Method for recovering tungsten and vanadium from waste denitration catalyst alkaline leaching solution and product thereof
By adjusting the pH value and using different types of anion exchange resins for adsorption and desorption treatment, the problem of low tungsten and vanadium recovery quality in the alkali leaching solution of spent denitrification catalysts was solved, efficient separation and the preparation of high-purity products were achieved, and the recovery efficiency was improved. and environmental protection.
Patent Information
- Application Number
- CN202410725078.3
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Filing Date
- 2024-06-06
- Publication Date
- 2024-10-01
AI Technical Summary
The products produced by the existing tungsten and vanadium recovery process in the alkali leaching solution of spent denitrification catalysts are of low quality, and the separation efficiency of vanadium and tungsten is not high, resulting in insufficient recovery efficiency and product purity.
By adjusting the pH value of the alkali immersion solution, macroporous strong alkaline styrene-based anion exchange resin D201 is used to adsorb vanadium, and weakly alkaline acrylic anion exchange resin D314 is used to adsorb tungsten under different pH conditions, combined with sodium hydroxide solution desorption and Ammonium sulfate is precipitated, evaporated and crystallized, and high-purity ammonium metavanadate and ammonium paratungstate are separated.
It achieves efficient separation and purification of vanadium and tungsten, improves recovery efficiency and product purity. The vanadium content is less than 0.001wt%, and the tungsten content is as high as 99.99wt%. The process is environmentally friendly and sustainable, and reduces the emission of harmful substances.
Abstract
Description
Technical Field
[0001] The invention belongs to the technical field of catalyst recovery and disposal, and in particular relates to a method for recovering tungsten and vanadium from an alkaline leaching solution of a waste denitration catalyst and a product thereof. Background Art
[0002] The spent denitrification catalyst contains 1-2 wt.% V 2 O 5 and 5-10wt.% WO 3 , the rest is 80-90wt.% TiO 2 , which has economic recovery value. The current mature extraction process is sodium carbonate roasting and water leaching or sodium hydroxide leaching to extract vanadium and tungsten into the solution, while TiO 2 Transformed to Na 2 TiO 3 Remain in the slag, and the leaching liquid is NaVO after impurities are removed 3 and Na 2 WO 4 The mixed solution (containing vanadium 1-2g / L, tungsten 5-8g / L) has similar properties and similar behaviors and trends in the solution. The existing recovery process is to directly use D314 resin to adsorb and enrich all vanadium and tungsten, and then desorb to obtain a mixed solution of sodium vanadate and sodium tungstate, add ammonium salt to precipitate ammonium metavanadate, filter and add acid to adjust the pH to acidic precipitation of tungstic acid. The tungsten content in the ammonium metavanadate produced by this process reaches 0.8-1.5wt%, and the vanadium content in the tungsten product reaches 1-1.5wt%, and the product quality is low. Summary of the invention
[0003] The purpose of the present invention is to solve the problem of low quality of tungsten and vanadium products recovered from the above-mentioned alkaline leaching solution, and to provide a method for recovering tungsten and vanadium from the alkaline leaching solution of a waste denitrification catalyst and its product.
[0004] In the first aspect, a method for recovering tungsten and vanadium from an alkaline leaching solution of a spent denitration catalyst adopts the following technical scheme:
[0005] A method for recovering tungsten and vanadium from an alkali leaching solution of a spent denitrification catalyst comprises the following steps: step (1), adjusting the pH of the alkali leaching solution, wherein the alkali leaching solution adsorbs vanadium through a strong alkaline styrene-based anion exchange resin column, and adjusting the pH of the adsorption solution, wherein the adsorption solution adsorbs tungsten through a weak alkaline acrylic acid-based anion exchange resin column;
[0006] Step (2), the strong basic styrene anion exchange resin is desorbed with a strong basic solution, ammonium salt is added to precipitate vanadium, and filtered to obtain ammonium metavanadate;
[0007] Step (3), the weak base acrylic anion exchange resin is desorbed with ammonia water, evaporated and crystallized to obtain ammonium paratungstate.
