Nickel-cobalt-based tungsten carbide wear-resistant powder preparation and high velocity oxy-fuel thermal spraying method

Through the improved nickel-cobalt-based tungsten carbide powder preparation process and supersonic flame thermal spraying method, the problems of insufficient powder particle size and purity in the traditional process are solved, and the preparation of high-purity powder and the density and bonding of the coating are achieved. Strength, improving the material's service life and performance.

CN118726889APending Publication Date: 2024-10-01YANTAI WEINA TECH CO LTD
View PDF 0 Cites 0 Cited by

Patent Information

Application Number
CN202410767132.0
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Filing Date
2024-06-14
Publication Date
2024-10-01

AI Technical Summary

Technical Problem

The traditional nickel-cobalt-based tungsten carbide wear-resistant powder preparation process cannot fully optimize the particle size distribution, morphology and purity of the powder, resulting in insufficient uniformity and density of the coating after spraying. Improper control of parameters in the supersonic flame thermal spraying process may result in coating defects. Insufficient layer bonding and excessive internal stress affect service life and performance, and poor material matching may cause coating peeling and cracking.

Method used

An improved nickel powder, cobalt powder and tungsten carbide powder preparation process is used to prepare high-purity powder through the steps of coating salt precursor solution precipitation, suction filtration, drying, sintering and ball milling, and during the supersonic flame thermal spraying process The powder is heated to a molten or semi-molten state to form a dense coating, combined with a two-way pressing method and airflow stirring technology to optimize spraying parameters such as gun distance, angle and speed.

Benefits of technology

The preparation of nickel-cobalt-based tungsten carbide powder with high purity, controllable particle size and shape is achieved, ensuring the density and bonding strength of the coating, reducing porosity and risk of shedding, and improving the service life and performance of the material.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN118726889A_ABST
    Figure CN118726889A_ABST
Patent Text Reader

Abstract

The invention relates to the technical field of material science and surface engineering, in particular to a nickel-cobalt-based tungsten carbide wear-resistant powder preparation and hypersonic flame thermal spraying method which comprises the steps of nickel powder preparation, cobalt powder preparation, tungsten carbide powder preparation, a nickel-cobalt-based tungsten carbide wear-resistant powder preparation process and a nickel-cobalt-based tungsten carbide wear-resistant powder hypersonic flame thermal spraying method. According to the method, in the spraying process, powder is heated to be in a molten or semi-molten state under the action of supersonic flame and impacts on the surface of the workpiece at an extremely high speed, a formed coating has high compactness and bonding strength, the porosity of the coating can be effectively reduced, the surface performance can be effectively improved, and the service life of the coating is prolonged. And firm combination between the coating and the workpiece can be ensured, and the risk of falling off and stripping is reduced.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The invention relates to the field of material science and surface engineering technology, in particular to a method for preparing nickel-cobalt-based tungsten carbide wear-resistant powder and a supersonic flame thermal spraying method. Background Art

[0002] With the rapid development of the industrial field, the requirements for material performance are also constantly increasing. Traditional surface treatment technology can no longer meet the requirements of modern industry for material performance. Therefore, the development of new wear-resistant powder materials and efficient spraying technology has become a research hotspot in the field of materials science. The preparation of nickel-cobalt-based tungsten carbide wear-resistant powder and supersonic flame thermal spraying technology are important research results in this context.

[0003] Traditional preparation processes may not be able to fully optimize the particle size distribution, morphology and purity of the powder, which directly affects the uniformity and density of the coating after spraying. If there are too many impurities or uneven particle size distribution in the powder, the coating after spraying may have defects, thereby reducing its service life and performance. Secondly, parameter control in the supersonic flame thermal spraying process is also a key factor. The selection of parameters such as spraying speed, temperature, and spraying distance has a significant impact on the quality and performance of the coating. If the parameters are not set properly, it may lead to problems such as loose bonding between the coating and the substrate and excessive internal stress in the coating, thereby affecting the service life and performance of the coating. In addition, the matching of materials is also an issue that needs to be considered. Different substrate materials and coating materials have different physical and chemical properties. If the matching is not good, it may cause the coating to peel off and crack during use, thereby reducing its service life and performance. For this reason, our nickel-cobalt-based tungsten carbide wear-resistant powder preparation and supersonic flame thermal spraying method solve the above problems. Summary of the invention

[0004] The purpose of the present invention is to provide a method for preparing nickel-cobalt-based tungsten carbide wear-resistant powder and a supersonic flame thermal spraying method to solve the problems raised in the above background technology.

