Method for synergistically extracting lithium from fluorgypsum and lithium ore
By roasting lithium ore and fluorogypsum at high temperature, the fluoride ions in the fluorogypsum are used to improve the extraction efficiency of lithium, solving the problems of low resource utilization and high cost in the lithium extraction process from lithium ore, and realizing efficient and environmentally friendly lithium production. resource development.
Patent Information
- Application Number
- CN202410742803.8
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Filing Date
- 2024-06-11
- Publication Date
- 2024-10-01
AI Technical Summary
In the existing lithium extraction process from lithium ores, the resource utilization rate of fluorogypsum is low, the cost is high, and there are problems of environmental pollution and equipment corrosion, making it difficult to achieve efficient lithium extraction.
The lithium ore and fluorogypsum are crushed, mixed, granulated and roasted at high temperature. CaF2 and H2SO4 in the fluorogypsum are used to generate free fluoride ions, which promote the reaction in the lithium ore, improve the extraction efficiency of lithium sulfate, and obtain high-quality lithium sulfate through water leaching. Concentration of lithium-containing mother liquor.
It achieves efficient extraction of lithium resources, reduces production costs, reduces waste emissions, improves lithium extraction efficiency, is suitable for large-scale production, and conforms to the principle of sustainable development.
Smart Images

Figure CN118726764A_ABST
Abstract
Description
Technical Field
[0001] The present invention relates to the field of lithium extraction from lithium ore, and in particular to a method for extracting lithium from fluorgypsum and lithium ore in a coordinated manner. Background Art
[0002] Lithium ore mining mainly comes from three types of deposits: pegmatite type, brine type, and sedimentary rock type. Lithium in pegmatite is often found in ores such as spodumene and lepidolite. Brine-type lithium deposits can be divided into underground brine type and salt lake brine type. Sedimentary rock type mainly refers to lithium ore with low lithium grade existing in sedimentary rocks. At present, the most mined lithium ore in the world is pegmatite type and brine type. my country has rich reserves of lepidolite resources, and the development of efficient lithium extraction technology is of great significance to the comprehensive utilization of lepidolite resources. Due to the low energy consumption of sulfate roasting method and short roasting and leaching time, the mainstream extraction process currently used for lepidolite is sulfate roasting method. However, there are few processes that use fluorgypsum as a sulfate source and lepidolite for coordinated smelting. With the widespread application of lithium batteries, the demand for lithium is increasing. Sedimentary rock type lithium ore has not been developed and utilized on a large scale due to its low lithium grade, different occurrence states of lithium in different types of lithium ores, and late discovery. In the context of vigorous development of new energy industry, in order to ease the shortage of lithium resources, lithium clay ore is expected to become the focus of research in the future. The main methods of extracting lithium from clay lithium ore are direct leaching and auxiliary roasting. There are few studies on the process of using fluorinated gypsum and lithium clay ore for synergistic smelting.
[0003] Fluorogypsum is a byproduct of the reaction between concentrated sulfuric acid and fluorite during the production of hydrofluoric acid. Fluorogypsum contains a small amount of unreacted CaF2 and H2SO4. The residual sulfuric acid needs to be neutralized with an appropriate amount of lime before it can be stored. In the hydrofluoric acid industry, about 3.6 tons of fluorogypsum are produced for every ton of hydrofluoric acid produced. With the rise of the fluorine chemical industry, the demand for hydrofluoric acid has gradually increased, and the resulting environmental problems have become more serious. The comprehensive utilization of waste residues is imminent.
