Nickel alloy and treatment method thereof
Through double-pass hot compression treatment and water quenching treatment, the problems of high deformation resistance and complex microstructure transformation of GH99 nickel alloy during hot processing are solved, the deformation resistance and grain size distribution of the nickel alloy are improved, and the degree of dynamic softening is improved. , simplifying the processing process.
Patent Information
- Application Number
- CN202410835956.7
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Filing Date
- 2024-06-26
- Publication Date
- 2024-10-01
- Estimated Expiration
- Not applicable · inactive patent
AI Technical Summary
GH99 nickel alloy has high deformation resistance and complex microstructural transformation during hot processing, which makes processing difficult. The precipitation and dissolution of coherent precipitates and secondary carbides play an important role in the safety of the hot processing process.
A double-pass thermal compression treatment method is adopted. The deformation conditions of the first and second passes of compression are 1100-1150°C and 1050-1100°C respectively, and the strain rate is 0.001-0.005s-1, combined with water quenching treatment. , improve the deformation resistance and grain size distribution of nickel alloys.
It improves the deformation resistance and grain size distribution uniformity of nickel alloys, improves the degree of dynamic softening, and reduces processing difficulty.
Smart Images

Figure CN118726873A_ABST
Abstract
Description
Technical Field
[0001] The present invention relates to the field of alloys, and in particular, to nickel alloys and methods for processing the same. Background Art
[0002] Nickel alloys, especially nickel-based high-temperature alloys, are metal materials that can withstand complex stresses at high temperatures of 600 to 1000°C and have good comprehensive properties such as high-temperature oxidation resistance and corrosion resistance. Therefore, they are widely used in high-precision and cutting-edge equipment manufacturing fields such as aircraft engines, gas turbines, and launch vehicles, with a utilization rate of more than 60%. GH99 alloy is a new type of nickel high-temperature alloy with a controllable solid solution and Ni3 (Ti, Al, Nb) type γ′ strengthening phase designed on the basis of Russian ЭП742 alloy by increasing the proportion of γ′ phase-forming elements (Al, Ti, Nb, Mo) to more than 8.5%, and scientifically and rationally balancing the content of other elements. The operating temperature of GH99 alloy can be increased to 750°C, and the γ′ phase content exceeds 50%, with excellent performance. However, during hot working, dislocation movement needs to overcome the obstruction of a large amount of high-temperature γ′ phase, so the deformation resistance is large, which makes the hot working of GH99 alloy more difficult. In addition, the precipitation and dissolution of coherent precipitates and secondary carbides in the alloy also play an important role in the safety of the hot working process. Therefore, the microstructure transformation of the GH99 alloy during hot working is complex and hot working is difficult.
[0003] Therefore, current nickel alloys and their processing methods still need to be improved. Summary of the invention
[0004] The present application aims to provide a method for double-pass hot compression processing of nickel alloy to solve or alleviate one or more technical problems in the related art.
[0005] In one aspect of the present application, a method for processing a nickel alloy is proposed. The method includes: cutting an alloy base material to obtain a cylindrical sample; performing a first compression on the cylindrical sample, wherein the deformation condition of the first compression is determined according to the result of a single compression test, and the deformation condition includes at least one of a deformation temperature and a strain rate; cooling the sample after the first compression until the temperature of the sample is reduced to the deformation temperature of the second compression, and performing a second compression, wherein the deformation temperature of the second compression is 1050-1100°C and the strain rate is 0.001-0.005s -1; The sample after the second compression is subjected to water quenching treatment to obtain the treated nickel alloy, wherein the single-pass compression experiment includes multiple single-pass compression treatments at different predetermined deformation temperatures and predetermined strain rates. The method can improve the deformation resistance of the alloy obtained after the treatment, and improve the grain size distribution and dynamic softening degree by improving the double-pass compression process.
[0006] According to an embodiment of the present application, the nickel alloy is GH99.
[0007] According to an embodiment of the present application, determining the deformation condition of the first compression according to the result of the single-pass compression experiment includes: selecting a predetermined deformation temperature of the single-pass compression treatment in which the rheological stress is low during multiple single-pass compression treatments, and / or the content of small-angle grain boundaries in the sample after treatment is less than 10% as the deformation temperature of the first compression treatment; and determining the strain rate of the first compression treatment: the critical strain of dynamic recrystallization of the deformation condition.