[0005] The technical scheme of the present invention is: a method for preparing nickel-cobalt-based tungsten carbide wear-resistant powder and a supersonic flame thermal spraying method, including the preparation of nickel powder, the preparation of cobalt powder, the preparation of tungsten carbide powder, the preparation process of nickel-cobalt-based tungsten carbide wear-resistant powder, and the supersonic flame thermal spraying method of nickel-cobalt-based tungsten carbide wear-resistant powder;

[0006] The preparation of the nickel powder comprises the following steps:

[0007] Step S1: prepare 1L of nickel sulfate solution with a concentration of 0.5mol / L, add 1000ml of 2% dispersant polyethylene glycol, continue to stir evenly, then add an equimolar amount of oxalic acid solution to perform precipitation reaction to generate a single precursor solution, and simultaneously add 2L (0.5mol / L) of zinc chloride solution to be coated and an equimolar amount of oxalic acid solution to the single precursor solution to generate a coating salt precursor solution;

[0008] Step S2: The coating salt precursor solution is filtered, dried, and sintered to obtain zinc oxide coated nickel powder, and finally washed with hydrochloric acid to remove the coating layer, rinsed with anhydrous ethanol, and dried at 65° C. in a vacuum atmosphere to obtain high-purity nickel powder;

[0009] The preparation of the cobalt powder comprises the following steps:

[0010] Step S3: Dissolve Co(Ac)2·4H2O (6.25 g 0.025 mol) in 50 mL of water, then add ethylenediaminetetraacetic acid (7.31 g 0.025 mol), heat, stir, dissolve, slowly dropwise add dilute NaOH solution, adjust the pH value of the mother solution to 1011, keep the temperature at 70°C, add 7 mL 85% hydrazine hydrate under uniform stirring, and continue the reaction for about 4 hours until the upper layer solution becomes colorless and transparent, and the lower layer is a gray powdery precipitate, filter, wash with distilled water, then wash with anhydrous ethanol and anhydrous ether, drain, and vacuum dry at below 40°C for 48 hours to obtain high-purity cobalt powder;

[0011] The preparation of the tungsten carbide powder comprises the following steps:

[0012] Step S4: carbon black is added with tungsten powder according to 4% to 6.13%, and the mixture is put into a ball mill tank for dry mixing, with a ball-to-material ratio of 1:1, and the mixture is ball milled for 6 hours. The mixed material is put into a cylindrical graphite crucible, loaded into a furnace, and nitrogen is introduced into the furnace to exhaust the air inside. After ensuring that the air in the furnace is exhausted, hydrogen is introduced and the exhausted hydrogen is ignited at the exhaust port of the furnace. The temperature is raised at the maximum power of the furnace, and the temperature reaches 2000° C. in about 1 hour, and then the temperature is kept for 5 hours. The power is turned off and the furnace is cooled for 18 hours before being taken out of the furnace. The tungsten carbide powder after carburization treatment is in the shape of a cylindrical block. After being crushed, it is ball milled for 30 minutes to obtain tungsten carbide powder;

[0013] The preparation process steps of the nickel-cobalt based tungsten carbide wear-resistant powder are as follows:

[0014] Step S5: Put the prepared high-purity nickel powder, high-purity cobalt powder and tungsten carbide powder into a mixer according to a preset ratio (1:1:1), mix them by airflow stirring to make the components fully and evenly distributed, and the powder after mixing evenly needs to be prepared by a molding process such as compression molding and static pressing molding, and the powder is compressed into a dense block. The formed block is sintered at a high temperature of 2000°C, and the sintered block is crushed into smaller particles, and a nickel-cobalt-based tungsten carbide wear-resistant powder is obtained by a screening process;

[0015] The nickel-cobalt-based tungsten carbide wear-resistant powder supersonic flame thermal spraying method comprises the following steps:

[0016] Step S6: cleaning, derusting and roughening the surface of the workpiece to be sprayed;

[0017] Step S7: feeding the nickel-cobalt-based tungsten carbide wear-resistant powder into the spray gun of the supersonic flame spraying equipment. During the spraying process, the powder is heated to a molten or semi-molten state under the action of the supersonic flame, and impacts the surface of the workpiece at a high speed to form a dense coating.

[0018] Preferably, a plurality of steel balls are arranged inside the ball mill, and the diameter of the steel balls is 45 mm.

