Corrosion-resistant aluminum alloy and preparation method thereof
By optimizing the chemical composition and process treatment of the aluminum alloy, a dense film layer is formed, which solves the problems of poor bonding force and insufficient corrosion resistance of the aluminum alloy surface film layer, achieving higher corrosion resistance and bonding force, and is suitable for many applications. kind of industrial application.
Patent Information
- Application Number
- CN202410692721.7
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Filing Date
- 2024-05-31
- Publication Date
- 2024-10-01
AI Technical Summary
The surface film layer of existing aluminum alloys has poor bonding strength and insufficient corrosion resistance, which cannot meet the market's demand for higher corrosion resistance and bonding strength.
By optimizing the chemical composition and component ratio of the aluminum alloy, an aluminum alloy substrate including Mg, Si, Mn, Cu, Zn, Ti, Sr and other components is prepared, and a dense film layer is formed on the surface to utilize corrosion resistance. Particles and specific process treatments, such as plasma spraying and heat treatment, improve the bonding force between the film layer and the substrate and the corrosion resistance.
Significantly improve the corrosion resistance and bonding strength of aluminum alloy, ensuring its mechanical properties while reducing the risk of corrosion, and improving the aesthetics and corrosion resistance of the surface appearance.
Smart Images

Figure BDA0004868779310000081 
Figure BDA0004868779310000091
Abstract
Description
Technical Field
[0001] The invention relates to the field of surface treatment of aluminum alloys, and in particular to a corrosion-resistant aluminum alloy and a preparation method thereof. Background Art
[0002] Aluminum alloy is the most widely used type of metal structural material in industry. Aluminum alloy has a series of advantages such as low density, high specific strength, good formability and corrosion resistance, low cost, etc. It is widely used in aviation, aerospace, automobile, machinery manufacturing, shipbuilding and chemical industries. The main components of traditional aluminum alloy are aluminum, magnesium and silicon. Due to the limitation of material structure, the processed aluminum alloy cannot meet the market demand. Among them, the functions of aluminum alloy are also expanding more and more, such as surface corrosion resistance, surface hydrophobicity, surface hardness, etc. In view of the surface functions of aluminum alloy, various methods are also used in the prior art to prepare a layer of functional material on the surface of aluminum alloy to give aluminum alloy certain functions, such as coating a layer of corrosion-resistant film on the surface of aluminum alloy to make aluminum alloy have higher corrosion resistance. For example, the patent application number CN201510762037.2 discloses a method for surface treatment of aluminum alloys, which reduces the traditional alkaline etching treatment, and by adding copper sulfate and polyethylene glycol to the chemical polishing solution to increase the viscosity of the chemical polishing solution, the corrosion of the aluminum alloy is reduced, and the influence of copper and zinc oxides on the formation of aluminum oxide film during anodizing is reduced, but the surface corrosion resistance of the aluminum alloy needs to be further improved. The current technology still has the problem of poor bonding between the film layer and the aluminum alloy and poor corrosion resistance. Therefore, it is of great significance to study the surface film layer of the aluminum alloy with both excellent bonding and corrosion resistance. Summary of the invention
[0003] Based on this, in order to solve the problems of poor bonding strength between aluminum alloy and its surface film layer and poor surface corrosion resistance in the prior art, the present invention provides a corrosion-resistant aluminum alloy and a preparation method thereof, and the specific technical scheme is as follows:
[0004] A corrosion-resistant aluminum alloy, comprising an aluminum alloy substrate and a film layer supported on the surface of the aluminum alloy substrate, wherein the aluminum alloy substrate comprises the following components in percentage by mass:
[0005] Mg 0.6%~0.8%, Si 0.1%~0.2%, Mn 0.01%~0.2%, Cu 0.01%~0.07%, Zn0.1%~0.5%, Ti 0.01%~0.02%, Sr 0.01%~0.03%, corrosion-resistant particles 0.01%~0.09%, the balance is Al and unavoidable impurities;
[0006] The material of the film layer includes the following preparation steps:
[0007] Tetrapropylammonium hydroxide, tetraethyl orthosilicate, sodium hydroxide, anhydrous ethanol and deionized water are mixed in a molar ratio of (5-7):(18-23):(500-550):(0.1-0.5):100, stirred at a stirring speed of 50r / min-150r / min and a temperature of 120°C-150°C for 5h-8h, then aged and washed, and then added to deionized water and dispersed evenly to obtain a film layer material with a mass fraction of 5%.
[0008] Furthermore, the aging treatment time is 10h to 15h.
[0009] Furthermore, the corrosion-resistant particles are obtained by ball-milling a mixture of chromium powder and nickel powder in a mass ratio of (1-7):(1-5).