[0008] According to an embodiment of the present application, the single-pass compression test includes: performing multiple single-pass compression treatments at a predetermined deformation temperature and a predetermined strain rate, wherein the predetermined deformation temperature and the predetermined strain rate of each single-pass compression treatment are different, and the predetermined deformation temperature is 1000-1200°C; the predetermined strain rate is 0.001-1s -1 .
[0009] According to an embodiment of the present application, the method further comprises: determining the strain amount of the first compression process according to the single-pass compression experiment; the strain amount is 0.1%-1%.
[0010] According to an embodiment of the present application, the strain amount of the second compression process is 0.65.
[0011] According to an embodiment of the present application, the method further comprises: before performing the thermal compression treatment, placing graphite sheets and Ta sheets on both ends of the columnar sample and applying a high-temperature lubricant.
[0012] According to an embodiment of the present application, the method satisfies at least one of the following conditions: the columnar specimen is a cylindrical specimen with a diameter of 8-12 mm and a height of 10-20 mm; and the thermal compression treatment is performed on a Gleeble-3500 thermal simulator.
[0013] According to an embodiment of the present application, the method includes: determining, through a single-pass compression test, that the conditions of the first-pass compression treatment are: a deformation temperature of 1100-1150° C., a strain rate of 0.001 s -1, strain 0.05; perform the first compression treatment, and directly cool the sample to the deformation temperature of the second compression; perform the second compression treatment on the sample, the deformation temperature of the second compression treatment is 1050-1100°C, and the strain rate is 0.001s -1 , strain value is 0.65.
[0014] In another aspect of the present application, the present application provides a nickel alloy which is processed by the above method.
[0015] The present invention provides a double-pass hot compression process for making GH99 alloy have low deformation resistance, uniform grain structure, and small internal orientation difference of the structure, and selects the deformation conditions in the first compression of the double-pass hot compression process according to the single-pass compression result. And directly cool down to the second compression temperature between passes. The above treatment can improve the deformation resistance, grain size distribution, dynamic softening degree and other aspects of the treated alloy.
[0016] The above summary is for the purpose of description only and is not intended to be limiting in any way. In addition to the illustrative aspects, embodiments and features described above, further aspects, embodiments and features of the present application will be readily apparent through the following detailed description. BRIEF DESCRIPTION OF THE DRAWINGS
[0017] Figure 1 The stress-strain test results of the embodiments of the present application and the comparative examples are shown;
[0018] Figure 2 The microstructure diagrams of the embodiments of the present application and the comparative examples are shown. DETAILED DESCRIPTION
[0019] In the following, only some exemplary embodiments are briefly described. As those skilled in the art will appreciate, the described embodiments may be modified in various ways without departing from the spirit or scope of the present application, and different embodiments may be combined arbitrarily without conflict. Therefore, the following description is considered to be exemplary and non-restrictive in nature.
[0020] In one aspect of the present application, a method for processing a nickel alloy is proposed. The method includes: cutting an alloy base material to obtain a cylindrical specimen, and performing a first compression on the cylindrical specimen. The deformation conditions of the first compression are determined based on the results of a single-pass compression test, and the single-pass compression test includes multiple single-pass compression treatments at different predetermined deformation temperatures and predetermined strain rates. The deformation temperature and / or strain rate of the first compression is then determined based on the results of the single-pass compression test. Subsequently, a temperature reduction treatment is performed on the sample that has undergone the first compression. The temperature reduction treatment is to lower the sample temperature to reduce the deformation temperature of the subsequent second compression, and then perform a second compression. The deformation temperature of the second compression is 1050-1100°C, and the strain rate is 0.001-0.005s -1 Finally, the sample after the second compression is subjected to water quenching treatment to obtain a treated nickel alloy. The method can improve the deformation resistance of the treated alloy, and improve the grain size distribution and dynamic softening degree by improving the double-pass compression process.
[0021] In the method proposed in the present application, the specific type of nickel alloy to be processed is not particularly limited. For example, the nickel alloy may be GH99. As mentioned above, due to the high content of γ′ phase-forming elements in GH99, the hot working of GH99 is particularly complicated. The present application first determines the optimal deformation conditions of the first pass through a single-pass compression test, thereby better improving the microstructure of the alloy and enhancing the processing performance.
[0022] The cylindrical specimen cut from the alloy base material may have a diameter of 8-12 mm and a height of 10-20 mm.
[0023] According to the embodiment of the present application, the first and second compression processes in the double-pass hot compression process and the single-pass compression experiment can be performed on a Gleeble-3500 thermal simulator. Those skilled in the art can also select other instruments with corresponding functions to perform the above experiments or processes.
