a multiple factor). It should not be misunderstood that, unlike the mass parts, the sum of the mass parts of all components is not limited to 100 parts.
[0029] "And / or" is used to indicate that one or both of the stated situations may occur, for example, A and / or B includes (A and B) and (A or B).
[0030] The present application provides a method for transformation of vanadium slag by oxygen-enriched flash roasting, comprising: Mechanically activating the vanadium slag to obtain vanadium slag powder; The vanadium slag powder is fed by oxygen-enriched injection, and oxygen-enriched flash roasting is performed to obtain a transformation product and roasting flue gas; The roasting flue gas is subjected to dust collection to obtain a fine particle transformation product; The time for the oxygen-enriched flash roasting of the vanadium slag powder is 3s-15s.
[0031] Optionally, the time for oxygen-enriched flash roasting of the vanadium slag powder can be 3s, 4s, 5s, 6s, 7s, 8s, 9s, 10s, 11s, 12s, 13s, 14s, 15s or any value between 3s and 15s.
[0032] It should be noted that the transformation products and fine-particle transformation products obtained in the present application complete the oxidation roasting process instantaneously, and no sintering occurs. In the subsequent leaching process, no secondary grinding is required. In addition, the method for oxygen-enriched flash roasting transformation of vanadium slag provided in the present application avoids the sintering and encapsulation of vanadium-containing minerals by impurity mineral phases and added auxiliary materials in the vanadium slag. The obtained transformation products and fine-particle transformation products are completely oxidized and transformed. In the subsequent leaching process, the wet treatment vanadium leaching rate is high. This method can significantly improve the oxidation transformation effect of iron-containing minerals in vanadium slag. The iron in the transformation products and fine-particle transformation products is produced in the form of Fe2O3, and is not dissolved during the leaching process of the roasted product, thereby improving the selectivity of the leaching of the roasted product.
[0033] In some embodiments, the method for transformation of vanadium slag by oxygen-enriched flash roasting satisfies at least one of the following conditions: A. The mechanical activation is dry grinding, which includes one or more of a rod mill, a ball mill, a vertical mill, and a fan mill; B. The particle size of the vanadium slag powder is -0.15mm, accounting for 100%, and the particle size of -0.074mm, accounting for 85%-98%.
[0034] Optionally, the proportion of the particle size of the vanadium slag powder -0.074 mm can be 85%, 86%, 87%, 88%, 89%, 90%, 91%, 92%, 93%, 94%, 95%, 96%, 97%, 98% or any value between 85% and 98%.
[0035] It should be noted that when the particle size of the vanadium slag powder is -0.15mm, accounting for 100%, and -0.074mm, accounting for 85%-98%, it is more appropriate to use flash roasting to convert the dissociation degree of the vanadium slag mineral under this particle size. If the particle size is too coarse, the conversion efficiency will be low, and if the particle size is too fine, the smoke rate during the flash roasting process will be high.
[0036] In some embodiments, the particle size of the vanadium slag powder is 25 μm-48 μm, accounting for 50%-80%.
[0037] Optionally, the proportion of the vanadium slag powder with a particle size of 25 μm-48 μm can be 50%, 55%, 60%, 65%, 70%, 75%, 80% or any value between 50% and 80%.
[0038] It should be noted that the particle size of vanadium slag powder is 25μm-48μm, accounting for 50%-80%, and the particle size of 25μm-48μm accounts for less than 50%. If the proportion is too high, the transformation rate of the roasting product will be low; if the proportion is too high, it will increase the mechanical activation cost, and at the same time, the smoke rate of the flash roasting process will increase, and the dust collection load will increase.