[0004] Therefore, considering that my country's industrial byproduct fluorinated gypsum has a large output and a low resource utilization rate. Adhering to the idea of green resource utilization, the above-mentioned byproduct fluorinated gypsum can be used to react with lithium clay ores and lithium mica with large reserves to obtain a high-concentration lithium-containing leachate, thereby realizing resource recycling and environmental improvement. Patent CN201410098348.9 proposes a modified roasting-heap leaching method, in which calcium fluoride is added during the roasting process, but the price of calcium fluoride is relatively high, and it is difficult to remove fluorine in the later stage. If it is not handled properly, it will pollute the environment. In addition, fluoride ions will corrode equipment and the cost is relatively high. Patent CN202210353260.1 involves a lithium clay ore mixed with soda ash and sodium sulfate for roasting and leaching. This method is easy to corrode equipment and has a high cost. Patent CN110697740A involves a lithium extraction method for smelting lithium porcelain stone and gypsum, and the gypsum includes industrial gypsum or flue gas desulfurization gypsum, but the patent does not involve the lithium extraction efficiency of the reaction between lithium porcelain stone and desulfurization gypsum. CN115821060A proposes to mix lepidolite, calcium carbonate, sodium sulfate, potassium sulfate, etc. and then roast them at high temperature. The process additives are complex and the price of potassium sulfate is high, resulting in high cost and difficult industrial use. In addition, potassium ions are introduced, which are difficult to separate from lithium in subsequent purification. Patent CN116219204A proposes to produce lithium carbonate by reacting lepidolite with gypsum and calcium oxide, wherein the gypsum can be solid waste gypsum produced by the lime process for producing lithium hydroxide or hydrofluoric acid smelting plants, but the content of solid waste gypsum cannot exceed 50% of the total gypsum, and the waste treatment capacity is low. Summary of the invention
[0005] The purpose of the present invention is to overcome the shortcomings of the prior art and provide a method for synergistically extracting lithium by using fluorgypsum and lithium ore, the method comprising the following steps: first, crushing the lithium ore to be extracted; second, mixing the lithium ore obtained by the crushing with the fluorgypsum evenly and granulating; then, placing the granulated balls into a muffle furnace for high-temperature roasting; finally, leaching the calcined product with water, and the filtrate is a lithium-containing mother liquor; the method effectively solves the difficult problems of fluorgypsum treatment and lithium ore resource development, utilizes the special components in fluorgypsum, creatively makes the lithium recovery rate high, the cost in the lithium extraction process low, and the process simple, plays an important role in waste resource utilization and efficient development and utilization of lithium resources, and has broad application prospects.
[0006] In order to achieve the above technical effects, the following technical solutions are adopted:
[0007] A method for extracting lithium by synergistically using fluorgypsum and lithium ore, comprising the following steps:
[0008] Step S1: crushing the lithium ore to be extracted;
[0009] Step S2: uniformly mixing the crushed lithium ore obtained in step S1 with fluorgypsum and granulating;
[0010] Step S3: calcining the granulated pellets in step S2 at high temperature to obtain a calcined product;
[0011] Step S4: The calcined product obtained in step S3 is leached with a leaching agent, the filtrate is a lithium-containing mother liquor, and the leached residue is a filler.
[0012] The key to the present invention is to carry out a coordinated roasting reaction between the difficult-to-treat fluorgypsum and lithium ore to achieve resource utilization of fluorgypsum and efficient extraction of lithium resources. The method utilizes fluorgypsum, a common waste resource, to achieve resource utilization and reduce environmental pollution. Through the reaction with lithium ore, efficient extraction of lithium is achieved, meeting the demand for lithium resources. The method has simple steps, low cost, easy operation and is suitable for large-scale production.
[0013] The principle of extracting lithium by reacting lithium ore and fluorgypsum is: under high temperature conditions, fluorgypsum solidifies the free silicon dioxide in the lithium ore and produces sulfur dioxide at the same time. The sulfur dioxide reacts with the lithium in the lithium ore to form soluble lithium sulfate.
[0014]
[0015] In the above reaction, although calcium sulfate fixes a part of the free silica in the lithium ore in the first step, in the second step, free silica is produced while lithium sulfate is produced. Due to the production of free silica, the reaction may lead to the reverse reaction of the second step (refer to the reaction mechanism of the first step), that is, lithium sulfate reacts with free silica to produce lithium ore products.