[0024] Specifically, the single-pass compression test includes performing multiple single-pass compression treatments at a predetermined deformation temperature and a predetermined strain rate. The predetermined deformation temperature and the predetermined strain rate of each single-pass compression treatment are different, for example, a different predetermined denaturation temperature or a different predetermined strain rate may be used. Alternatively, the deformation temperature and strain rate of each single-pass compression treatment may be different from those of the previous treatment. By performing multiple single-pass compression treatments and analyzing the properties of the treated samples, the optimal single-pass compression conditions can be determined, and then the deformation conditions of the first compression treatment can be determined.
[0025] Specifically, the predetermined deformation temperature of the single-pass compression test may be between 1000-1200°C, and a value between 1000-1200°C may be selected as the predetermined deformation temperature for each single-pass compression process. Similarly, the predetermined strain rate may be 0.001-1s -1 Each time a single compression process is performed, a value can be selected within the above-mentioned predetermined strain rate range as the predetermined deformation rate.
[0026] According to some specific examples of the present application, four single-pass compression tests may be performed. The deformation temperatures of the single-pass compression tests may be 1020°C, 1070°C, 1120°C, 1170°C, etc., and the strain rate may be 0.001s -1 、0.01s -1 , 0.1s -1 , 1s -1 wait.
[0027] In some specific examples, the following temperature and strain rate parameters can be used for 16 single-pass compressions: 1020°C, 0.001 / s; 1020°C, 0.01 / s; 1020°C, 0.1 / s; 1020°C, 1 / s; 1070°C, 0.001 / s; 1070°C, 0.01 / s; 1070°C, 0.1 / s; 1070°C, 1 / s; 1120°C, 0.001 / s; 1120°C, 0.01 / s; 1120°C, 0.1 / s; 1120°C, 1 / s; 1170°C, 0.001 / s; 1170°C, 0.01 / s; 1170°C, 0.1 / s; 1170°C, 1 / s.
[0028] Subsequently, the deformation condition of the first compression can be determined according to the result of the single-pass compression test. The determination of the deformation condition can include determining at least one of the deformation temperature, the strain rate, and the strain amount. Preferably, the deformation temperature, the strain rate, and the strain amount are determined according to the result of the single-pass compression test.
[0029] Specifically, the deformation temperature can be selected under experimental conditions with low rheological stress, suitable processing area in the thermal processing diagram, and good microstructure during multiple single-pass compression treatments. For example, the predetermined deformation temperature of a single-pass compression treatment with a small content of small-angle grain boundaries in the treated sample can be selected as the deformation temperature of the first compression treatment.
[0030] In the present application, the low-angle grain boundary content can be determined by local mismatch angle analysis, and can be specifically obtained through a KAM diagram of the microstructure of the alloy.
[0031] Specifically, the optimal deformation conditions can be screened according to the microstructure of the alloy after treatment: for example, according to the microstructure observation of the alloy, such as the IPF, KAM and GBs diagram, the processing parameters with fewer deformed grains and more uniform grain size distribution can be selected as the conditions for the first compression treatment.
[0032] Determining the deformation conditions of the first compression process may also include determining the strain rate of the first compression process, and the determination of the strain rate may also select experimental conditions with better alloy microstructure. The strain amount may be determined based on the dynamic recrystallization critical strain amount of the previously determined deformation conditions (deformation temperature and strain rate). Specifically, the strain amount of the first compression process may be 0.1%-1%.
[0033] According to the embodiment of the present application, in order to further improve the effect of using the method to treat the alloy, before the hot compression treatment, graphite sheets and Ta sheets can be placed at both ends of the cylindrical sample and high-temperature lubricant can be applied, thereby better reducing these frictional heat insulation effects.
[0034] After the first compression treatment, the temperature of the sample can be directly cooled to the deformation temperature of the second compression by cooling treatment, and then the second compression treatment is performed. In some embodiments, the deformation temperature of the second compression treatment is 1050-1100°C, and the strain rate is 0.001s -1 , strain value is 0.65.
[0035] In another aspect of the present application, the present application provides a nickel alloy which is processed by the above method.
[0036] In general, the method proposed in this application can better improve the deformation resistance, grain size distribution, dynamic softening degree, etc. of nickel alloys, especially GH99.
[0037] The method proposed in this application is described below by means of specific examples. The methods used in the following examples are conventional methods unless otherwise specified, and the reagents used are commercially available reagents unless otherwise specified.