[0010] In addition, the present invention also provides a method for preparing a corrosion-resistant aluminum alloy, the preparation method comprising the following steps:
[0011] Al-Mg alloy, Al-Si alloy, Al-Mn alloy, Al-Cu alloy, Al-Zn alloy, titanium ingot and Al-Sr alloy are added to a smelting furnace for smelting treatment, the obtained aluminum liquid is added to a holding furnace for refining, and then slag is removed, and then degassed through a filter box, and cast through a crystallizer to obtain an ingot;
[0012] Plasma spraying the corrosion-resistant particles on the surface of the ingot to obtain an aluminum alloy matrix;
[0013] The aluminum alloy substrate is subjected to a heating treatment, air-cooled to room temperature, and then placed in the material of the film layer. After being immersed, washed, and dried, a corrosion-resistant aluminum alloy is obtained.
[0014] Furthermore, the casting temperature is 720° C. to 740° C., the casting speed is 45 mm / min to 55 mm / min, and the casting cooling water flow rate is 200 L / min to 230 L / min.
[0015] Furthermore, the spraying voltage of the plasma spraying process is 65V-70V, the spraying distance is 25mm-35mm, the rotation rate is 120rpm-130rpm, the powder feeding rate is 120g / min-180g / min, and the spraying angle is 45°.
[0016] Furthermore, the particle size of the corrosion-resistant particles is 25 μm to 30 μm.
[0017] Furthermore, the heating treatment is as follows: heating the aluminum alloy substrate to 90°C-100°C at a rate of 1°C / min-3°C / min, keeping the temperature for 3h-5h, continuing to heat the aluminum alloy substrate to 120°C-180°C, keeping the temperature for 1h-5h, then cooling the aluminum alloy substrate to 90°C-100°C at a rate of 1°C / min-3°C / min, keeping the temperature for 3h-5h, heating the aluminum alloy substrate to 180°C-250°C again, keeping the temperature for 3h-5h, and then cooling the aluminum alloy substrate to 100°C-120°C.
[0018] Furthermore, the immersion treatment is carried out at a temperature of 100° C. to 120° C. and for a time of 2 h to 5 h.
[0019] Furthermore, the drying process is carried out at a temperature of 95° C. to 105° C. and for a time of 30 min to 50 min.
[0020] In the above scheme, by optimizing the chemical composition and component ratio of the aluminum alloy, the β phase does not appear in the aluminum alloy matrix, and the defects in the crystal are relatively few. While ensuring the mechanical properties of the aluminum alloy, the corrosion resistance of the aluminum alloy can be further promoted. In addition, by adding corrosion-resistant particles, a dense protective layer can be formed, which is stable in chemical corrosion resistance. After heating treatment, the thermal stress between the coating and the substrate can be reduced, thereby improving its bonding strength. After being placed in the material of the film layer and soaked, not only a dense film layer is formed on the surface of the aluminum alloy matrix, but also the molecular sieve crystals have a certain orientation, and the crystals grow cross-linked, which slows down the corrosion of the aluminum alloy matrix to a greater extent, and obtains an aluminum alloy with beautiful surface appearance and significant corrosion resistance. DETAILED DESCRIPTION
[0021] In order to make the purpose, technical solution and advantages of the present invention more clearly understood, the present invention is further described in detail below in conjunction with its embodiments. It should be understood that the specific implementation methods described herein are only used to explain the present invention and do not limit the protection scope of the present invention.
[0022] Unless otherwise defined, all technical and scientific terms used herein have the same meaning as those commonly understood by those skilled in the art of the present invention. The terms used herein in the specification of the present invention are only for the purpose of describing specific embodiments and are not intended to limit the present invention. The term "and / or" used herein includes any and all combinations of one or more related listed items.
[0023] A corrosion-resistant aluminum alloy in one embodiment of the present invention includes an aluminum alloy substrate and a film layer supported on the surface of the aluminum alloy substrate, wherein the aluminum alloy substrate includes the following components in percentage by mass:
[0024] Mg 0.6%~0.8%, Si 0.1%~0.2%, Mn 0.01%~0.2%, Cu 0.01%~0.07%, Zn0.1%~0.5%, Ti 0.01%~0.02%, Sr 0.01%~0.03%, corrosion-resistant particles 0.01%~0.09%, the balance is Al and unavoidable impurities;
[0025] The material of the film layer includes the following preparation steps:
[0026] Tetrapropylammonium hydroxide, tetraethyl orthosilicate, sodium hydroxide, anhydrous ethanol and deionized water are mixed in a molar ratio of (5-7):(18-23):(500-550):(0.1-0.5):100, stirred at a stirring speed of 50r / min-150r / min and a temperature of 120°C-150°C for 5h-8h, then aged and washed, and then added to deionized water and dispersed evenly to obtain a film layer material with a mass fraction of 5%.