[0039] In some embodiments, the method for transformation of vanadium slag by oxygen-enriched flash roasting satisfies at least one of the following conditions: A. The volume concentration of oxygen in the oxygen-enriched oxygen is 25%-60%; Optionally, the volume concentration of oxygen in the oxygen enrichment may be 25%, 30%, 35%, 40%, 45%, 50%, 55%, 60% or any value between 25% and 60%; It should be noted that when the volume concentration of oxygen in oxygen-enriched gas is 25%-60%, the total gas volume entering the furnace during flash roasting is more consistent with the mechanical activation particle size of the vanadium slag, ensuring sufficient oxygen concentration (oxygen potential) for the transformation of the vanadium slag and a reasonable residence time; if the oxygen concentration is too low, the total gas volume entering the furnace is large, the vanadium slag particles stay in the high temperature zone for insufficient time, and the instantaneous transformation is not complete; if the oxygen concentration is too high, the overall gas volume is relatively small, and the vanadium slag particles are not well dispersed, which will also affect the transformation effect.
[0040] B. The oxygen excess coefficient during the oxygen-enriched flash roasting process is 1.05-1.3; Optionally, the oxygen excess coefficient during oxygen-enriched flash roasting may be 1.05, 1.1, 1.15, 1.2, 1.25, 1.3 or any value between 1.05 and 1.3; It should be noted that when the oxygen excess coefficient is 1.05-1.3 during oxygen-enriched flash roasting, the total amount of flue gas / oxygen is small, and the heat consumption and cost are low while ensuring the oxidation transformation of vanadium slag; when the oxygen excess coefficient is lower than 1.05, the transformation efficiency of vanadium slag will be insufficient, and when the oxygen excess coefficient exceeds 1.3, the oxygen consumption will be large, the flue gas heat loss will be high, and the cost will be high. C. The maximum temperature of the vanadium slag powder during the oxygen-enriched flash roasting is 800°C-900°C.
[0041] Optionally, the maximum temperature of the vanadium slag powder during oxygen-enriched flash roasting can be 800°C, 810°C, 820°C, 830°C, 840°C, 850°C, 860°C, 870°C, 880°C, 890°C, 900°C or any value between 800°C and 900°C.
[0042] It should be noted that when the maximum temperature of the vanadium slag powder during oxygen-enriched flash roasting is 800℃-900℃, it can ensure the complete transformation of the vanadium slag and avoid bonding at the source; if the temperature of the vanadium slag powder is lower than 800℃, the transformation is incomplete and the leaching rate of the transformation product is low; if the temperature of the vanadium slag powder exceeds 900℃, it may cause the vanadium slag particles to melt, bond and agglomerate, which will also reduce the transformation effect.
[0043] In some embodiments, the flash roasting is performed in a flash roasting furnace.
[0044] In some embodiments, the flash roasting furnace includes an injection port, which is a spiral injection port and is divided into a powder channel, a central air channel and an external air channel; The fine-particle vanadium slag powder enters the injection port through the powder channel, is dispersed by the central wind in the central wind channel, and is supplemented by the external wind in the external wind channel, and is injected into the flash roasting furnace in an atomized and dispersed state.
[0045] In some embodiments, the method for transformation of vanadium slag by oxygen-enriched flash roasting satisfies at least one of the following conditions: A. The flash roasting furnace includes a ship-shaped furnace body, a discharge furnace bottom, a heating system, a flue gas dust collection system and a smoke exhaust system. The heating system includes a heating method of hot air and / or a combustion gun; B. During the oxygen-enriched flash roasting, the temperature of the high temperature zone of the flash roasting furnace is 800°C-1050°C, and the residence time of the vanadium slag powder in the high temperature zone is 3s-10s.
[0046] Optionally, during oxygen-enriched flash roasting, the temperature of the high temperature zone of the flash roasting furnace can be 800°C, 850°C, 900°C, 950°C, 1000°C, 1050°C or any value between 800°C and 1050°C, and the residence time of the vanadium slag powder in the high temperature zone can be 3s, 4s, 5s, 6s, 7s, 8s, 9s, 10s or any value between 3s and 10s.