[0038] Example 1
[0039] Step 1: Before hot compression, place graphite sheets and Ta sheets on both ends of the sample and evenly apply high-temperature lubricant to minimize the friction and thermal insulation effects.
[0040] Step 2: Cut a cylindrical specimen with a diameter of 10 mm and a height of 15 mm from the alloy base material and grind it. Perform a single-pass hot compression test on a Gleeble-3500 thermal simulator. The experimental conditions for 16 times are as follows:
[0041] 1020℃, 0.001 / s;
[0042] 1020℃, 0.01 / s;
[0043] 1020℃, 0.1 / s;
[0044] 1020℃, 1 / s;
[0045] 1070℃, 0.001 / s;
[0046] 1070℃, 0.01 / s;
[0047] 1070℃, 0.1 / s;
[0048] 1070℃, 1 / s;
[0049] 1120℃, 0.001 / s;
[0050] 1120℃, 0.01 / s;
[0051] 1120℃, 0.1 / s;
[0052] 1120℃, 1 / s;
[0053] 1170℃, 0.001 / s;
[0054] 1170℃, 0.01 / s;
[0055] 1170℃, 0.1 / s;
[0056] 1170℃, 1 / s.
[0057] Step 3: Perform the first compression of the double-pass hot compression process. The deformation conditions are selected according to the single-pass compression results. The deformation temperature is 1120℃ and the strain rate is 0.001s -1 .
[0058] Step 4: Select the process between passes and choose to directly cool down to the second pass compression temperature between passes ( Figure 2 The marked cooling process).
[0059] Step 5: Perform the second compression of the double-pass hot compression process, with a deformation temperature of 1070°C and a strain rate of 0.001s -1 .
[0060] Step 6: After the compression, the sample is immediately quenched in water to retain the structure after thermal deformation.
[0061] Step 7: Cut the compressed sample along the compression axis, grind and polish. Use EBSD characterization method to analyze the grain morphology, grain orientation and grain boundary of the alloy. The electrolyte ratio of electrolytic polishing is perchloric acid (HClO 4 ):Ethanol (C 2 H 5 OH)=10:90 (volume ratio), electropolishing for 30s at 25V voltage and room temperature, and the current was controlled at about 1.5mA.
[0062] Comparative Example 1
[0063] Only a single hot compression is performed on the sample of Example 1, with a deformation temperature of 1070°C and a strain rate of 0.001s -1 ( Figure 2 single pass marked).
[0064] Comparative Example 2
[0065] The sample of Example 1 was subjected to a double-pass hot compression process. The process flow was the same as that of Example 1. The difference from Example 1 was that in step 4, the process between passes was immediately water-cooled and then heated again to the second pass deformation temperature ( Figure 2 Water cooling as marked).
[0066] Comparative Example 3
[0067] The sample of Example 1 was subjected to a double-pass hot compression process. The process flow was the same as that of Example 1. The difference from Example 1 was that in step 4, the temperature was lowered to the second deformation temperature and then kept warm for 180 seconds between passes. Figure 2 marked cooling-insulation process).
[0068] The compressive stress-strain test of Example 1 and Comparative Examples 1-3 yields the following test curves: Figure 1 As shown. Specifically, the alloy was recorded on a Gleeble-3500 thermal simulator during the aforementioned hot compression treatment, and the tensile, compressive and torsional deformations at different speeds. At the same time, the changes in parameters such as temperature, force, strain and stress in the test area were recorded to obtain a curve of true strain (Truestrain) versus true stress (True stress). The second compression stress value of the cooling process after the first compression treatment is the lowest, while the second compression stress values of the cooling-insulation process, single compression and water cooling process increase in turn.
[0069] EBSD was used to observe the microstructure of the compressed sample. The IPF, KAM and GBs diagrams are shown in Figure 2. Figure 2As shown. Among them, (b1)-(b4) are the organization diagrams after the cooling process deformation, the deformed grains disappear, and the grain size distribution is relatively uniform. From the KAM diagram, it can be seen that the average orientation difference in the organization is small, and the content of small-angle grain boundaries is 8.9%. However, the organization after the cooling-insulation process, single-pass compression and water cooling process deformation is not uniform, the orientation difference inside the organization is large, and the content of small-angle grain boundaries is high, which is 12.3%, 11.2%, and 12.9% respectively.