[0027] In one embodiment, the aging treatment time is 10h to 15h.
[0028] In one embodiment, the corrosion-resistant particles are obtained by ball-milling a mixture of chromium powder and nickel powder in a mass ratio of (1-7):(1-5).
[0029] In addition, the present invention also provides a method for preparing a corrosion-resistant aluminum alloy, the preparation method comprising the following steps:
[0030] Al-Mg alloy, Al-Si alloy, Al-Mn alloy, Al-Cu alloy, Al-Zn alloy, titanium ingot and Al-Sr alloy are added to a smelting furnace for smelting treatment, the obtained aluminum liquid is added to a holding furnace for refining, and then slag is removed, and then degassed through a filter box, and cast through a crystallizer to obtain an ingot;
[0031] Plasma spraying the corrosion-resistant particles on the surface of the ingot to obtain an aluminum alloy matrix;
[0032] The aluminum alloy substrate is subjected to a heating treatment, air-cooled to room temperature, and then placed in the material of the film layer. After being immersed, washed, and dried, a corrosion-resistant aluminum alloy is obtained.
[0033] In one of the embodiments, the casting temperature is 720° C. to 740° C., the casting speed is 45 mm / min to 55 mm / min, and the casting cooling water flow rate is 200 L / min to 230 L / min.
[0034] In one embodiment, the plasma spraying process has a spraying voltage of 65V to 70V, a spraying distance of 25mm to 35mm, a rotation rate of 120rpm to 130rpm, a powder feeding rate of 120g / min to 180g / min, and a spraying angle of 45°.
[0035] In one embodiment, the particle size of the corrosion-resistant particles is 25 μm to 30 μm.
[0036] In one embodiment, the heating treatment is as follows: the aluminum alloy substrate is heated to 90°C to 100°C at a rate of 1°C / min to 3°C / min, kept warm for 3h to 5h, then heated to 120°C to 180°C, kept warm for 1h to 5h, then cooled to 90°C to 100°C at a rate of 1°C / min to 3°C / min, kept warm for 3h to 5h, then heated to 180°C to 250°C again, kept warm for 3h to 5h, then cooled to 100°C to 120°C, kept warm for 1h to 2h
[0037] In one embodiment, the immersion treatment is carried out at a temperature of 100° C. to 120° C. and for a time of 2 h to 5 h.
[0038] In one embodiment, the drying process is carried out at a temperature of 95°C to 105°C and for a time of 30 min to 50 min.
[0039] The present application optimizes the chemical composition and component ratio of the aluminum alloy so that no β phase appears in the aluminum alloy matrix, fewer defects in the crystal, and the prepared aluminum alloy has significant corrosion resistance.
[0040] The embodiments of the present invention will be described in detail below with reference to specific examples.
[0041] Embodiment 1~3:
[0042] The difference between Examples 1 to 3 is that the composition and proportion of the aluminum alloy matrix are different, as shown in Table 1;
[0043] A method for preparing a corrosion-resistant aluminum alloy comprises the following steps:
[0044] Tetrapropylammonium hydroxide, ethyl orthosilicate, sodium hydroxide, anhydrous ethanol and deionized water in a molar ratio of 7:20:500:0.5:100 were mixed, stirred at a stirring speed of 50 r / min and a temperature of 120° C. for 8 hours, then aged for 10 hours, washed, and then added to deionized water and dispersed evenly to obtain a film material with a mass fraction of 5%;
[0045] Adding Al-Mg alloy, Al-Si alloy, Al-Mn alloy, Al-Cu alloy, Al-Zn alloy, titanium ingot and Al-Sr alloy into a smelting furnace for smelting treatment, adding the obtained aluminum liquid into a holding furnace for refining, then slagging treatment, and then degassing through a filter box, and casting through a crystallizer, the casting temperature is 720° C., the casting speed is 45 mm / min, the casting cooling water flow rate is 200 L / min, and an ingot is obtained;
[0046] Plasma spraying is performed on the surface of the ingot by using corrosion-resistant particles, and the spraying voltage of the plasma spraying process is 65V, the spraying distance is 25mm, the rotation rate is 120rpm, the powder feeding rate is 120g / min, and the spraying angle is 45°, to obtain an aluminum alloy matrix;
[0047] The aluminum alloy substrate is subjected to a heat treatment, and the heat treatment is as follows: the aluminum alloy substrate is heated to 95°C at a rate of 3°C / min, kept warm for 3 hours, continued to be heated to 120°C, kept warm for 3 hours, then cooled to 90°C at a rate of 1°C / min, kept warm for 3 hours, heated to 250°C again, kept warm for 3 hours, then cooled to 100°C, kept warm for 1 hour, cooled to room temperature and placed in the material of the film layer, immersed at 100°C for 3 hours, washed, and dried at 95°C for 50 minutes to obtain a corrosion-resistant aluminum alloy.