[0008] Preferably, the pH of the alkaline leaching solution is adjusted to 6.5-8.5; and the pH of the adsorption solution is adjusted to 3.0-3.5.
[0009] Preferably, 20% sulfuric acid solution is used to adjust the pH.
[0010] Preferably, the strongly basic styrene anion exchange resin is D201 resin; and the weakly basic acrylic anion exchange resin is D314 resin.
[0011] Preferably, the strong alkaline solution is a 5-10wt% sodium hydroxide solution.
[0012] Preferably, the ammonium salt is ammonium sulfate.
[0013] Preferably, the concentration of the aqueous ammonia is 10-20%.
[0014] In the second aspect, a tungsten-vanadium product recovered from an alkaline leaching solution of a spent denitration catalyst adopts the following technical solution:
[0015] A tungsten-vanadium product recovered from an alkaline leaching solution of a spent denitrification catalyst, comprising an ammonium metavanadate product and an ammonium paratungstate product obtained by using any of the above-mentioned methods for recovering tungsten and vanadium from an alkaline leaching solution of a spent denitrification catalyst.
[0016] Furthermore, the content of the ammonium metavanadate product is >99.0wt%.
[0017] Furthermore, the ammonium paratungstate product has a content of >99.99wt% and a vanadium content of <0.001wt%.
[0018] Beneficial effects of the present invention:
[0019] Efficient separation and purification: By adjusting the pH value of the leaching solution, vanadium and tungsten are formed into V 4 O 12 4- and WO 4 2- , using macroporous strong alkaline anion exchange resin D201 for adsorption, effectively achieving the separation of vanadium and a small amount of tungsten.
[0020] High tungsten recovery rate: In the liquid after D201 resin adsorption, by adjusting the pH value again and using D314 resin to adsorb tungsten, a tungsten recovery rate of up to 99.98% can be achieved. This not only further improves the tungsten recovery efficiency, but also ensures that the tungsten content in the liquid after adsorption is reduced to an extremely low level (<30 mg / L), thereby improving the economy and environmental protection of the overall process.
[0021] Preparation of high-purity products: After the D201 resin is saturated with adsorption, sodium hydroxide solution is used for desorption and ammonium sulfate is added to form ammonium metavanadate precipitation with vanadium, and high-purity ammonium metavanadate products (main content of more than 99%) are obtained by filtration. Similarly, after the D314 resin is saturated with adsorption, ammonia water is used for desorption and evaporation and crystallization can be used to obtain high-purity ammonium paratungstate products (main content of more than 99.99%, vanadium content <0.001%).
[0022] Environmental protection and sustainability: The entire process not only achieves efficient separation and purification, but also pays attention to environmental protection and sustainability. By precisely controlling the conditions and process steps, the emission of harmful substances is minimized, while the recovery rate of valuable metals is increased, which meets the requirements of contemporary industry for environmental protection and efficient use of resources. DETAILED DESCRIPTION
[0023] The following examples further describe in detail the method for recovering tungsten and vanadium from the alkaline leaching solution of a waste denitrification catalyst described in the present invention and its products. For the sake of simplicity, this document cannot list all the alternative technical features and implementation schemes contained in the present invention. Therefore, those skilled in the art should know that any technical features and implementation schemes in this embodiment do not limit the scope of protection of the present invention, which includes any alternative technical features and implementation schemes adopted by all those skilled in the art without creative labor. Specifically, the implementation schemes obtained by replacing any technical feature in the present invention or combining any two or more technical features provided by the present invention should be within the scope of protection of the present invention. For those examples where specific techniques and conditions are not specified, they are carried out in accordance with the techniques and conditions described in the literature in the field or in accordance with the product manual. The reagents or instruments used where the manufacturer is not specified are all conventional products that can be purchased commercially.