[0016] On the other hand, according to the above reaction mechanism, in the second step of the reaction, since lithium sulfate and free silica are generated at the same time, the free silica will wrap or adhere to the generated lithium sulfate, so that the lithium sulfate enters the surface or inside of the free silica, hindering the dissolution of lithium sulfate in the subsequent leaching agent, so that the lithium extraction efficiency of the calcium sulfate auxiliary agent (gypsum) alone is not high. It is recorded in relevant literature that calcium sulfate itself participates in the lithium extraction reaction as an auxiliary agent, and is roasted with lithium clay ore at 800°C, 900°C, 1000°C and 1050°C for 4h, and the roasted samples are treated with water for water leaching, and the lithium leaching rates are 6%, 41%, 72% and 68% respectively.
[0017] However, the fluorinated gypsum of the present invention contains, in addition to the gypsum component, namely calcium sulfate, a small amount of unreacted CaF2 and H2SO4, which can generate free fluoride ions in the reaction system at high temperature. The fluoride ions react with the free silicon dioxide produced in the second step reaction at high temperature, and the silicon dioxide in the second step product is converted into fluorosilicate ions and removed (fluoride ions and silicon dioxide undergo ion exchange reaction, fluoride ions replace part of oxygen ions in silicon dioxide to form fluorosilicate ions, an exothermic reaction, and the reaction rate increases with increasing temperature). The advantages are: first, the reduction of free silicon dioxide is beneficial to the second step. The reaction proceeds in the forward direction, thereby increasing the yield of lithium sulfate and reducing the reverse reaction, so as to reduce the loss of lithium sulfate; on the second aspect, the reduction of free silica in the second step reaction reduces the free silica generated at the same time to wrap or adhere to the generated lithium sulfate, reduces the leaching barrier of silica to lithium sulfate, and is more conducive to the dissolution of lithium sulfate in the subsequent leaching agent, thereby further increasing the extraction efficiency of lithium sulfate; therefore, the present invention can generate free fluoride ions at high temperature through the special residual components in fluorgypsum, and the fluoride ions can greatly improve the lithium extraction efficiency of calcium sulfate as an auxiliary agent, thereby achieving a better lithium extraction effect than the prior art.
[0018] On the other hand, the negative monovalent F in fluorgypsum - During high temperature roasting, it can replace the negative divalent O in the aluminosilicate structure of lithium ore. 2- , which causes the Al-O and Si-O bonds in the mineral structure to be destroyed. To maintain the electrical neutrality of the mineral, the excess positive one-valent Li + will be "pushed out" of the lattice structure, making it susceptible to leaching.
[0019] Furthermore, the lithium ore includes one or more of lithium mica and lithium clay ore.
[0020] Furthermore, the lithium ore is crushed and ground to 200 mesh, accounting for 70% by mass.
[0021] Furthermore, the mixing mass ratio of the lithium ore to fluorgypsum is 0.5-2:1, the calcium sulfate content in the fluorgypsum is 80-85%; the calcium fluoride content is 5-10%. When the amount of fluorgypsum is too low, it cannot react completely and it is difficult to achieve efficient lithium extraction; when the amount of fluorgypsum is too high, it will lead to excessive amount of lithium extraction tailings and high processing costs.
[0022] Furthermore, the granulation uses polyacrylamide as a granulating agent, and the amount of the granulating agent is 1 to 2 wt% of the lithium ore.
[0023] The viscosity of polyacrylamide can ensure that the materials are evenly mixed, volatilize during high-temperature roasting, and produce no or small amounts of impurities.
[0024] Furthermore, the particle size of the granulated balls is 5-10 mm.
[0025] Furthermore, the calcination temperature is 800-1100° C., and the calcination time is 1-4 hours.
