Novel light alloy component formula and preparation process
Through the composition and preparation process of Al15Mg40Li35Si5Zn5 alloy, the problems of brittleness and low toughness of multi-component lightweight alloys at room temperature are solved, and a lightweight alloy with high strength and excellent compression plasticity is achieved, with low density and excellent yield strength-compression plasticity. balance.
Patent Information
- Application Number
- CN202410807772.X
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Filing Date
- 2024-06-21
- Publication Date
- 2024-10-01
AI Technical Summary
Existing multi-component lightweight alloys exhibit brittleness and low toughness at room temperature, and their preparation is difficult due to uneven volatilization and precipitation among elements.
Using the composition formula of Al15Mg40Li35Si5Zn5 alloy, it is prepared through a smelting process under the protection of argon gas to form a BCC+HCP phase with a solid solution phase volume fraction of close to 60%. The phase size distribution is uniform and the problem of splitting and cracking of the matrix caused by intermetallic compounds is improved.
A lightweight alloy with high yield strength of 410MPa, compressive strength of 546MPa and compression plasticity of 15.3% has been achieved, improving the strength and plasticity properties of the alloy.
Smart Images

Figure CN118726818A_ABST
Abstract
Description
Technical Field
[0001] The invention relates to the technical field of alloy preparation, and in particular to a novel light alloy component formula and preparation process. Background Art
[0002] Metal materials have been widely used in all walks of life as engineering structural materials. However, with the development of science and technology, the requirements for metal materials have also increased, requiring better working performance, higher reliability and low cost. The idea of traditional alloys based on a single main element and micro-alloying limits the possibility of alloy performance development. Multi-component alloys can break through the alloying limitations of traditional alloys, thereby obtaining excellent properties that traditional materials cannot match, such as high strength, high hardness, high wear resistance, good corrosion resistance, high temperature oxidation resistance, high temperature softening resistance, etc.
[0003] The multi-component lightweight alloys reported at this stage still have some problems. Although these alloys show low density (2.2 g cm -3 -6.2 g cm -3 ), high hardness (up to 911HV), high specific hardness, high temperature strength, oxidation resistance and high temperature stability, but this type of alloy does not show good plasticity at room temperature. Most of them show outstanding brittleness and have extremely low toughness. In addition, since the saturated vapor pressure of most light elements is very different from that of heavier elements, it may lead to uneven volatilization and precipitation between alloy elements, so the preparation of multi-component light alloys will be limited. In order to solve these problems, it is necessary to develop a new system of multi-component light high entropy alloys. Summary of the invention
[0004] The purpose of the present invention is to provide a new light alloy composition formula and preparation process to solve the above-mentioned problems in the background technology. 15 Mg 40 Li 35 The volume fraction of the solid solution phase in Si5Zn5 alloy is close to 60% (BCC+HCP), and the size distribution of each phase is relatively uniform, which effectively improves the splitting of the matrix by the intermetallic compound and alleviates the generation of cracks. 15 Mg 40 Li 35 Si5Zn5 alloy has excellent compression plasticity. The present invention provides a composition formula and preparation process of a novel lightweight Al-Mg-Li-Si-Zn multi-component alloy with excellent performance. It has been measured that the yield strength of the product of the present invention can reach 410MPa, the compressive strength can reach 546MPa, and the compression plasticity can reach 15.3%.
[0005] To achieve the above object, the present invention provides the following technical solutions:
[0006] One of the technical solutions of the present invention is to provide a lightweight Al-Mg-Li-Si-Zn multi-component alloy, which comprises the following chemical components in atomic percentage:
[0007] Al 15-16%, Mg 40-41%, Li 34-35%, Si 4-5% and Zn 4-5%.
[0008] Preferably, the chemical composition of the alloy is, by atomic percentage:
[0009] Al 15%, Mg 40%, Li 35%, Si 5% and Zn 5%.
[0010] The second technical solution of the present invention is to provide a method for preparing the above-mentioned lightweight Al-Mg-Li-Si-Zn multi-component alloy, comprising the following steps:
[0011] The chemical components are mixed and smelted to obtain the lightweight Al-Mg-Li-Si-Zn multi-component alloy.
[0012] Preferably, the smelting atmosphere is a protective atmosphere.
[0013] More preferably, the protective atmosphere is an argon atmosphere.
[0014] Preferably, the smelting is carried out in a vacuum induction melting furnace.
