Preparation method of low-cost reduction microalloyed steel
By adding cost-effective associated iron ore powder during the smelting process of micro-alloy steel, increasing the Ni, Cr, and V elements in the molten iron, reducing the use of external alloys, solving the problems of high cost and composition uniformity, and achieving low-cost, stable Preparation of high-quality micro-alloyed steel enhances the corrosion resistance and resource utilization efficiency of the steel.
Patent Information
- Application Number
- CN202410823223.1
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Filing Date
- 2024-06-25
- Publication Date
- 2024-10-01
AI Technical Summary
In the existing micro-alloy steel smelting methods, the use of high-cost micro-alloys such as vanadium nitrogen, ferroniobium and other alloys increases production costs and affects the uniformity of molten steel composition and the quality of the steel. The fluctuation of the alloy addition affects the market resistance. Risk capabilities and resource utilization efficiency.
By adding cost-effective associated iron ore powder to the sinter, the Ni, Cr, and V elements in the molten iron are increased, the amount of external alloy added is reduced, and the residual elements in the blast furnace smelting and converter smelting processes are used to replace trace elements to control the molten steel. It forms a protective layer of nickel oxide and chromium oxide to delay corrosion of the steel surface.
It reduces alloy consumption and production costs, improves the uniformity of molten steel composition and the corrosion resistance of steel, optimizes resource utilization, and stabilizes the quality and economic benefits of steel.
Abstract
Description
Technical Field
[0001] The invention relates to the technical field of metallurgical production, in particular to a method for preparing low-cost reduced-weight microalloy steel. Background Art
[0002] With the sharp decline in downstream demand for steel, the era of increasing output to achieve profitability has become a thing of the past. At present and for a long time to come, the steel market is a period of volatile low prices. Technological innovation and process innovation are effective measures to reduce costs.
[0003] The existing smelting method of micro-alloy steels such as HRB400 / 400E, HRB500 / 500E, and HRB600 is to add alloys during the steel-making process after molten iron + scrap steel is smelted in a converter (the alloys of HRB500E, HRB600 and higher-grade steel grades are added in a refining furnace). During the alloy-adding process, nitrogen or argon is blown into the ladle (generally for more than 6 minutes), and then the steel bar head / scrap billet head is added to adjust the temperature to the required temperature, and the ladle is hoisted to the packaging turntable for continuous casting into billets. Commonly used alloys include bulk alloys such as silicon-manganese and ferrosilicon. Micro-alloys such as vanadium-nitrogen and ferroniobium need to be added to achieve grain refinement, improve strength and strength-to-yield ratio and low-temperature performance, and improve the welding performance of steel to meet the strength, toughness and welding performance of steel. The main purpose of blowing nitrogen or argon during the alloy addition process is to make the composition of the molten steel uniform. For HRB500E, HRB600 and higher grade series of micro-alloyed steels, refining furnaces are required to further improve the uniformity of alloy elements in the molten steel and reduce the impurity content, making the molten steel more uniform and cleaner.
[0004] The existing technology has the following problems: first, the prices of alloys, especially microalloys such as vanadium nitrogen and niobium iron, are high and fluctuate greatly, which increases the cost of steel billets and reduces the market's risk resistance. Large-scale consumption is not conducive to resource conservation; second, the amount of alloy added directly affects the time for blowing nitrogen or argon into the ladle, thereby affecting the uniformity of the composition of the molten steel and the start temperature of continuous casting, which in turn affects the quality of the steel and the production rhythm. Summary of the invention
[0005] The object of the present invention is to provide a method for preparing a low-cost reduced-weight microalloy steel to solve the problems existing in the above-mentioned background technology.
[0006] To achieve the above-mentioned purpose, the present invention provides the following technical scheme: a method for preparing low-cost reduced-weight micro-alloy steel, comprising sintering iron ore powder into agglomerates, smelting the sintered ore in a blast furnace and smelting molten iron in a converter, characterized in that: during the sintering process, cost-effective and difficult-to-separate associated iron ore powder containing Ni, Cr and V is added, the sintered ore increases the content of Ni, Cr and V elements in the molten iron during smelting in the blast furnace, and the residual Ni, Cr and V elements in the molten iron after smelting in the converter enter the molten steel, replacing Mn, Si, V, Nb and other trace elements in the molten steel, thereby reducing the amount of external silicon-manganese alloy, silicon-iron alloy, vanadium-nitrogen alloy and niobium-iron alloy added.
[0007] Furthermore, in the sintering process, 6.0-9.0% of low-nickel laterite nickel ore and 15% of Russian fine powder are added to the sintered ore, the Cr content in the molten iron is controlled to be less than or equal to 0.25%, and the TiO 2 The load shall not exceed 5.30 kg / t.