[0070] In addition, the terms "first" and "second" are used for descriptive purposes only and should not be understood as indicating or implying relative importance or implicitly indicating the number of technical features indicated. Therefore, a feature defined as "first" or "second" may explicitly or implicitly include one or more of the features. In the description of this application, the meaning of "plurality" is two or more, unless otherwise clearly and specifically defined.
[0071] The above application provides many different embodiments or examples to realize the different structures of the present application. In order to simplify the present application, the parts and settings of specific examples are described above. Of course, they are only examples, and the purpose is not to limit the present application. In addition, the present application can repeat reference numbers and / or reference letters in different examples, and this repetition is for the purpose of simplification and clarity, which itself does not indicate the relationship between the various embodiments and / or settings discussed.
[0072] The above are only specific implementations of the present application, but the protection scope of the present application is not limited thereto. Any technician familiar with the technical field can easily think of various changes or substitutions within the technical scope disclosed in the present application, which should be included in the protection scope of the present application. Therefore, the protection scope of the present application should be based on the protection scope of the claims.
Claims
1. A method for treating a nickel alloy, characterized in that: include: The alloy base material is cut to obtain cylindrical specimens; Performing a first compression on the cylindrical sample, wherein the deformation condition of the first compression is determined according to the result of a single-pass compression test, and the deformation condition includes at least one of a deformation temperature and a strain rate; The sample after the first compression is subjected to a cooling treatment until the temperature of the sample is reduced to the deformation temperature of the second compression, and then subjected to a second compression, wherein the deformation temperature of the second compression is 1050-1100°C and the strain rate is 0.001-0.005s -1 ; The sample subjected to the second compression is subjected to water quenching treatment to obtain the treated nickel alloy. in, The single-pass compression test includes performing multiple single-pass compression processes at different predetermined deformation temperatures and predetermined strain rates.
2. The method according to claim 1, characterized in that: The nickel alloy is GH99.
3. The method according to claim 1 or 2, characterized in that: The deformation conditions of the first compression pass are determined according to the results of the single-pass compression test, including: selecting a predetermined deformation temperature and a predetermined strain rate of a single-pass compression treatment in which the flow stress is low during the multiple single-pass compression treatments and / or the content of small-angle grain boundaries in the sample after treatment is less than 10% as the deformation temperature of the first compression treatment; and The strain rate of the first compression treatment is determined: the critical strain of dynamic recrystallization under this deformation condition.
4. The method according to claim 3, characterized in that The single-pass compression test includes: Multiple single-pass compression processes are performed at a predetermined deformation temperature and a predetermined strain rate, wherein the predetermined deformation temperature and the predetermined strain rate of each single-pass compression process are different. The predetermined deformation temperature is 1000-1200°C; The predetermined strain rate is 0.001-1s -1 .
5. The method according to claim 3, characterized in that: Further including: Determining the strain amount of the first compression process according to the single-pass compression experiment; The strain amount is 0.1%-1%.
6. The method according to claim 1, characterized in that The strain amount of the second compression process is 0.
65.
7. The method according to claim 1, characterized in that The method further comprises: Before the hot compression treatment, graphite sheets and Ta sheets were placed on both ends of the columnar sample and high-temperature lubricant was applied.
8. The method according to claim 1, characterized in that The method satisfies at least one of the following conditions: The cylindrical specimen is a cylindrical specimen with a diameter of 8-12 mm and a height of 10-20 mm; The thermal compression treatment was carried out on a Gleeble-3500 thermal simulator.
9. The method according to claim 1, characterized in that: include: The conditions of the first compression treatment were determined by a single-pass compression test as follows: deformation temperature of 1100-1150°C, strain rate of 0.001s -1 , strain value 0.05; The first compression process is performed, and the sample is directly cooled to the deformation temperature of the second compression process; The sample is subjected to a second compression treatment, wherein the deformation temperature of the second compression treatment is 1050-1100°C and the strain rate is 0.001s -1 , strain value is 0.
65.
10. A nickel alloy, characterized in that: The nickel alloy is processed by the method according to any one of claims 1-9.
Citation Information
Patent Citations
Method for refining nickel-base superalloy forge piece grain structures
CN106756685A
Method for predicting dissolution fraction of delta phase of Nb-containing nickel-based alloy under time-varying working condition
CN110751991A
Making method of nickel-based alloy hot working process
CN110964994A
High-strength and high-toughness copper alloy material and preparation method thereof
CN111187941A
Physical simulation method for nickel-based superalloy forging process
CN115323298A