[0019] Preferably, the filtration device is composed of a filtration bottle, a funnel, a safety bottle, and an air pump component, and filter paper is arranged in the funnel.

[0020] Preferably, the core step of the molding preparation process is to adopt a bidirectional pressing method, in which plastic deformation and diffusion occur between the powder particles, and the powder particles are combined together to form a continuous and dense structure.

[0021] Preferably, the air flow stirring is performed using a bubbler, the tube wall of the bubbler is composed of a tube with multiple small holes, and the stirring achieves mixing of the powders through the movement of bubbles.

[0022] Preferably, during the supersonic flame thermal spraying, the distance between the spray gun and the workpiece is adjusted to 220 mm, the spraying angle is 60°, and the spraying speed is 500 m / s.

[0023] Preferably, when the carbonization temperature is 2000° C., the free carbon content is 0.015% and the combined carbon content is 6.6115%.

[0024] Preferably, the sintering temperature of the coating salt precursor solution in a reducing atmosphere furnace is 900-1200°C.

[0025] The present invention provides a grass mosaic material science and surface engineering by improvement, which has the following improvements and advantages compared with the prior art:

[0026] First, the present invention can effectively remove the zinc oxide coating and other impurities through hydrochloric acid washing to ensure the high purity of the nickel powder, and the rinsing with anhydrous ethanol can further remove the trace impurities that may remain, laying the foundation for finally obtaining high-purity nickel powder. The 65°C drying in a vacuum atmosphere can prevent the nickel powder from contacting with oxygen in the air during the drying process, thereby preventing the nickel powder from being oxidized. This low-temperature drying method also helps to maintain the stability of the physical and chemical properties of the nickel powder. The low-temperature drying at 65°C can reduce the thermal expansion and deformation of the nickel powder and maintain its original shape and structure, which is particularly important for the application of nickel powder that requires a specific shape or structure. The 65°C vacuum drying oven has a significant energy-saving advantage. Through efficient energy utilization and a closed drying process, almost no waste heat and dust are generated, and high-purity nickel powder can be prepared efficiently and environmentally friendly, providing a high-quality raw material basis for the further application of nickel powder.

[0027] Second, the present invention can effectively remove impurities through suction filtration, washing and vacuum drying, thereby obtaining high-purity cobalt powder. The reaction conditions and subsequent processing steps can be precisely controlled to achieve effective regulation of the particle size and morphology of the cobalt powder. Heating, stirring and slowly dropping a dilute NaOH solution can accelerate the reaction process, improve the reaction efficiency, help shorten the production cycle, and reduce production costs. The reagents and solvents used in the process, such as ethylenediaminetetraacetic acid and hydrazine hydrate, can be recycled or harmlessly treated after the reaction is completed, thereby reducing pollution to the environment. In addition, by optimizing the reaction conditions and process parameters, energy consumption and emissions can be further reduced. The preparation process is relatively simple, easy to operate, and has high repeatability, which helps to ensure the stability of product quality and is convenient for industrial production. Through this series of reactions and processing steps, high-purity cobalt powder with controllable particle size and morphology can be obtained, while realizing an environmentally friendly, efficient and sustainable production process.

[0028] Thirdly, in the present invention, during the spraying process, the powder is heated to a molten or semi-molten state under the action of a supersonic flame, and impacts the surface of the workpiece at an extremely high speed. The formed coating has a high degree of density and bonding strength, which can not only effectively reduce the porosity of the coating and improve the surface performance, but also ensure that the bonding between the coating and the workpiece is more firm, reducing the risk of falling off and peeling. BRIEF DESCRIPTION OF THE DRAWINGS

[0029] The present invention will be further explained below in conjunction with the accompanying drawings and embodiments:

[0030] Figure 1 Schematic diagram of the supersonic flame thermal spraying method under different conditions of the present invention;

[0031] Figure 2 It is a schematic diagram of the initial grain size of the nickel powder obtained at different calcination temperatures of the present invention. DETAILED DESCRIPTION

[0032] The present invention is described in detail below, and the technical solutions in the embodiments of the present invention are clearly and completely described. Obviously, the described embodiments are only part of the embodiments of the present invention, not all of the embodiments. Based on the embodiments of the present invention, all other embodiments obtained by ordinary technicians in this field without creative work are within the scope of protection of the present invention.