[0008] Furthermore, the low-nickel laterite nickel ore contains 0.50-0.80% Ni and 0.50-0.80% Cr. 2 O 3 The content of ore is between 3.60% and 4.30%, and it needs to be screened and dried before sintering.
[0009] Furthermore, the Russian refined powder TFe is about 64.00%, V 2 O 5 Between 0.210 and 0.245%.
[0010] Furthermore, in the blast furnace smelting process, the binary basicity of the slag is 1.05 to 1.15 times, and the silicon content of the molten iron is controlled at 0.30 to 0.60%.
[0011] Furthermore, during the converter smelting, the oxygen blowing time and intensity are controlled to ensure that the final carbon content of the molten steel is above 0.050%.
[0012] Compared with the prior art, the beneficial effects of the present invention are: first, the cost of ingredients is reduced, and the consumption of alloys is reduced, thereby achieving good economic benefits; second, due to the addition of residual Ni, Cr, V and other elements in the molten steel, the composition of the molten steel is more uniform, the composition deviation is reduced, the quality of the steel is more stable, and a nickel oxide and chromium oxide protective layer is formed on the surface of the steel, which slows down the surface corrosion rate of the steel and enhances the surface corrosion resistance of the steel; third, through sintering, roasting and blast furnace smelting, the cost-effective and difficult-to-separate multi-metal associated ores are fully utilized, thereby achieving resource optimization and reducing resource waste. DETAILED DESCRIPTION
[0013] The invention provides a technical solution: a preparation method of low-cost reduced-volume microalloy steel, comprising sintering iron ore powder into blocks, smelting the sintered ore in a blast furnace and smelting molten iron in a converter, characterized in that: during the sintering process, associated iron ore powder containing Ni, Cr and V with high cost performance and difficult to separate is added, the sintered ore increases the content of Ni, Cr and V elements in the molten iron during smelting in the blast furnace, and the residual Ni, Cr and V elements in the molten iron after smelting in the converter enter into molten steel, replace Mn, Si, V, Nb and other trace elements in the molten steel, and reduce the addition amount of external silicon-manganese alloy, silicon-iron alloy, vanadium-nitrogen alloy and niobium-iron alloy.
[0014] Addition and control of Ni and Cr elements: The key to increasing the residual Ni and Cr content in molten steel by adding laterite nickel ore is to control the [Cr] content in molten iron to not exceed 0.25%; adding 6.0-9.0% low-nickel laterite nickel ore (Ni at 0.50-0.80%, Cr at 0.50-0.80%) to the sintered ore is to increase the residual Ni and Cr content in molten steel by adding laterite nickel ore. 2 O 3 When the sintering ratio is controlled at 3.60-4.30%, the sintering ratio is controlled at 75.0-80.0%, 100% of Ni and 80.0% of Cr enter the molten iron during blast furnace smelting, and the Ni and Cr contents in the molten iron are 0.060-0.090% and 0.20-0.25% respectively; the molten iron consumption for steelmaking is 800 kg / t (about 76%), and the recovery rates of Ni and Cr elements are 99.0% and 60.0-70.0% respectively during converter smelting, and the residual Ni and Cr contents in the molten steel are 0.046-0.068% and 0.0092-0.115% respectively.
[0015] Since laterite nickel ore has high water content (about 20.0% crystal water content, about 15.0% natural water content), high impurity content of raw ore, high viscosity, large fluctuation of composition, etc., it needs to be screened and dried before sintering. The proportion of laterite nickel ore in sintering is determined according to the specific composition of each laterite nickel ore and the proportion of sintered ore added to the blast furnace. The test results show that it is reasonable to control it at 6.0-9.0%.
[0016] Increase and control of V element: The key to increasing the residual V content of molten steel by adding Russian refined powder is to control the TiO 2 The load does not exceed 5.30 kg / t. Sintered ore is added with 15.00% TFe, about 64.00%, V 2 O 5 When the Russian fine powder is 0.210-0.245%, the sintering ore ratio is controlled at 75.0-80.0% (at this time, the blast furnace TiO 2The load is 5.22 kg / t), the vanadium recovery rate of vanadium-containing iron ore during blast furnace smelting is about 45.0-65.0%, and the vanadium content in molten iron is 0.010-0.014%; the single consumption of molten iron for steelmaking is 800 kg / t (about 76.0%), the V recovery rate during converter smelting is about 25.0-65.0%, and the residual V content in molten steel is about 0.004-0.006%.
[0017] The recovery rates of Ni and Cr in the iron ore entering the blast furnace are 99.0% and 75.0-85.0% respectively, and the Cr content in the molten iron is not more than 0.25%, otherwise it is easy to cause the gun to stick during converter smelting. At the same time, the binary basicity of the slag is 1.05-1.15 times, and the silicon content of the molten iron is controlled at 0.30-0.60%, ensuring the smooth smelting of the blast furnace and good slag fluidity.