[0047] It should be noted that when the high temperature zone of the flash roasting furnace is 800℃-1050℃ and the residence time of the vanadium slag powder in the high temperature zone is 3s-10s, the transformation of the vanadium slag is achieved quickly. When the temperature is lower than 800℃, the transformation is incomplete. When the temperature exceeds 1050℃, local adhesion and wrapping may occur, which will also cause a low transformation rate. In addition, within a reasonable temperature range, the residence time in the high temperature zone can be reduced as the temperature rises.
[0048] In some embodiments, the high temperature zone in the flash calcining furnace has a temperature of 900°C-1000°C.
[0049] Optionally, the temperature of the high temperature zone in the flash roasting furnace can be 900°C, 910°C, 920°C, 930°C, 940°C, 950°C, 960°C, 970°C, 980°C, 990°C, 1000°C or any value between 900°C and 1000°C.
[0050] It should be noted that when the temperature of the high temperature zone in the flash roasting furnace is 900℃-1000℃ (the temperature of the high temperature zone of the heat supplement gun), the temperature of the vanadium slag powder can reach 800-900℃ after instantaneous heat exchange, and the oxidation transformation is completed under the action of oxygen enrichment.
[0051] In some embodiments, the dust collection includes dry dust collection, and the dry dust collection includes one or more of sedimentation bin dust collection, cyclone dust collection and bag dust collection.
[0052] In some embodiments, the dust collection also produces dust collection tail gas, which is sprayed with alkali solution before being discharged in compliance with emission standards.
[0053] It should be noted that the method for oxygen-enriched flash roasting transformation of vanadium slag provided in the present application does not involve the addition of auxiliary materials such as calcium compounds and sodium compounds, so the prepared dust-collected tail gas contains less harmful components such as SO2 and HCl, and only requires alkaline solution spraying to remove a small amount of SO2 brought in by the fuel to meet emission standards.
[0054] The embodiments of the present application will be described in detail below in conjunction with specific examples, but it will be appreciated by those skilled in the art that the following examples are only used to illustrate the present application and should not be considered as limiting the scope of the present application. If specific conditions are not specified in the examples, they are carried out according to normal conditions or the conditions recommended by the manufacturer. If the manufacturer is not specified for the reagents or instruments used, they are all conventional products that can be purchased commercially.
[0055] Prior to this, the injection port provided in this application is described. Figure 1 and Figure 2 As shown, the injection port of the present application includes 1-central wind channel, 2-powder channel inlet, 3-external wind channel, 4-external wind channel outlet, 5-powder channel outlet, 6-spiral guide cone and 7-central wind channel outlet, wherein 4-external wind channel outlet is evenly distributed in an annular pattern, and 5-powder channel outlet is annularly distributed. The present application generates negative pressure at 5-powder channel outlet (annular discharge port) through the synergistic effect of 7-central wind channel outlet and 4-external wind channel outlet, and vanadium slag powder is added through 2-powder channel inlet to 5-annular discharge port, and after dispersed flow guidance by 6-spiral guide cone, it enters the preheated flash furnace in an atomized and dispersed state with the synergistic effect of 7-central wind and 4-external wind, and the powder particles are instantly heated up and complete oxidation transformation under the action of oxygen enrichment.
[0056] Example 1 This embodiment provides a method for transformation of vanadium slag by oxygen-enriched flash roasting, comprising: Take 500kg of vanadium slag (V9.81%, TFe32.94%, Cr3.06%), use dry ball mill mechanical activation to obtain -0.15mm vanadium slag powder, of which -0.074mm accounts for 95%, and 25μm-48μm accounts for 63%; The vanadium slag powder is added into a flash roasting furnace preheated to 950°C by oxygen-enriched injection, wherein: the oxygen-enriched concentration is 40% and the oxygen excess coefficient is 1.2; The oxygen-enriched flash roasting time of the vanadium slag powder is 10 seconds, and the residence time in the high temperature zone of the flash furnace is 6 seconds. The maximum temperature of the vanadium slag powder is 860°C, and the transformation product and roasting flue gas are obtained. The roasting flue gas is collected by settling bin, cyclone and bag to obtain fine particle transformation products and dust collection tail gas, which is then discharged after being sprayed with alkali solution.