[0015] The beneficial technical effects of the present invention are as follows:
[0016] The high strength of the alloy prepared by the present invention mainly comes from the strengthening effect of a large number of high-hardness, high-modulus intermetallic compounds in the alloy. The presence of high-hardness, high-modulus intermetallic compounds will lead to a large number of strain fields in the alloy caused by the mismatch between hardness and modulus, which will seriously hinder the movement of dislocations, thereby causing dislocation pile-up, so that the alloy has higher strength. The modulus difference between the hard phase and the matrix in the product of the present invention is large, so this effect can be enhanced, and the strength of the product can be greatly improved. In terms of alloy compression plasticity, the Al 15 Mg 40 Li 35 The volume fraction of the solid solution phase in Si5Zn5 alloy is close to 60% (BCC+HCP), and the size distribution of each phase is relatively uniform, which effectively improves the splitting of the matrix by the intermetallic compound and alleviates the generation of cracks. 15 Mg 40 Li 35 Si5Zn5 alloy has excellent compression plasticity.
[0017] The present invention provides a novel light Al-Mg-Li-Si-Zn multi-component alloy with excellent performance, a component formula and a preparation process. According to the test, the yield strength of the product of the present invention can reach 410MPa, the compressive strength can reach 546MPa, and the compression plasticity can reach 15.3%.
[0018] The present invention aims to improve the existing light multi-component alloys with high density and low room temperature plasticity. The present invention uses Mg, Al, Li, Si and Zn elements to control the composition and test the mechanical properties of the light multi-component alloy of the present invention, and finally obtains a new Al-Mg-Li-Si-Zn multi-component alloy with low density and excellent yield strength-compression plasticity balance, which is of great significance to the development of multi-component light alloys. BRIEF DESCRIPTION OF THE DRAWINGS
[0019] In order to more clearly illustrate the embodiments of the present invention or the technical solutions in the prior art, the drawings required for use in the embodiments will be briefly introduced below. Obviously, the drawings described below are only some embodiments of the present invention. For ordinary technicians in this field, other drawings can be obtained based on these drawings without paying creative work.
[0020] Figure 1 Schematic diagram of smelting and macroscopic image of the product of Example 1.
[0021] Figure 2 It is a comparison chart of the compression curves of the products of Example 1, Comparative Examples 1-2 and pure Mg.
[0022] Figure 3 is Al in Example 1 15 Mg 40 Li 35 X-ray diffraction pattern of Si5Zn5.
[0023] Figure 4 is Al in Example 1 15 Mg 40 Li 35 Microstructure and element distribution diagram of Si5Zn5. (a) and (b) are microstructure diagrams at different magnifications, and (c)-(f) are element distribution diagrams of different elements.
[0024] Figure 5 is Al in Example 1 15 Mg 40 Li 35 Load-displacement curve and modulus and hardness distribution diagram of Si5Zn5. (a) is the load-displacement curve diagram, and (b) is the modulus and hardness distribution diagram. DETAILED DESCRIPTION
[0025] Now, various exemplary embodiments of the present invention are described in detail, and this detailed description should not be considered as a limitation of the present invention, but should be understood as a more detailed description of certain aspects, characteristics and embodiments of the present invention. It should be understood that the terms described in the present invention are only for describing specific embodiments and are not used to limit the present invention.
[0026] In addition, for the numerical range in the present invention, it is understood that each intermediate value between the upper and lower limits of the range is also specifically disclosed. The intermediate value in any stated value or stated range, and each smaller range between any other stated value or intermediate value in the range is also included in the present invention. The upper and lower limits of these smaller ranges can be independently included or excluded in the scope.
[0027] Unless otherwise specified, all technical and scientific terms used herein have the same meaning as commonly understood by those skilled in the art to which the invention pertains. Although only preferred methods and materials are described herein, any methods and materials similar or equivalent to those described herein may also be used in the practice or testing of the present invention.
[0028] The words “include,” “including,” “have,” “contain,” etc. used in the present invention are open-ended terms, meaning including but not limited to.
[0029] All raw materials used in the following examples and comparative examples of the present invention are commercially available products.
[0030] Example 1
[0031] The chemical composition ratios of the lightweight Al-Mg-Li-Si-Zn multi-component alloy are shown in Table 1.
[0032] Table 1
[0033] chemical composition Atomic percentage (%) Mass percentage (%) Al 15 19.39 Mg 40 46.58 Li 35 11.64 Si 5 6.73 Zn 5 15.66
[0034] Preparation of lightweight Al-Mg-Li-Si-Zn multi-component alloy:
[0035] (1) Select the above chemical raw materials with a purity of 99.95%, clean the impurities such as oxides on the surface of the raw materials, then use acetone ultrasonic cleaning, and use a hair dryer to dry. According to the above ratio, use a balance with an accuracy of (0.001) to weigh each raw material.