[0026] When the temperature is too low or the roasting time is too short, the reaction is not sufficient. As the temperature rises, the reaction between lithium ore and fluorgypsum becomes more and more complete, and the lithium leaching rate is higher. When the roasting temperature is too high, the clinker is partially sintered, and the sintered part is difficult to break, which is difficult to release during the leaching process, resulting in a decrease in the lithium leaching rate.
[0027] Furthermore, the granulated balls are calcined in a muffle furnace, and the mesh size of the calcined product is less than 100 meshes. Controlling the particle size of the calcined product within a reasonable range is conducive to improving the leaching efficiency.
[0028] Furthermore, the leaching agent is water, and the volume ratio of the calcined product to the leaching agent is 1:2-4.
[0029] Furthermore, the leaching temperature is 30-90°C, the leaching time is 30-60min, and a lithium-containing leaching solution is obtained. Controlling the liquid-to-solid ratio, leaching temperature and leaching time of the leaching process can effectively improve the leaching efficiency. Too low liquid-to-solid ratio, too low leaching temperature and too short leaching time will reduce the leaching efficiency. Too high liquid-to-solid ratio, too high leaching temperature and too long leaching time will make the leaching process costly.
[0030] The leached residue is used as cement admixture or concrete admixture.
[0031] The beneficial effects of the present invention are:
[0032] (1) Fluorogypsum is an industrial byproduct. Using it to extract lithium resources can achieve the recycling of waste, comply with the principle of sustainable development, and promote the development of the green economy.
[0033] (2) The comprehensive utilization of fluorinated gypsum and lithium ore can reduce the discharge and storage of waste, reduce the risk of pollution to soil, water sources and air, and is beneficial to the environment;
[0034] (3) The use of fluorspar and lithium ore to extract lithium in a coordinated manner can reduce the purchase of sulfate raw materials. The special residual components in fluorspar can generate free fluoride ions at high temperatures. Fluoride ions can greatly improve the efficiency of lithium extraction using calcium sulfate as an auxiliary agent, thereby achieving a better lithium extraction effect than the existing technology; reducing production costs and improving economic benefits; the method is mature, low-cost, and has strong system adaptability. BRIEF DESCRIPTION OF THE DRAWINGS
[0035] In order to more clearly illustrate the embodiments of the present invention or the technical solutions in the prior art, the drawings required for use in the embodiments or the description of the prior art will be briefly introduced below. The drawings in the following description are merely embodiments of the present invention. For ordinary technicians in this field, other drawings can be obtained based on the provided drawings without paying any creative work.
[0036] Figure 1 Schematic diagram of the process of synergistic lithium extraction from fluorgypsum and lithium ore provided in an embodiment of the present invention; DETAILED DESCRIPTION
[0037] In order to make the purpose, technical solution and advantages of the present invention more clearly understood, the present invention is further described in detail below in conjunction with the embodiments. It should be understood that the specific embodiments described herein are only used to explain the present invention and are not used to limit the present invention.
[0038] It should be noted that the following detailed descriptions are exemplary and are intended to provide further explanation of the present invention. Unless otherwise specified, all technical and scientific terms used herein have the same meanings as those commonly understood by those skilled in the art to which the present invention belongs.
[0039] It should be noted that the terms used herein are only for describing specific embodiments and are not intended to limit exemplary embodiments according to the present invention. As used herein, unless the context clearly indicates otherwise, the singular form is also intended to include the plural form. In addition, it should be understood that when the terms "comprising" and / or "including" are used in this specification, it indicates the presence of features, steps, operations and / or combinations thereof.