[0057] The method flow of this embodiment is as follows Figure 3 shown.
[0058] After the above treatment, 455.9 kg of transformation product (roasted sand) was obtained; 85.8 kg of roasting flue gas was obtained, and after uniform mixing, 541.7 kg of mixed material (V 9.03%, TFe 30.32%, Cr 2.81%) was obtained; after leaching inspection, the vanadium leaching rate of the product was 97.83%, and the Fe and Cr leaching rates were only 1.58% and 0.87% respectively.
[0059] Example 2 This embodiment provides a method for transformation of vanadium slag by oxygen-enriched flash roasting, comprising: Take 500kg of vanadium slag (V9.81%, TFe32.94%, Cr3.06%) and use vibrating rod mill for mechanical activation to obtain -0.15mm vanadium slag powder, of which -0.074mm accounts for 93% and 25μm-48μm accounts for 52%; The vanadium slag powder is added into a flash roasting furnace preheated to 900°C by oxygen-enriched injection, wherein: the oxygen-enriched concentration is 28% and the oxygen excess coefficient is 1.1; The oxygen-enriched flash roasting time of the vanadium slag powder is 6 seconds, and the residence time in the high temperature zone of the flash furnace is 4 seconds. The maximum temperature of the vanadium slag powder is 845°C, and the transformation product and roasting flue gas are obtained. The roasting flue gas is collected by settling bin, cyclone and bag to obtain fine particle transformation products and dust collection tail gas, which is then discharged after being sprayed with alkali solution.
[0060] After the above treatment, 462.5 kg of transformation product (roasted sand) was obtained; 78.6 kg of roasting flue gas was evenly mixed to obtain 541.1 kg of mixed material (V9.04%, TFe30.35%, Cr2.82%); after leaching inspection, the vanadium leaching rate of the product was 97.25%, and the Fe and Cr leaching rates were 1.89% and 0.99% respectively.
[0061] Example 3 This embodiment provides a method for transformation of vanadium slag by oxygen-enriched flash roasting, comprising: Take 500kg of vanadium slag (V9.81%, TFe32.94%, Cr3.06%), use vertical mill dry grinding mechanical activation to obtain -0.15mm vanadium slag powder, of which -0.074mm accounts for 95%, and 25μm-48μm accounts for 78%; The vanadium slag powder is added into a flash roasting furnace preheated to 880°C by oxygen-enriched injection, wherein: the oxygen-enriched concentration is 55%, and the oxygen excess coefficient is 1.15; The oxygen-enriched flash roasting time of the vanadium slag powder is 12 seconds, and the residence time in the high temperature zone of the flash furnace is 7 seconds. The maximum temperature of the vanadium slag powder is 835°C, and the transformation product and roasting flue gas are obtained. The roasting flue gas is collected by settling bin, cyclone and bag to obtain fine particle transformation products and dust collection tail gas, which is then discharged after being sprayed with alkali solution.
[0062] After the above treatment, 445.4 kg of transformation product (roasted sand) was obtained; 97.8 kg of roasting flue gas was mixed evenly to obtain 543.2 kg of mixed material (V9.00%, TFe30.23%, Cr2.81%); after leaching inspection, the vanadium leaching rate of the product was 98.13%, and the Fe and Cr leaching rates were only 1.23% and 0.68% respectively.
[0063] Comparative Example 1 This comparative example provides a method for roasting transformation of vanadium slag, which is different from Example 1 in that: in this comparative example, the particle size of the vanadium slag powder is -0.15mm, accounting for 80%, of which -0.074mm accounts for 73%, and 25μm-48μm accounts for 20%. Other conditions are consistent with Example 1.
[0064] The vanadium leaching rate of the roasted product was 85.34%, and the leaching rates of Fe and Cr were 9.58% and 1.87%, respectively.