[0033] The present invention provides a method for preparing nickel-cobalt-based tungsten carbide wear-resistant powder and a supersonic flame thermal spraying method by improving the present invention. The technical solution of the present invention is:

[0034] like Figure 1 - Figure 2 As shown, the preparation of nickel-cobalt-based tungsten carbide wear-resistant powder and the supersonic flame thermal spraying method include the preparation of nickel powder, the preparation of cobalt powder, the preparation of tungsten carbide powder, the preparation process of nickel-cobalt-based tungsten carbide wear-resistant powder, and the supersonic flame thermal spraying method of nickel-cobalt-based tungsten carbide wear-resistant powder;

[0035] The preparation of nickel powder comprises the following steps:

[0036] Step S1: prepare 1L of nickel sulfate solution with a concentration of 0.5mol / L, add 1000ml of 2% dispersant polyethylene glycol, continue to stir evenly, then add an equimolar amount of oxalic acid solution to perform precipitation reaction to generate a single precursor solution, and simultaneously add 2L (0.5mol / L) of zinc chloride solution to be coated and an equimolar amount of oxalic acid solution to the single precursor solution to generate a coating salt precursor solution;

[0037] Step S2: The coating salt precursor solution is filtered, dried, and sintered to obtain zinc oxide coated nickel powder, and finally washed with hydrochloric acid to remove the coating layer, rinsed with anhydrous ethanol, and dried at 65° C. in a vacuum atmosphere to obtain high-purity nickel powder;

[0038] The preparation of cobalt powder includes the following steps:

[0039] Step S3: Dissolve Co(Ac)2·4H2O (6.25 g 0.025 mol) in 50 mL of water, then add ethylenediaminetetraacetic acid (7.31 g 0.025 mol), heat, stir, dissolve, slowly dropwise add dilute NaOH solution, adjust the pH value of the mother solution to 1011, keep the temperature at 70°C, add 7 mL 85% hydrazine hydrate under uniform stirring, and continue the reaction for about 4 hours until the upper layer solution becomes colorless and transparent, and the lower layer is a gray powdery precipitate, filter, wash with distilled water, then wash with anhydrous ethanol and anhydrous ether, drain, and vacuum dry at below 40°C for 48 hours to obtain high-purity cobalt powder;

[0040] The preparation of tungsten carbide powder includes the following steps:

[0041] Step S4: carbon black is added with tungsten powder according to 4% to 6.13%, and the mixture is put into a ball mill tank for dry mixing, with a ball-to-material ratio of 1:1, and the mixture is ball milled for 6 hours. The mixed material is put into a cylindrical graphite crucible, loaded into a furnace, and nitrogen is introduced into the furnace to exhaust the air inside. After ensuring that the air in the furnace is exhausted, hydrogen is introduced and the exhausted hydrogen is ignited at the exhaust port of the furnace. The temperature is raised at the maximum power of the furnace, and the temperature reaches 2000° C. in about 1 hour, and then the temperature is kept for 5 hours. The power is turned off and the furnace is cooled for 18 hours before being taken out of the furnace. The tungsten carbide powder after carburization treatment is in the shape of a cylindrical block. After being crushed, it is ball milled for 30 minutes to obtain tungsten carbide powder;

[0042] The preparation process steps of nickel-cobalt based tungsten carbide wear-resistant powder are as follows:

[0043] Step S5: Put the prepared high-purity nickel powder, high-purity cobalt powder and tungsten carbide powder into a mixer according to a preset ratio (1:1:1), mix them by airflow stirring to make the components fully and evenly distributed, and the powder after mixing evenly needs to be prepared by a molding process such as compression molding and static pressing molding, and the powder is compressed into a dense block. The formed block is sintered at a high temperature of 2000°C, and the sintered block is crushed into smaller particles, and a nickel-cobalt-based tungsten carbide wear-resistant powder is obtained by a screening process;

[0044] The method for supersonic flame thermal spraying of nickel-cobalt-based tungsten carbide wear-resistant powder comprises the following steps:

[0045] Step S6: cleaning, derusting and roughening the surface of the workpiece to be sprayed;

[0046] Step S7: feeding the nickel-cobalt-based tungsten carbide wear-resistant powder into the spray gun of the supersonic flame spraying equipment. During the spraying process, the powder is heated to a molten or semi-molten state under the action of the supersonic flame, and impacts the surface of the workpiece at a high speed to form a dense coating.

[0047] Furthermore, a plurality of steel balls are arranged inside the ball mill, and the diameter of the steel balls is 45 mm. The 45 mm steel balls also have good wear resistance and strength, and can withstand long-term, high-intensity grinding work, thereby reducing the frequency of replacing steel balls and reducing maintenance costs.