[0018] During converter smelting, since the molten iron temperature is 20 to 30°C higher than that of ordinary steelmaking pig iron, the oxygen blowing time and intensity must be reasonably controlled to ensure that the final carbon content of the molten steel is above 0.050%. This reduces the oxygen blowing time and the chance of the oxygen lance sticking, while ensuring the steelmaking temperature and reducing molten steel inclusions, thereby achieving the purpose of improving the quality of molten steel.
[0019] Industrial tests have shown that there is the following quantitative substitution relationship between Ni, Cr, V and Mn in steel: (1) In HRB400E, HRB500E, and HRB600 steel bars, increasing Cr by 0.11% and Ni by 0.050% can simultaneously reduce Mn by 0.10% brought into silicon-manganese alloy and V by 0.005% brought into vanadium-nitrogen alloy.
[0020] (2) The residual V content in the molten steel cannot be equivalent to the V content increased by the external addition of vanadium-nitrogen alloy. The fundamental reason is that the vanadium-nitrogen alloy contains nitrogen, which can better promote the precipitation of vanadium and obtain a greater precipitation strengthening effect. However, industrial rolling practice has proved that every increase of 0.005% can simultaneously reduce the V content brought into the vanadium-nitrogen alloy by 0.002%.
[0021] The improved process has achieved good economic benefits: First, it reduces the cost of ingredients and alloy consumption. The cost of steelmaking ingredients is reduced by 9.88 yuan / t steel. The increase of Ni and Cr elements reduces the consumption of silicon-manganese alloy and vanadium-nitrogen alloy by 1.71 kg / t steel and 0.070 kg / t steel respectively. The increase of residual V element reduces the consumption of vanadium-nitrogen alloy by 0.028 kg / t steel and reduces the alloy cost by 22.02 yuan / t steel. The total reduction of steel cost is 31.90 yuan / t steel.
[0022] Secondly, the quality of steel is improved. Since residual Ni, Cr, V and other elements are added to the molten steel and the amount of alloy added is reduced, under the same time of post-furnace nitrogen or argon blowing, the composition of the molten steel is more uniform, the composition deviation is reduced, and the quality of the steel is more stable. The V element refines the grain size of the steel and provides the toughness of the steel. The Ni and Cr elements form a protective layer of nickel oxide and chromium oxide on the surface of the steel, which slows down the surface corrosion rate of the steel and enhances the surface corrosion resistance of the steel.
[0023] Although embodiments of the present invention have been shown and described, it will be appreciated by those skilled in the art that various changes, modifications, substitutions and variations may be made to the embodiments without departing from the principles and spirit of the present invention, and that the scope of the present invention is defined by the appended claims and their equivalents.
Claims
1. A method for preparing low-cost reduced-weight microalloy steel, comprising sintering iron ore powder into agglomerates, smelting the sintered ore in a blast furnace and smelting molten iron in a converter, characterized in that: During the sintering process, cost-effective and difficult-to-separate associated iron ore powder containing Ni, Cr and V is added. The sintered ore increases the content of Ni, Cr and V in molten iron during blast furnace smelting. The residual Ni, Cr and V elements in the molten iron after smelting in the converter enter the molten steel, replacing Mn, Si, V, Nb and other trace elements in the molten steel, and reducing the amount of external silicon-manganese alloy, ferrosilicon alloy, vanadium-nitrogen alloy and ferroniobium alloy added.
2. The method for preparing low-cost reduced-weight microalloyed steel according to claim 1, characterized in that: In the sintering process, 6.0-9.0% of low-nickel laterite nickel ore and 15.0% of Russian fine powder are added to the sintered ore, the Cr content in the molten iron is controlled to be less than or equal to 0.25%, and the TiO2 load of the blast furnace charge is controlled not to exceed 5.30 kg / t.
3. A method for preparing low-cost reduced-weight microalloyed steel according to claim 2, characterized in that: The low-nickel laterite nickel ore contains 0.50-0.80% Ni and 3.60-4.30% Cr2O3, and needs to be screened and dried before sintering and batching.
4. The method for preparing low-cost reduced-weight microalloyed steel according to claim 2, characterized in that: The Russian refined powder has a TFe content of about 64.00% and a V2O5 content of 0.210-0.245%.
5. The method for preparing low-cost reduced-weight microalloyed steel according to claim 1, characterized in that: In the blast furnace smelting process, the binary basicity of the slag is 1.05-1.15 times, and the silicon content of the molten iron is controlled at 0.30-0.60%.
6. The method for preparing low-cost reduced-weight microalloyed steel according to claim 1, characterized in that: During the converter smelting, the oxygen blowing time and intensity are controlled to ensure that the final carbon content of the molten steel is above 0.050%.