[0036] (2) Place the prepared raw materials in a graphite crucible mold and cover it with a graphite cover to prevent the pure lithium raw materials from being contaminated and to avoid contamination caused by the volatilization of the raw materials during the smelting process. After placing them in place, place them in the coil of a vacuum induction melting furnace, evacuate to below 0.005Pa, and then fill the furnace cavity with argon to flush. After flushing three times, turn on the power under the protection of argon and heat the raw materials through the induction coil to initially melt the raw materials. After the alloy rod and the mold have cooled, take out the graphite mold, reverse the smelted alloy rod in each hole in the graphite mold, and then melt it repeatedly for at least 4 times; then take it out to prepare a lightweight Al-Mg-Li-Si-Zn multi-component alloy round rod with a diameter of 10 mm (such as Figure 1 ), and then wire cutting (as shown in the cast sample in Figure 1 The compressed sample in the figure shows a light Al-Mg-Li-Si-Zn multi-component alloy (denoted as Al 15 Mg 40 Li 35 Si5Zn5, where the numbers represent the atomic percentage of each element).
[0037] The theoretical density of the alloy is calculated using the mixing method. After calculation, the theoretical density of this alloy is 1.64g / cm 3 .
[0038] Figure 1 Schematic diagram of smelting and macroscopic image of the product of Example 1.
[0039] Comparative Example 1
[0040] Preparation of AlLiMgSnZn:
[0041] The only difference from Example 1 is that, in terms of atomic percentage, the chemical composition of the multi-component alloy is as follows:
[0042] Al 20%, Li 20%, Mg 20%, Sn. 20% and Zn. 20%.
[0043] After calculation, the theoretical density of this alloy is 4.23g / cm 3 .
[0044] Comparative Example 2
[0045] Mg 33 (MnAlZnCu) 67 Preparation:
[0046] The only difference from Example 1 is that, in terms of atomic percentage, the chemical composition of the multi-component alloy is as follows:
[0047] Mg 33%, Mn 16.75%, Al 16.75%, Zn 16.75% and Cu 16.75%.
[0048] After calculation, the theoretical density of this alloy is 6.13g / cm 3 .
[0049] Effect verification
[0050] (1) Al of Example 1 15 Mg 40 Li 35 Si5Zn5 compression test:
[0051] The compression test was completed on an MTS-CMT5205 universal mechanical testing machine with a strain rate of 10 -4 s -1 The compression sample is a round rod sample with a diameter of 6 mm and a height of 12 mm. It was measured that the yield strength of the product of Example 1 is 410 MPa and the compressive strength is 546 MPa; the yield strength of the product of Comparative Example 1 is 600 MPa and the compressive strength is 615 MPa; the yield strength of the product of Comparative Example 2 is 437 MPa and the compressive strength is 437 MPa. The compression curve is as follows Figure 2 shown.
[0052] Figure 2 It is a comparison chart of the compression curves of the products of Example 1, Comparative Examples 1-2 and pure Mg.
[0053] As can be seen from the figure, the product of Example 1 of the present invention also has a compression plasticity of 15.3%, which is much higher than 1.2% of Comparative Example 1 and 3.41% of Comparative Example 2, and has relatively good compression deformation ability.
[0054] Although the strength of Comparative Examples 1 and 2 is slightly higher than that of the embodiment, the two comparative examples have almost no plasticity and are brittle; while the strength of Example 1 is slightly lower, the plasticity is far superior to that of Comparative Examples 1 and 2. Based on this, the specific yield strength (specific yield strength = yield strength / density) of the products of Example 1 and Comparative Examples 1-2 is calculated; it is measured that the specific yield strength of Example 1 is 250 MPa cm 3 / g, Comparative Example 1 is 141.85MPa cm 3 / g; Comparative Example 2 is 71.29MPacm 3 / g.
[0055] (2) Al of Example 1 15 Mg 40 Li 35 The crystal structure of Si5Zn5 is characterized:
[0056] The alloy crystal structure was characterized by X-ray diffraction using a D\max-2550 X-ray diffractometer with a scanning angle of 10-90°, a scanning speed of 8° / min, a step length of 0.02°, a current of 40mA, and a voltage of 40kV. The test results are as follows Figure 3 shown.
[0057] Figure 3 is Al in Example 1 15 Mg 40 Li 35 X-ray diffraction spectrum of Si5Zn5. The horizontal axis is the 2q angle (°); the vertical axis is the normalized intensity.