[0040] Embodiment 1:
[0041] according to Figure 1 As shown, the lithium extraction operation of lithium ore is carried out:
[0042] Take 100g of lithium clay ore and grind it to 200 meshes, accounting for 70% of the mass. The main components of lithium clay ore are Li2O content of 0.58%, SiO2 content of 40.48%, Al2O3 content of 20.36%, and CaO content of 20.52%. Add 50g of fluorgypsum, mix evenly, and the granulating agent is polyacrylamide, and mix to prepare a spherical material with a particle size of 10mm. The material is placed in a muffle furnace for high-temperature roasting, the roasting temperature is set to 800℃, and the roasting time is 1h. After the roasting is completed, the roasted material is cooled to 100℃ and ball-milled to less than 100 meshes, and then all the ball-milled fine materials are placed in a volume of 1L (the volume ratio of calcined material and leaching agent is 1:4) and a temperature of 30℃. Stir at a constant speed for 30min. Then filter to obtain the leachate, the leached slag is calcium aluminosilicate, which can be used as a cement admixture. After detection and analysis, the lithium extraction rate of Example 1 is 90.5%. It shows that the technical solution can use fluorinated gypsum and lithium clay ore to extract lithium in coordination. Fluorinated gypsum reacts with lithium clay ore to solidify the free silicon dioxide in the lithium clay ore sample and release sulfur dioxide, which then reacts with lithium in lithium-containing silicates to form soluble lithium sulfate. The free fluoride ions in fluorinated gypsum at high temperature further increase the efficiency of lithium extraction, making the lithium ore extraction rate 90.5%. The chemical composition of the fluorinated gypsum used is shown in Table 1.
[0043] Table 1 Chemical composition of fluorgypsum
[0044]
[0045] Embodiment 2:
[0046] according to Figure 1 As shown, the lithium extraction operation of lithium ore is carried out:
[0047] Take 100g of lithium clay ore and grind it to 200 meshes, accounting for 70% of the mass. The main components of lithium clay ore are Li2O content of 0.58%, SiO2 content of 40.48%, Al2O3 content of 20.36%, and CaO content of 20.52%. Add 200g of fluorgypsum, mix evenly, and the granulating agent is polyacrylamide, and mix to prepare a spherical material with a particle size of 5mm. The material is placed in a muffle furnace for high-temperature roasting, the roasting temperature is set to 1100℃, and the roasting time is 4h. After the roasting is completed, the roasted material is cooled to 100℃ and ball-milled to less than 100 meshes, and then all the ball-milled fine materials are placed in a volume of 1.2L (the volume ratio of the calcined material and the leaching agent is 1:2) and a temperature of 90℃. Stir at a uniform speed for 60min. Then, the leachate is obtained by filtration, and the leached slag is calcium aluminosilicate, which can be used as a cement admixture. After detection and analysis, the lithium extraction rate of Example 2 is 95.3%. This shows that the technical solution can use fluorinated gypsum and lithium clay ore to extract lithium in coordination. Fluorinated gypsum reacts with lithium clay ore to solidify the free silicon dioxide in the lithium clay ore sample and release sulfur dioxide, which then reacts with lithium in lithium-containing silicates to form soluble lithium sulfate. The free fluoride ions in fluorinated gypsum at high temperature further increase the efficiency of lithium extraction, making the lithium ore extraction rate 95.3%. The chemical composition of the fluorinated gypsum used is shown in Table 2.
[0048] Table 2 Chemical composition of fluorgypsum
[0049]
[0050] Comparative Example 1:
[0051] As a comparison with Example 1, fluorinated gypsum was replaced with natural gypsum.
[0052] Take 100g of lithium clay ore and grind it to 200 mesh, accounting for 70% by mass. Add 50g of natural gypsum, mix evenly, and use polyacrylamide as the granulating agent to prepare a spherical material with a particle size of 10mm. The material is placed in a muffle furnace for high-temperature roasting, the roasting temperature is set to 800℃, and the roasting time is 4h. After the roasting is completed, the roasted material is cooled to 100℃ and ball-milled to less than 100 mesh, and then all the ball-milled fine materials are placed in a 1L aqueous solution at a temperature of 30℃, and stirred at a uniform speed for 30min. Then the leaching solution is obtained by filtration. After detection and analysis, the lithium extraction rate of comparative example 1 is 20.5%.