[0024] Example
[0025] Example 1
[0026] Example 1 provides a method for recovering tungsten and vanadium from an alkaline leaching solution of a spent denitration catalyst, comprising the following steps: (1) taking 1L of the original alkaline leaching solution (containing vanadium 1g / L, tungsten 5g / L, alkalinity NaOH=10g / L), adding 20% sulfuric acid to adjust the pH of the solution to 6.9, passing through a D201 resin column for adsorption separation, and after adsorption, the remaining solution is 500ml, containing vanadium 8mg / L, tungsten 4.8g / L, and pH=7.1;
[0027] (2) Add 20% sulfuric acid to the remaining solution after D201 resin adsorption to adjust the solution pH to 3.0-3.5, and pass it through D314 resin column to adsorb tungsten. After adsorption, the tungsten content in the solution is 10 mg / L;
[0028] (3) After the D201 resin is saturated with adsorption, it is desorbed with a 5% sodium hydroxide solution. 100 ml of the desorbed solution contains 40 g / L vanadium and 8 g / L tungsten. Ammonium sulfate, which is twice the theoretical amount of vanadium, is added and reacted at room temperature for 3 hours with stirring. The filtrate is 100 ml and contains 1 g / L vanadium and 7.8 g / L tungsten. The main content of the ammonium metavanadate product is 99.3%, and the tungsten content is 0.03%. The solution after vanadium precipitation is then separated by adsorption by D201 resin;
[0029] (4) After the D314 resin is saturated with adsorption, it is analyzed with 10% ammonia water to obtain an ammonium tungstate solution containing 200 g / L of tungsten. The ammonium paratungstate product is obtained by evaporation and crystallization. The main content of ammonium paratungstate is 99.95% and the content of vanadium is 0.002%.
[0030] The final vanadium yield was 99.995% and the tungsten yield was 99.98%.
[0031] Example 2
[0032] Example 2 provides a method for recovering tungsten and vanadium from an alkaline leaching solution of a spent denitration catalyst, comprising the following steps: (1) taking 1L of the original alkaline leaching solution (containing vanadium 1.5 g / L, tungsten 7 g / L, alkalinity NaOH=12 g / L), adding 20% sulfuric acid to adjust the solution pH to 7.5, passing through a D201 resin column for adsorption separation, and after adsorption, the remaining solution is 500 ml, containing vanadium 5 mg / L, tungsten 6.7 g / L, and pH=7.8;
[0033] (2) Add 20% sulfuric acid to the remaining solution after D201 resin adsorption to adjust the solution pH to 3.0-3.5, and pass it through D314 resin column to adsorb tungsten. The tungsten content in the solution after adsorption is 8 mg / L;
[0034] (3) After the D201 resin is saturated with adsorption, it is desorbed with 8% sodium hydroxide solution. 100 ml of the desorbed solution contains 50 g / L vanadium and 10 g / L tungsten. Ammonium sulfate twice the theoretical amount of vanadium is added, stirred at room temperature for 3 hours, filtered, and the filtrate is 100 ml, containing 0.8 g / L vanadium and 9.9 g / L tungsten. The main content of ammonium metavanadate product is 99.5%, and the tungsten content is 0.02%. The solution after precipitating vanadium is then separated by adsorption on a D201 resin column;
[0035] (4) After the D314 resin is saturated with adsorption, it is analyzed with 10% ammonia water to obtain an ammonium tungstate solution containing 250g / L of tungsten. The ammonium paratungstate product is obtained by evaporation and crystallization. The main content of ammonium paratungstate is 99.98% and the content of vanadium is 0.001%.
[0036] The final vanadium yield was 99.997% and the tungsten yield was 99.98%.