[0058] Figure 3 The phase composition of this lightweight multi-component alloy includes a body-centered cubic phase (BCC), a close-packed hexagonal phase (HCP), Mg2Si, Al5Mg 11 Zn4 and Zn 5.28 Li 3.74 .exist Figure 3 In the figure, spades are diffraction peaks corresponding to the BCC phase. Squares are diffraction peaks corresponding to the HCP phase, plum blossoms are diffraction peaks of LiAl or Mg2Si, and hearts are diffraction peaks of Al5Mg 11 Zn4 intermetallic compound, the dots are Zn 5.28 Li 3.74 Intermetallic compounds. As can be seen from the figure, the phase with the largest volume fraction is the BCC phase. Since the diffraction peaks of AlLi and Mg2Si are very close, they cannot be distinguished. In general, the BCC and HCP phases in this alloy only account for about 60% of the phase volume fraction, and the intermetallic compounds still have a large volume fraction.
[0059] (3) Al of Example 1 15 Mg 40 Li 35 Characterization of the microstructure of Si5Zn5:
[0060] The backscattering mode of the field emission scanning electron microscope and the matching EDS Oxford spectrometer were used to observe the microstructure morphology of the alloy and analyze the composition of different phases. Figure 4 shown.
[0061] Figure 4 is Al in Example 1 15 Mg 40 Li 35 Microstructure and element distribution diagram of Si5Zn5. (a) and (b) are microstructure diagrams at different magnifications, and (c)-(f) are element distribution diagrams of different elements.
[0062] Figure 4This reflects the Al content of Example 1 in the backscattering mode. 15 Mg 40 Li 35 Microstructure and elemental analysis of Si5Zn5. Figure 4 As can be seen in (a), there are at least four materials with different contrasts, including dark gray block material (represented by "A"), dark gray granular material (represented by "B"), gray block material (represented by "C") and bright white mesh material (represented by "D"). In order to explore the phases to which these four materials belong, the composition of these four materials was analyzed respectively. The results of the Oxford spectrometer test show that the composition of the area corresponding to "A" is: Al 69.4%, Mg 15.7%, Si 9.8% and Zn 5.1% (all atomic ratios); the Mg content of the area corresponding to "B" is 93.8%, and the Zn content is about 6.2% (atomic ratio); the composition of the area corresponding to "C" is Mg 57.5% and Si42.5% (atomic ratio); the composition test results of the area "D" are Al 17.5%, Mg 74.4% and Zn8.1%. Combined with the phase calibration results of XRD, this alloy contains BCC, HCP, LiAl / Mg2Si, Al5Mg 11 Zn4 and Zn 5.28 Li 3.74 Therefore, it can be determined that the phase represented by "C" is Mg2Si / MgSi phase, and the phase represented by "D" is Al5Mg 11 Zn4. It is difficult to distinguish what "A" and "B" represent.
[0063] Figure 4(b) is a backscattered image of the alloy at a high magnification, and (c), (d), (e) and (f) are element distribution maps of the corresponding surface scans. (c) is the surface distribution of the Al element. It can be found from the figure that the Al element is distributed almost throughout the entire surface scan area. The phase corresponding to the Al element enrichment is consistent with the red circle marker in (b), that is, "A" in (a). Al is the main component element in this phase. Combined with the XRD results, Li cannot be detected. Therefore, this phase "A" can be determined to be LiAl phase. (d) reflects the distribution of the Mg element. The Mg element enrichment area is relatively continuous and it is not easy to distinguish the specific phase. (e) reflects the distribution of the Si element. There are also some enriched areas of the Si element. For example, there is corresponding Si element enrichment in the area marked by the pink circle in (b). Comparing the same position in (d), it is found that the Mg element is also enriched in this area. Therefore, it can be determined that this area is the same phase as "C" (MgSi / Mg2Si) in (a). Except for the MgSi / Mg2Si phase, Si is distributed evenly. (f) is the Zn element distribution diagram, and there is also an obvious enrichment area of Zn element, among which the typical area is the area marked by the light blue circle in (b). This area contains not only Zn, but also Mg and Al. It can be seen that the phase corresponding to this enrichment area is Al5Mg 11 Zn4.
[0064] (4) Perform indentation test:
[0065] According to the results of mechanical properties test, Al 15 Mg 40 Li 35 The high strength and high specific strength (yield strength / density) of Si5Zn5 alloy are superior to other comparative examples. There are many factors that affect the strength of alloys, including alloy composition, lattice type, grain size and substructure contained, solute element size in solid solution, and the nature of the strengthening phase in multiphase structure. The alloy designed by the present invention has the obvious feature of complex multiphase structure. Compared with other factors, the influence of alloy phase composition on the mechanical properties of alloy is particularly obvious. According to Al 15 Mg 40 Li 35 The phase composition analysis of Si5Zn5 alloy shows that the phase composition of this alloy is relatively complex. 15 Mg 40 Li 35 In Si5Zn5 alloy, the six different phases are BCC solid solution phase, HCP phase, LiAl, MgSi / Mg2Si, Al5Mg 11 Zn4 and Zn 5.28 Li 3.74Phases, the volume fraction of these phases in the alloy, their distribution in the alloy, the shape and size of the phases, the hardness and modulus of the phases all have different degrees of influence on the mechanical properties of the alloy.