[0065] Comparative Example 2 This comparative example provides a method for roasting transformation of vanadium slag, which is different from Example 1 in that the injection gas is compressed air, the air excess coefficient is 1.0, and other conditions are consistent with Example 1.
[0066] The leaching rate of vanadium in the roasted product was 87.34%, and the leaching rates of Fe and Cr were 9.66% and 1.59%, respectively.
[0067] Comparative Example 3 This comparative example provides a method for vanadium slag roasting transformation, which is different from Example 1 in that this comparative example uses a conventional spiral chute to feed vanadium slag powder into a flash roasting furnace, and oxygen-enriched air is added to the flash furnace. Other conditions are consistent with Example 1.
[0068] The leaching rates of vanadium, Fe and Cr in the roasted product were 80.05%, 15.87% and 2.31%, respectively.
[0069] Comparative Example 4 This comparative example provides a method for roasting transformation of vanadium slag, which is different from Example 1 in that the vanadium slag powder in this comparative example stays in the high temperature zone of the flash furnace for 30 seconds, the maximum temperature of the vanadium slag powder is 780°C, and other conditions are consistent with Example 1.
[0070] The vanadium leaching rate of the roasted product was 86.13%, and the Fe and Cr leaching rates were 7.89% and 2.34%, respectively.
[0071] Comparative Example 5 This comparative example provides a method for roasting transformation of vanadium slag, which is different from Example 1 in that: the vanadium slag powder in this comparative example stays in the high temperature zone of the flash furnace for 5 seconds, the maximum temperature of the vanadium slag powder is 1080°C, and other conditions are consistent with Example 1.
[0072] The vanadium leaching rate of the roasted product was 95.21%, and the Fe and Cr leaching rates were 1.74% and 0.98%, respectively.
[0073] It can be seen from the above experiments that, relative to Example 1, when the particle size of mechanical activation in Comparative Example 1 is not within the scope of the present application, the powder particle size is coarse, the instantaneous conversion is not complete, and the vanadium leaching rate is low.
[0074] Compared with Example 1, when the oxygen excess coefficient in Comparative Example 2 is not within the scope of the present application, the air process coefficient is insufficient, the degree of vanadium oxidation transformation is insufficient, and the vanadium leaching rate of the roasting product is low.
[0075] Compared with Example 1, when Comparative Example 3 adopts conventional feeding method, so that the vanadium slag powder cannot be sprayed into the flash roasting furnace in an atomized and dispersed state, the vanadium slag powder is aggregated and accumulated, the oxygen potential of the aggregated micro-area is insufficient, the transformation is not complete, and the vanadium leaching rate of the product is low.
[0076] Compared with Example 1, when the temperature of the high temperature zone of oxygen-enriched flash roasting in Comparative Example 4 is lower than 800°C, even if it stays in the high temperature zone for 30 seconds, the vanadium leaching rate of the roasted product is only 86.13%; and when the temperature exceeds 1050°C, micro-region sintering and encapsulation may occur in the powder, and the vanadium leaching rate of the roasted product decreases to 96.13%.
[0077] In summary, the method of the present invention can achieve rapid and efficient transformation of vanadium slag. The above method obtains vanadium slag particles by mechanical activation, and then by oxygen-enriched injection, the powder particles are dispersed and rapidly heated and instantly oxidized and transformed by oxygen-enriched, which significantly improves the oxidation transformation effect of roasted sand, and effectively inhibits the leaching of Fe and Cr. The vanadium leaching rate of the roasted product is >97%, the iron leaching rate is <2%, and the chromium leaching rate is <1%, and the selective extraction effect is significant.
[0078] Finally, it should be noted that the above embodiments are only used to illustrate the technical solutions of the present application, rather than to limit it. Although the present application has been described in detail with reference to the aforementioned embodiments, those skilled in the art should understand that they can still modify the technical solutions described in the aforementioned embodiments, or replace some or all of the technical features therein with equivalents. However, these modifications or replacements do not cause the essence of the corresponding technical solutions to deviate from the scope of the technical solutions of the embodiments of the present application.