[0048] Embodiment 4:
[0049] The difference between Example 4 and Example 3 is that the preparation method of the membrane layer material in Example 4 is as follows, and the rest is the same as Example 3.
[0050] Tetrapropylammonium hydroxide, ethyl orthosilicate, sodium hydroxide, anhydrous ethanol and deionized water in a molar ratio of 7:21:500:0.4:100 are mixed, stirred at a stirring speed of 50 r / min and a temperature of 125°C for 7 hours, then aged for 12 hours, washed, added to deionized water, and evenly dispersed to obtain a film layer material with a mass fraction of 5%.
[0051] Comparative Examples 1 to 4:
[0052] The difference between Comparative Examples 1 to 4 and Example 3 is that the composition and component ratio of the aluminum alloy matrix are different, as shown in Table 1, and the rest are the same as Example 3.
[0053] Comparative Example 5:
[0054] The difference between Comparative Example 5 and Example 3 is that the preparation method of the aluminum alloy sample in Comparative Example 5 includes the following steps:
[0055] Tetrapropylammonium hydroxide, ethyl orthosilicate, sodium hydroxide, anhydrous ethanol and deionized water in a molar ratio of 7:20:500:0.5:100 were mixed, stirred at a stirring speed of 50 r / min and a temperature of 120° C. for 8 hours, then aged for 10 hours, washed, and then added to deionized water and dispersed evenly to obtain a film material with a mass fraction of 5%;
[0056] Adding Al-Mg alloy, Al-Si alloy, Al-Mn alloy, Al-Cu alloy, Al-Zn alloy, titanium ingot and Al-Sr alloy into a smelting furnace for smelting treatment, adding the obtained aluminum liquid into a holding furnace for refining, then slagging treatment, and then degassing through a filter box, and casting through a crystallizer, the casting temperature is 720° C., the casting speed is 45 mm / min, the casting cooling water flow rate is 200 L / min, and an ingot is obtained;
[0057] Plasma spraying is performed on the surface of the ingot by using corrosion-resistant particles, and the spraying voltage of the plasma spraying process is 65V, the spraying distance is 25mm, the rotation rate is 120rpm, the powder feeding rate is 120g / min, and the spraying angle is 45°, to obtain an aluminum alloy matrix;
[0058] The aluminum alloy substrate is subjected to a heat treatment, and the heat treatment is as follows: the aluminum alloy substrate is heated to 95°C at a rate of 3°C / min, kept warm for 3 hours, continued to be heated to 120°C, kept warm for 3 hours, then cooled to 90°C at a rate of 1°C / min, kept warm for 3 hours, heated to 250°C again, kept warm for 3 hours, then cooled to 100°C, kept warm for 1 hour, and cooled to room temperature to obtain an aluminum alloy.
[0059] Comparative Example 6:
[0060] The difference between Comparative Example 6 and Example 3 is that Comparative Example 6 is not subjected to heat treatment, and the rest is the same as Example 3.
[0061] Comparative Example 7:
[0062] The difference between Comparative Example 7 and Example 3 is that the heating treatment in Comparative Example 7 is: heating the aluminum alloy substrate to 200° C. at a rate of 10° C. / min and keeping the temperature for 3 hours. The other steps are the same as those in Example 3.
[0063] Table 1: Chemical composition (%)
[0064]
[0065] The samples obtained in Examples 1 to 4 and the comparative samples obtained in Comparative Examples 1 to 7 were subjected to performance analysis, and the results are shown in Table 2. Among them, the mechanical properties testing standard: GB / T228 Room temperature tensile test method for metal materials. Corrosion test standard: GB / T15970.7-2000 Corrosion stress corrosion test for metals and alloys Part 7: Slow strain rate test.
[0066] Table 2: Performance analysis results
[0067]
[0068] From the data analysis of Table 2, it can be seen that after optimizing the composition and the ratio of components, the present application can obtain an aluminum alloy with remarkable mechanical properties and corrosion resistance, and after combining with process optimization, it can obtain a tensile strength of more than 720MPa, a yield strength of more than 680MPa, a growth rate of more than 11%, and at the same time, significant corrosion resistance, which has a wider range of use value.