[0048] Furthermore, the filtration device is composed of a filtration bottle, a funnel, a safety bottle, and an air pump component. Filter paper is arranged in the funnel. The filtration device has a simple structure, the equipment is easily available, and the operation is simple. The user can easily master the operation method without having a sophisticated technical background.

[0049] Furthermore, the core step of the molding preparation process is to adopt a bidirectional pressing method, in which plastic deformation and diffusion occur between the powder particles, and they combine together to form a continuous and dense structure. Through bidirectional pressing, the powder particles are subjected to pressure from both ends in the mold cavity, which makes the contact between the particles closer, helps to eliminate the gaps between the particles, can significantly improve the density of the compact, and ensure the uniformity of the density.

[0050] Furthermore, air flow stirring uses a bubbler for stirring. The tube wall of the bubbler is composed of a tube with multiple small holes. The stirring is achieved by the movement of bubbles to mix the powder. When the bubbles generated by the bubbler move in the liquid, they can drive the powder particles to form effective convection and diffusion, thereby achieving efficient mixing. The mixing method is more uniform than traditional mechanical stirring.

[0051] Furthermore, during supersonic flame thermal spraying, the distance between the spray gun and the workpiece is adjusted to 220 mm, the spraying angle is 60°, and the spraying speed is 500 m / s. The distance between the spray gun and the workpiece is 220 mm, which helps to ensure that the spraying particles still maintain a high speed and energy when reaching the workpiece surface, thereby enhancing the bonding strength between the coating and the substrate. The spraying angle of 60° helps to achieve uniform distribution of the spraying particles, making the coating smoother and denser. The spraying speed of 500 m / s gives the particles higher kinetic energy, which can more effectively penetrate the tiny pores and uneven areas on the workpiece surface to form a tighter coating.

[0052] Furthermore, when the carbonization temperature is 2000°C, the free carbon content is 0.015% and the combined carbon content is 6.6115%, which helps to enhance the structural stability of the material and reduce the degradation of material performance caused by the activity of carbon elements. Too high a free carbon content may cause the material to become brittle, while an increase in combined carbon helps to reduce this brittleness and improve the toughness and impact resistance of the material.

[0053] Furthermore, the sintering temperature of the coating salt precursor solution in a reducing atmosphere furnace is 900-1200°C. Compared with higher sintering temperatures, the temperature range of 900-1200°C can reduce energy consumption and improve production efficiency while ensuring product quality. The lower temperature also means relatively lower requirements for equipment, reducing production costs.

[0054] The above description enables those skilled in the art to implement or use the present invention. Various modifications to these embodiments will be apparent to those skilled in the art, and the general principles defined herein may be implemented in other embodiments without departing from the spirit or scope of the present invention. Therefore, the present invention will not be limited to the embodiments shown herein, but will conform to the widest scope consistent with the principles and novel features disclosed herein.