[0053] Comparative Example 2:
[0054] As a comparison with Example 2, fluorinated gypsum was replaced with natural gypsum.
[0055] Take 100g of lithium clay ore and grind it to 200 mesh, accounting for 70% by mass. Add 200g of natural gypsum, mix evenly, and use polyacrylamide as the granulating agent to prepare a spherical material with a particle size of 5mm. The material is placed in a muffle furnace for high-temperature roasting, the roasting temperature is set to 1100℃, and the roasting time is 4h. After the roasting is completed, the roasted material is cooled to 100℃ and ball-milled to less than 100 mesh, and then all the ball-milled fine materials are placed in a 1L aqueous solution at a temperature of 90℃, and stirred at a uniform speed for 30min. Then the leaching solution is obtained by filtration. After detection and analysis, the lithium extraction rate of comparative example 2 is 60.5%.
[0056] Comparative Example 3:
[0057] As a comparison with Example 1, fluorgypsum was replaced with calcium sulfate.
[0058] Take 100g of lithium clay ore and grind it to 200 mesh, accounting for 70% by mass. Add 50g of calcium sulfate, mix evenly, and use polyacrylamide as the granulating agent to prepare a spherical material with a particle size of 10mm. The material is placed in a muffle furnace for high-temperature roasting, the roasting temperature is set to 800℃, and the roasting time is 4h. After the roasting is completed, the roasted material is cooled to 100℃ and ball-milled to less than 100 mesh, and then all the ball-milled fine materials are placed in a 1L aqueous solution at a temperature of 30℃, and stirred at a uniform speed for 30min. Then the leaching solution is obtained by filtration. After detection and analysis, the lithium extraction rate of comparative example 3 is 23.7%.
[0059] Comparative Example 4:
[0060] As a comparison with Example 2, fluorgypsum was replaced with calcium sulfate.
[0061] Take 100g of lithium clay ore and grind it to 200 mesh, accounting for 70% by mass. Add 200g of calcium sulfate, mix evenly, and use polyacrylamide as the granulating agent to prepare a spherical material with a particle size of 5mm. The material is placed in a muffle furnace for high-temperature roasting, the roasting temperature is set to 1100℃, and the roasting time is 4h. After the roasting is completed, the roasted material is cooled to 100℃ and ball-milled to less than 100 mesh, and then all the ball-milled fine materials are placed in a 1L aqueous solution at a temperature of 90℃, and stirred at a uniform speed for 30min. Then the leaching solution is obtained by filtration. After detection and analysis, the lithium extraction rate of comparative example 4 is 67.4%.
[0062] Comparative Example 5:
[0063] As a comparison with Example 1, fluorgypsum was replaced with calcium sulfate.
[0064] Take 100g of lithium clay ore and grind it to 200 mesh, accounting for 70% by mass. Add 50g of calcium sulfate, mix evenly, and use polyacrylamide as the granulating agent to prepare a spherical material with a particle size of 10mm. The material is placed in a muffle furnace for high-temperature roasting, the roasting temperature is set to 1100℃, and the roasting time is 4h. After the roasting is completed, the roasted material is cooled to 100℃ and ball-milled to less than 100 mesh, and then all the ball-milled fine materials are placed in a 1L aqueous solution at a temperature of 30℃, and stirred at a uniform speed for 30min. Then the leaching solution is obtained by filtration. After detection and analysis, the lithium extraction rate of comparative example 5 is 55.9%.