[0079] In addition, those skilled in the art will appreciate that, although some embodiments herein include certain features included in other embodiments but not other features, the combination of features of different embodiments is meant to be within the scope of the present application and form different embodiments. For example, in the above claims, any one of the claimed embodiments may be used in any combination. The information disclosed in this background technology section is intended only to deepen the understanding of the overall background technology of the present application and should not be regarded as an admission or in any form of implication that the information constitutes prior art known to those skilled in the art.
Claims
1. A method for transformation of vanadium slag by oxygen-enriched flash roasting, characterized in that: include: Mechanically activating the vanadium slag to obtain vanadium slag powder; The vanadium slag powder is fed by oxygen-enriched injection, and oxygen-enriched flash roasting is performed to obtain a transformation product and roasting flue gas; The roasting flue gas is subjected to dust collection to obtain a fine particle transformation product; The time for the oxygen-enriched flash roasting of the vanadium slag powder is 3s-15s.
2. The method for transformation of vanadium slag by oxygen-enriched flash roasting according to claim 1, characterized in that: At least one of the following conditions is met: A. The mechanical activation is dry grinding, which includes one or more of a rod mill, a ball mill, a vertical mill, and a fan mill; B. The particle size of the vanadium slag powder is -0.15mm, accounting for 100%, and the particle size of -0.074mm, accounting for 85%-98%.
3. The method for transformation of vanadium slag by oxygen-enriched flash roasting according to claim 2, characterized in that: The particle size of the vanadium slag powder is 25 μm-48 μm, accounting for 50%-80%.
4. The method for transformation of vanadium slag by oxygen-enriched flash roasting according to claim 1, characterized in that: At least one of the following conditions is met: A. The volume concentration of oxygen in the oxygen-enriched oxygen is 25%-60%; B. The oxygen excess coefficient during the oxygen-enriched flash roasting process is 1.05-1.3; C. The maximum temperature of the vanadium slag powder during the oxygen-enriched flash roasting is 800°C-900°C.
5. The method for transformation of vanadium slag by oxygen-enriched flash roasting according to claim 1, characterized in that: The oxygen-enriched flash roasting is carried out in a flash roasting furnace.
6. The method for transformation of vanadium slag by oxygen-enriched flash roasting according to claim 5, characterized in that: The flash roasting furnace comprises an injection port, which is a spiral injection port and is divided into a powder channel, a central air channel and an external air channel; The fine-particle vanadium slag powder enters the injection port through the powder channel, is dispersed by the central wind in the central wind channel, and is supplemented by the external wind in the external wind channel, and is injected into the flash roasting furnace in an atomized and dispersed state.
7. The method for transformation of vanadium slag by oxygen-enriched flash roasting according to claim 5, characterized in that: At least one of the following conditions is met: A. The flash roasting furnace comprises a ship-shaped furnace body, a discharge furnace bottom, a heating system, a flue gas dust collection system and a smoke exhaust system, and the heating system comprises a heating method of hot air and / or a combustion gun; B. During the oxygen-enriched flash roasting, the temperature of the high temperature zone of the flash roasting furnace is 800°C-1050°C, and the residence time of the vanadium slag powder in the high temperature zone is 3s-10s.
8. The method for transformation of vanadium slag by oxygen-enriched flash roasting according to claim 7, characterized in that: The temperature of the high temperature zone in the flash roasting furnace is 900°C-1000°C.
9. The method for transformation of vanadium slag by oxygen-enriched flash roasting according to claim 1, characterized in that: The dust collection includes dry dust collection, and the dry dust collection includes one or more of sedimentation bin dust collection, cyclone dust collection and bag dust collection.
10. The method for transformation of vanadium slag by oxygen-enriched flash roasting according to any one of claims 1 to 9, characterized in that: The dust collection also obtains dust collection tail gas, and the dust collection tail gas meets the emission standards after being sprayed with alkali solution.