[0066] In order to explore the properties of specific phases in the alloy, the nanoindentation method is used to perform indentation tests on phases with greater differentiation, such as Figure 5 shown.
[0067] Figure 5 is Al in Example 1 15 Mg 40 Li 35 Load-displacement curve and modulus and hardness distribution diagram of Si5Zn5. (a) is the load-displacement curve diagram, and (b) is the modulus and hardness distribution diagram.
[0068] Alloy Al 15 Mg 40 Li 35 The matrix of Si5Zn5 is composed of BCC+HCP solid solution. According to nanoindentation test, the modulus of the matrix ranges from 30-50GPa and the hardness is about 1GPa. The modulus and hardness of LiAl intermetallic compound are slightly higher than that of the matrix, with a modulus of 50-60GPa and a hardness of about 1.5GPa. The modulus of Mg2Si phase is similar to that of LiAl phase, but the hardness is slightly higher (about 2GPa). Among them, Al5Mg has the larger hardness and modulus. 11 Zn4, modulus about 70GPa, hardness about 2.5GPa. From the nanoindentation test results, it can be seen that the typical feature of this alloy is a low hardness, low modulus matrix containing a large amount of high modulus, high hardness intermetallic compounds.
[0069] Therefore, the high strength of the alloy prepared by the present invention mainly comes from the strengthening effect of a large amount of high hardness and high modulus intermetallic compounds in the alloy. The presence of high hardness and high modulus intermetallic compounds will lead to a large amount of strain fields in the alloy caused by the mismatch between hardness and modulus, which will seriously hinder the movement of dislocations, thereby causing dislocation pile-up, so that the alloy has higher strength. The greater the difference in modulus between the hard phase and the matrix, the more significant this effect is. In terms of alloy compression plasticity, the plastic deformation ability of the soft solid solution phase is stronger than that of the hard intermetallic compound. When the volume fraction of the solid solution phase in the alloy is larger, the corresponding plastic deformation ability is better. Al 15 Mg 40 Li 35 The volume fraction of the solid solution phase in Si5Zn5 alloy is close to 60% (BCC+HCP), and the size distribution of each phase is relatively uniform, which effectively improves the splitting of the matrix by the intermetallic compound and alleviates the generation of cracks. 15 Mg 40 Li35 Si5Zn5 alloy has excellent compression plasticity.
[0070] The present invention aims to improve the existing light multi-component alloys with high density and low room temperature plasticity. The present invention uses Mg, Al, Li, Si and Zn elements to control the composition and test the mechanical properties of the light multi-component alloy of the present invention, and finally obtains a new Al-Mg-Li-Si-Zn multi-component alloy with low density and excellent yield strength-compression plasticity balance, which is of great significance to the development of multi-component light alloys.
[0071] The embodiments described above are only descriptions of the preferred modes of the present invention, and are not intended to limit the scope of the present invention. Without departing from the design spirit of the present invention, various modifications and improvements made to the technical solutions of the present invention by ordinary technicians in this field should all fall within the protection scope determined by the claims of the present invention.
Claims
1. A lightweight Al-Mg-Li-Si-Zn multi-component alloy, characterized in that: In terms of atomic percentage, it includes the following chemical components: Al 15-16%, Mg 40-41%, Li 34-35%, Si 4-5% and Zn 4-5%.
2. The lightweight Al-Mg-Li-Si-Zn multi-component alloy according to claim 1, characterized in that: The chemical composition of the alloy is, in atomic percentage,: Al 15%, Mg 40%, Li 35%, Si 5% and Zn 5%.
3. A method for preparing the lightweight Al-Mg-Li-Si-Zn multi-component alloy according to claim 1 or 2, characterized in that: The following steps are involved: The chemical components are mixed and smelted to obtain the lightweight Al-Mg-Li-Si-Zn multi-component alloy.
4. The preparation method according to claim 3, characterized in that: The smelting atmosphere is a protective atmosphere.
5. The preparation method according to claim 4, characterized in that: The protective atmosphere is argon atmosphere.
6. The preparation method according to claim 3, characterized in that: The smelting is carried out in a vacuum induction melting furnace.