[0069] The technical features of the above-described embodiments may be arbitrarily combined. To make the description concise, not all possible combinations of the technical features in the above-described embodiments are described. However, as long as there is no contradiction in the combination of these technical features, they should be considered to be within the scope of this specification.
[0070] The above-mentioned embodiments only express several implementation methods of the present invention, and the descriptions thereof are relatively specific and detailed, but they cannot be understood as limiting the scope of the invention patent. It should be pointed out that, for ordinary technicians in this field, several variations and improvements can be made without departing from the concept of the present invention, and these all belong to the protection scope of the present invention. Therefore, the protection scope of the patent of the present invention shall be subject to the attached claims.
Claims
1. A corrosion-resistant aluminum alloy, characterized in that: The corrosion-resistant aluminum alloy comprises an aluminum alloy substrate and a film layer supported on the surface of the aluminum alloy substrate, wherein the aluminum alloy substrate comprises the following components in percentage by mass: Mg 0.6%~0.8%, Si 0.1%~0.2%, Mn 0.01%~0.2%, Cu 0.01%~0.07%, Zn0.1%~0.5%, Ti 0.01%~0.02%, Sr 0.01%~0.03%, corrosion-resistant particles 0.01%~0.09%, the balance is Al and unavoidable impurities; The material of the film layer includes the following preparation steps: Tetrapropylammonium hydroxide, tetraethyl orthosilicate, sodium hydroxide, anhydrous ethanol and deionized water are mixed in a molar ratio of (5-7):(18-23):(500-550):(0.1-0.5):100, stirred at a stirring speed of 50r / min-150r / min and a temperature of 120°C-150°C for 5h-8h, then aged and washed, and then added to deionized water and dispersed evenly to obtain a film layer material with a mass fraction of 5%.
2. The corrosion-resistant aluminum alloy according to claim 1, characterized in that: The aging treatment time is 10h to 15h.
3. The corrosion-resistant aluminum alloy according to claim 2, characterized in that: The corrosion-resistant particles are obtained by ball-milling chromium powder and nickel powder in a mass ratio of (1-7):(1-5).
4. A method for preparing a corrosion-resistant aluminum alloy, characterized in that: The preparation method is used to prepare the corrosion-resistant aluminum alloy according to any one of claims 1 to 3, and the preparation method comprises the following steps: Al-Mg alloy, Al-Si alloy, Al-Mn alloy, Al-Cu alloy, Al-Zn alloy, titanium ingot and Al-Sr alloy are added to a smelting furnace for smelting treatment, the obtained aluminum liquid is added to a holding furnace for refining, and then slag is removed, and then degassed through a filter box, and cast through a crystallizer to obtain an ingot; Plasma spraying the corrosion-resistant particles on the surface of the ingot to obtain an aluminum alloy matrix; The aluminum alloy substrate is subjected to a heating treatment, air-cooled to room temperature, and then placed in the material of the film layer. After being immersed, washed, and dried, a corrosion-resistant aluminum alloy is obtained.
5. The preparation method according to claim 4, characterized in that: The casting temperature is 720° C. to 740° C., the casting speed is 45 mm / min to 55 mm / min, and the casting cooling water flow rate is 200 L / min to 230 L / min.
6. The preparation method according to claim 4, characterized in that: The plasma spraying process has a spraying voltage of 65V to 70V, a spraying distance of 25mm to 35mm, a rotation rate of 120rpm to 130rpm, a powder feeding rate of 120g / min to 180g / min, and a spraying angle of 45°.
7. The preparation method according to claim 4, characterized in that: The particle size of the corrosion-resistant particles is 25 μm to 30 μm.
8. The preparation method according to claim 4, characterized in that: The heating treatment is as follows: heating the aluminum alloy substrate to 90°C-100°C at a rate of 1°C / min-3°C / min, keeping the temperature for 3h-5h, continuing to heat the aluminum alloy substrate to 120°C-180°C, keeping the temperature for 1h-5h, then cooling the aluminum alloy substrate to 90°C-100°C at a rate of 1°C / min-3°C / min, keeping the temperature for 3h-5h, heating the aluminum alloy substrate to 180°C-250°C again, keeping the temperature for 3h-5h, and then cooling the aluminum alloy substrate to 100°C-120°C.
9. The preparation method according to claim 4, characterized in that: The immersion treatment is carried out at a temperature of 100° C. to 120° C. and for a time of 2 h to 5 h.
10. The preparation method according to claim 4, characterized in that: The drying process is carried out at a temperature of 95° C. to 105° C. and for a time of 30 min to 50 min.