[0065] In summary, the present invention discloses a method for synergistically extracting lithium by using fluorgypsum and lithium ore, and the method comprises the following steps: first, crushing the lithium ore to be extracted; second, mixing the lithium ore obtained by the crushing with the fluorgypsum evenly and granulating; then, placing the granulated balls into a muffle furnace for high-temperature roasting; finally, leaching the calcined product with water, and the filtrate is a lithium-containing mother liquor; the method effectively solves the difficult problems of fluorgypsum treatment and lithium ore resource development, and utilizes the special components in fluorgypsum to generate free fluoride ions at high temperature, and the fluoride ions can greatly improve the lithium extraction efficiency of calcium sulfate as an auxiliary agent, thereby achieving a better lithium extraction effect than the prior art; the method creatively makes the lithium recovery rate high, the cost in the lithium extraction process low, and the process simple, plays an important role in the waste resource utilization and the efficient development and utilization of lithium resources, and has broad application prospects.
[0066] At this point, those skilled in the art recognize that, although the embodiments of the present invention have been shown and described in detail herein, many other variations or modifications that conform to the principles of the present invention can still be directly determined or derived based on the contents disclosed in the present invention without departing from the spirit and scope of the present invention. Therefore, the scope of the present invention should be understood and recognized as covering all such other variations or modifications.
Claims
1. A method for extracting lithium by synergistically using fluorgypsum and lithium ore. It is characterized in that The lithium extraction method comprises the following steps: Step S1: crushing the lithium ore to be extracted; Step S2: uniformly mixing the crushed lithium ore obtained in step S1 with fluorgypsum and granulating; Step S3: calcining the granulated pellets in step S2 at high temperature to obtain a calcined product; Step S4: The calcined product obtained in step S3 is leached with a leaching agent, the filtrate is a lithium-containing mother liquor, and the leached residue is a filler.
2. A method for extracting lithium by synergistically using fluorgypsum and lithium ore as claimed in claim 1, It is characterized in that The lithium ore includes one or more of lithium mica and lithium clay ore.
3. A method for extracting lithium by synergistically using fluorgypsum and lithium ore as claimed in claim 1, It is characterized in that The lithium ore is crushed and ground to 200 mesh, and the mass content accounts for 70%.
4. A method for extracting lithium by synergistically using fluorgypsum and lithium ore as claimed in claim 1, It is characterized in that The mixing mass ratio of the lithium ore to the fluorspar is 0.5-2:1, the calcium sulfate content in the fluorspar is 80-85%; the calcium fluoride content is 5-10%.
5. A method for extracting lithium by synergistically using fluorgypsum and lithium ore as claimed in claim 1, It is characterized in that The granulation adopts polyacrylamide as a granulating agent, and the dosage of the granulating agent is 1-2wt% of the lithium ore.
6. A method for extracting lithium by synergistically using fluorgypsum and lithium ore as claimed in claim 1, It is characterized in that The particle size of the granulated balls is 5-10 mm.
7. A method for extracting lithium by synergistically using fluorgypsum and lithium ore as claimed in claim 1, It is characterized in that The calcination temperature is 800-1100° C., and the calcination time is 1-4 hours.
8. A method for extracting lithium by synergistically using fluorgypsum and lithium ore as claimed in claim 1, It is characterized in that The granulated balls are calcined in a muffle furnace, and the mesh number of the calcined product is less than 100 meshes.
9. A method for extracting lithium by synergistically using fluorgypsum and lithium ore as claimed in claim 1, It is characterized in that The leaching agent is water, and the volume ratio of the calcined product to the leaching agent is 1:2-4.
10. A method for extracting lithium by synergistically using fluorgypsum and lithium ore as claimed in claim 1, It is characterized in that The leaching temperature is 30-90° C., the leaching time is 30-60 min, and a lithium-containing leaching solution is obtained. The leached residue is used as a cement admixture or a concrete admixture.
Citation Information
Cited By
Method for efficiently extracting lithium from high-potassium and high-phosphorus complex spodumene ore
CN119640051A
Resource recycling method for thallium in desulfurized gypsum and multi-stage elution device
CN121005416A
A method for resource recovery of thallium from desulfurized gypsum and a multi-stage washing and extraction device
CN121005416B
Method for extracting lithium, rubidium and cesium from lepidolite by using acidic fluorgypsum
CN121450955A