Claims

1. Preparation of nickel-cobalt-based tungsten carbide wear-resistant powder and supersonic flame thermal spraying method, characterized in that: Including the preparation of nickel powder, the preparation of cobalt powder, the preparation of tungsten carbide powder, the preparation process of nickel-cobalt-based tungsten carbide wear-resistant powder, and the supersonic flame thermal spraying method of nickel-cobalt-based tungsten carbide wear-resistant powder; The preparation of the nickel powder comprises the following steps: Step S1: prepare 1L of nickel sulfate solution with a concentration of 0.5mol / L, add 1000ml of 2% dispersant polyethylene glycol, continue to stir evenly, then add an equimolar amount of oxalic acid solution to perform precipitation reaction to generate a single precursor solution, and simultaneously add 2L (0.5mol / L) of zinc chloride solution to be coated and an equimolar amount of oxalic acid solution to the single precursor solution to generate a coating salt precursor solution; Step S2: The coating salt precursor solution is filtered, dried, and sintered to obtain zinc oxide coated nickel powder, and finally washed with hydrochloric acid to remove the coating layer, rinsed with anhydrous ethanol, and dried at 65° C. in a vacuum atmosphere to obtain high-purity nickel powder; The preparation of the cobalt powder comprises the following steps: Step S3: Dissolve Co(Ac)2·4H2O (6.25 g 0.025 mol) in 50 mL of water, then add ethylenediaminetetraacetic acid (7.31 g 0.025 mol), heat, stir, dissolve, slowly dropwise add dilute NaOH solution, adjust the pH value of the mother solution to 1011, keep the temperature at 70°C, add 7 mL 85% hydrazine hydrate under uniform stirring, and continue the reaction for about 4 hours until the upper layer solution becomes colorless and transparent, and the lower layer is a gray powdery precipitate, filter, wash with distilled water, then wash with anhydrous ethanol and anhydrous ether, drain, and vacuum dry at below 40°C for 48 hours to obtain high-purity cobalt powder; The preparation of the tungsten carbide powder comprises the following steps: Step S4: carbon black is added with tungsten powder according to 4% to 6.13%, and the mixture is put into a ball mill tank for dry mixing, with a ball-to-material ratio of 1:1, and the mixture is ball milled for 6 hours. The mixed material is put into a cylindrical graphite crucible, loaded into a furnace, and nitrogen is introduced into the furnace to exhaust the air inside. After ensuring that the air in the furnace is exhausted, hydrogen is introduced and the exhausted hydrogen is ignited at the exhaust port of the furnace. The temperature is raised at the maximum power of the furnace, and the temperature reaches 2000° C. in about 1 hour, and then the temperature is kept for 5 hours. The power is turned off and the furnace is cooled for 18 hours before being taken out of the furnace. The tungsten carbide powder after carburization treatment is in the shape of a cylindrical block. After being crushed, it is ball milled for 30 minutes to obtain tungsten carbide powder; The preparation process steps of the nickel-cobalt based tungsten carbide wear-resistant powder are as follows: Step S5: Put the prepared high-purity nickel powder, high-purity cobalt powder and tungsten carbide powder into a mixer according to a preset ratio (1:1:1), mix them by airflow stirring to make the components fully and evenly distributed, and the powder after mixing evenly needs to be prepared by a molding process such as compression molding and static pressing molding, and the powder is compressed into a dense block. The formed block is sintered at a high temperature of 2000°C, and the sintered block is crushed into smaller particles, and a nickel-cobalt-based tungsten carbide wear-resistant powder is obtained by a screening process; The nickel-cobalt-based tungsten carbide wear-resistant powder supersonic flame thermal spraying method comprises the following steps: Step S6: cleaning, derusting and roughening the surface of the workpiece to be sprayed; Step S7: feeding the nickel-cobalt-based tungsten carbide wear-resistant powder into the spray gun of the supersonic flame spraying equipment. During the spraying process, the powder is heated to a molten or semi-molten state under the action of the supersonic flame, and impacts the surface of the workpiece at a high speed to form a dense coating.

2. The method for preparing nickel-cobalt-based tungsten carbide wear-resistant powder and supersonic flame thermal spraying according to claim 1, characterized in that: A plurality of steel balls are arranged inside the ball mill, and the diameter of the steel balls is 45 mm.

3. The method for preparing nickel-cobalt-based tungsten carbide wear-resistant powder and supersonic flame thermal spraying according to claim 1, characterized in that: The suction filtration device is composed of a suction filtration bottle, a funnel, a safety bottle, and a suction pump component, and filter paper is arranged in the funnel.

4. The method for preparing nickel-cobalt-based tungsten carbide wear-resistant powder and supersonic flame thermal spraying according to claim 1, characterized in that: The core step of the molding preparation process is to adopt a bidirectional pressing method.

5. The method for preparing nickel-cobalt-based tungsten carbide wear-resistant powder and supersonic flame thermal spraying according to claim 1, characterized in that: The air flow stirring is performed by using a bubbler, the tube wall of the bubbler is composed of a tube with multiple small holes, and the stirring achieves mixing of the powder through the movement of bubbles.

6. The method for preparing nickel-cobalt-based tungsten carbide wear-resistant powder and supersonic flame thermal spraying according to claim 1, characterized in that: During the supersonic flame thermal spraying, the distance between the spray gun and the workpiece was adjusted to 220 mm, the spraying angle was 60°, and the spraying speed was 500 m / s.

7. The method for preparing nickel-cobalt-based tungsten carbide wear-resistant powder and supersonic flame thermal spraying according to claim 1, characterized in that: When the carbonization temperature is 2000° C., the free carbon content is 0.015% and the combined carbon content is 6.6115%.

8. The method for preparing nickel-cobalt-based tungsten carbide wear-resistant powder and supersonic flame thermal spraying according to claim 1, characterized in that: The sintering temperature of the coating body salt precursor solution in a reducing atmosphere furnace is 900-1200°C.