[0037] Example 3
[0038] Example 3 provides a method for recovering tungsten and vanadium from an alkaline leaching solution of a spent denitration catalyst, comprising the following steps: (1) taking 1L of the original alkaline leaching solution (containing vanadium 1.5 g / L, tungsten 7 g / L, alkalinity NaOH = 15 g / L), adding 20% sulfuric acid to adjust the pH of the solution to 8.0, passing through a D201 resin column for adsorption separation, and after adsorption, the remaining solution of 500 ml contains vanadium 8 mg / L, tungsten 4.8 g / L, and pH = 7.8;
[0039] (2) Add 20% sulfuric acid to the remaining solution after D201 resin adsorption to adjust the solution pH to 3.0-3.5, and pass it through D314 resin column to adsorb tungsten. After adsorption, the tungsten content in the solution is 10 mg / L;
[0040] (3) After the D201 resin is saturated with adsorption, it is desorbed with a 5% sodium hydroxide solution. The desorbed solution contains 40 g / L vanadium and 8 g / L tungsten in 100 ml. Ammonium sulfate, which is twice the theoretical amount of vanadium, is added and reacted at room temperature for 3 hours. The filtrate is 100 ml and contains 1 g / L vanadium and 7.8 g / L tungsten. The main content of ammonium metavanadate product is 99.3% and the tungsten content is 0.03%. The solution after precipitating vanadium is then separated by adsorption on a D201 resin column;
[0041] (4) After the D314 resin is saturated with adsorption, it is analyzed with 10% ammonia water to obtain an ammonium tungstate solution containing 250g / L of tungsten. The ammonium paratungstate product is obtained by evaporation and crystallization. The main content of ammonium paratungstate is 99.95% and the content of vanadium is 0.002%.
[0042] The final vanadium yield was 99.96%, and the tungsten yield was 99.98%.
[0043] For ordinary technicians in the relevant field, other different forms of changes or modifications can be made based on the above description. It is not necessary and impossible to list all the implementation methods here, and the obvious changes or modifications derived from them are still within the scope of protection of the claims of the invention.
Claims
1. A method for recovering tungsten and vanadium from an alkaline leaching solution of a spent denitrification catalyst, characterized in that: The following steps are involved: Step (1), adjusting the pH of the alkaline leaching solution, the alkaline leaching solution adsorbs vanadium through a strong alkaline styrene-based anion exchange resin column, and adjusting the pH of the adsorption solution, the adsorption solution adsorbs tungsten through a weak alkaline acrylic acid-based anion exchange resin column; Step (2), the strong basic styrene anion exchange resin is desorbed with a strong basic solution, ammonium salt is added to precipitate vanadium, and filtered to obtain ammonium metavanadate; Step (3), the weak base acrylic anion exchange resin is desorbed with ammonia water, evaporated and crystallized to obtain ammonium paratungstate.
2. The method for recovering tungsten and vanadium from alkaline leaching solution of a spent denitration catalyst according to claim 1, characterized in that: The pH of the alkaline leaching solution is adjusted to 6.5-8.5; and the pH of the adsorption solution is adjusted to 3.0-3.
5.
3. The method for recovering tungsten and vanadium from an alkaline leaching solution of a spent denitration catalyst according to claim 1, characterized in that: 20% sulfuric acid solution was used to adjust the pH.
4. The method for recovering tungsten and vanadium from alkaline leaching solution of a spent denitration catalyst according to claim 1, characterized in that: The strong base styrene anion exchange resin is D201 resin; the weak base acrylic anion exchange resin is D314 resin.
5. The method for recovering tungsten and vanadium from alkaline leaching solution of a spent denitration catalyst according to claim 1, characterized in that: The strong alkali solution is a 5-10wt% sodium hydroxide solution.
6. The method for recovering tungsten and vanadium from alkaline leaching solution of a spent denitration catalyst according to claim 1, characterized in that: The ammonium salt is ammonium sulfate.
7. The method for recovering tungsten and vanadium from alkaline leaching solution of a spent denitration catalyst according to claim 1, characterized in that: The concentration of the aqueous ammonia is 10-20%.
8. A method for recovering tungsten and vanadium products from alkaline leaching solution of spent denitrification catalyst, characterized in that: An ammonium metavanadate product and an ammonium paratungstate product are obtained by using the method for recovering tungsten and vanadium from an alkaline leaching solution of a waste denitration catalyst as described in any one of claims 1 to 7.
9. The method for recovering tungsten and vanadium products from alkaline leaching solution of a spent denitrification catalyst according to claim 8, characterized in that: The content of the ammonium metavanadate product is >99.0wt%.
10. The method for recovering tungsten and vanadium products from alkaline leaching solution of a spent denitrification catalyst according to claim 8, characterized in that: The ammonium paratungstate product has a content of >99.99wt% and a vanadium content of <0.001wt%.