Preparation method and application of transition metal sulfide catalyst

The transition metal sulfide catalyst is synthesized by hydrothermal method, and carbon nanotubes are used to enhance the conductivity and specific surface area, which solves the problem of high cost of precious metal catalysts, achieves efficient catalysis and stability of electrolysis of water for hydrogen production, and provides a cheap catalyst solution The plan expands the development ideas of catalysts for electrolyzing water to produce hydrogen.

CN118727042APending Publication Date: 2024-10-01KUNMING UNIV OF SCI & TECH
View PDF 0 Cites 0 Cited by

Patent Information

Application Number
CN202410784280.3
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Filing Date
2024-06-18
Publication Date
2024-10-01

AI Technical Summary

Technical Problem

The current precious metal catalysts used in the electrolysis of water to produce hydrogen are high in cost and scarce in resources, which limits the commercial application of hydrogen production in the electrolysis of water. It is necessary to develop efficient and cheap non-noble metal catalysts.

Method used

Transition metal sulfide catalysts are synthesized using a hydrothermal method, and carbon nanotubes are used as the substrate of the catalyst to enhance conductivity and specific surface area, improve catalytic activity, and prepare spherical Fe, Co or Cu sulfide catalysts for use in hydrogen evolution reactions. working electrode.

Benefits of technology

It has achieved excellent catalytic performance and stability in an alkaline environment, reduced the cost of hydrogen production by electrolysis of water, provided a cheap catalyst solution, and expanded the development ideas for future catalysts for hydrogen production by electrolysis of water.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN118727042A_ABST
    Figure CN118727042A_ABST
Patent Text Reader

Abstract

The invention discloses a preparation method and application of a transition metal sulfide catalyst, and is characterized in that the preparation method comprises the following steps: by taking acetic acid metal salt as a transition metal source, sodium thiosulfate as a sulfur source and a carbon nanotube as a material substrate, synthesizing a material by adopting a hydrothermal method, and preparing the carbon nanotube loaded transition metal sulfide catalyst; the transition metal sulfide catalyst is used for preparing a working electrode and can be applied to a hydrogen evolution reaction. The operation process is simple and easy to implement, the prepared material electrode has good electrochemical performance and stability, raw materials are cheap, easy to obtain and non-toxic, conditions are mild and controllable, and the material electrode is suitable for large-scale industrial production, can be directly used as an electrode for hydrogen evolution reaction through electro-catalytic water decomposition and can also be suitable for preparation of other transition metal sulfides.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The invention relates to the technical field of catalysts for producing hydrogen by electrolysis of water, and in particular to a preparation method of a transition metal sulfide catalyst and application thereof. Background Art

[0002] The continuous growth of fossil fuel consumption has led to a series of problems such as air pollution, energy shortage and global warming. Therefore, it is imperative to develop clean energy. Hydrogen energy has high energy density and is pollution-free. It is an excellent energy carrier and a potential candidate for future low-carbon energy systems. The hydrogen evolution reaction (HER) is one of the key processes that limits the efficiency of water splitting devices by electrochemically reducing water to generate molecular hydrogen.

[0003] At present, the main way to prepare hydrogen commercially is to reform fossil energy such as natural gas and coal to produce hydrogen. Although the cost is low, the carbon cycle cannot be avoided. Hydrogen production by water electrolysis has the advantages of being clean, efficient and sustainable. However, the catalysts currently used for hydrogen production by water electrolysis are precious metal catalysts, which leads to high costs for hydrogen production by water electrolysis. Precious metal-based catalysts (especially Pt-based catalysts) show good reaction rates for both HER and ORR. However, the scarcity of platinum metal resources, high cost and poor stability still hinder its practical application. In the future, in order to realize the commercial application of hydrogen production by water electrolysis, efficient and inexpensive non-precious metal catalysts must be developed.

[0004] Compared with precious metals such as Pt, Ru, and Ir, transition metals are stored in large quantities on Earth and have the characteristics of being cheap, low toxic, and having a wide range of applications. At present, electrocatalysts developed based on transition metals have been proven to be able to catalyze the HER reaction. Among them, catalysts synthesized based on Fe and Co or Cu have better catalytic effects. It is expected to further reduce the cost of hydrogen production from water electrolysis and hydrogen fuel cell catalysts; designing efficient catalysts based on abundant and cheap elements on Earth to promote HER catalysis is crucial for the development of new energy equipment in the future.

[0005] Therefore, the present invention provides a preparation method of a transition metal sulfide catalyst and application thereof. Summary of the invention

[0006] The purpose of the present invention is to provide a transition metal sulfide catalyst which is synthesized by a hydrothermal method and uses carbon nanotubes as a catalyst substrate, thereby enhancing its conductivity while increasing the specific surface area and carbon edge defects of the catalyst, so that the catalyst obtains more active sites, and synthesizes transition metal sulfides as catalytic active centers, thereby improving its catalytic activity; the prepared catalyst exhibits excellent catalytic performance and stability in an alkaline environment.

[0007] In order to achieve the above technical effects, the present invention is implemented by the following technical scheme: A method for preparing a transition metal sulfide catalyst, characterized in that it comprises the following steps:

[0008] S1. Weighing metal acetate, sodium thiosulfate, carbon nanotubes and deionized water as raw materials in a mass ratio of 1-2:1-2:5-10:50-100 = metal acetate: sodium thiosulfate: carbon nanotubes: deionized water;

[0009] S2. Add the obtained raw materials into a beaker and mix them evenly to obtain M x S y -CNT catalyst precursor solution;

[0010] S3, 50-100 ml of the precursor solution is transferred to a high-pressure reactor, and in an air atmosphere, a blast drying oven is used to reach a temperature of 160-200° C., and the reaction is carried out for 11-13 hours. After the reaction is completed, the temperature is cooled to room temperature, the solid part is filtered out and dried, and M x S y -CNT transition metal sulfide catalyst; wherein M = Fe, Co or Cu; x = 1, 2; y = 1, 2.

[0011] Furthermore, in S1, the metal acetate salt is one or more of ferric acetate, cobalt acetate or copper acetate.

[0012] Furthermore, in S3, the obtained M x S y The metal element content in the CNT transition metal sulfide catalyst is not less than 20%, the sulfur element exists in the form of sulfide with the metal element, and the catalyst morphology is spherical.

[0013] Another object of the present invention is to provide an application of a transition metal sulfide catalyst, characterized in that the transition metal sulfide catalyst is used to prepare a working electrode and is used in a hydrogen evolution reaction.

[0014] Furthermore, the transition metal sulfide catalyst is used to prepare a working electrode and is used in a hydrogen evolution reaction, and the steps are as follows:

[0015] A. Mix ultrapure water and 5% Nafion solution in a volume ratio of 9-18:1-2 to prepare a dispersed environment solution, and mix the prepared M x S y - The CNT transition metal sulfide catalyst sample is mixed with a dispersion environment solution to obtain a dispersion solution;

[0016] B. Ultrasonic dispersion of the dispersed solution for 1 hour to obtain a homogeneous catalyst ink. 30 μL of the dispersed solution was dropped on the surface of a glassy carbon electrode to form a working electrode. After natural drying, it was used for hydrogen evolution reaction.

[0017] C. The hydrogen evolution reaction was carried out in a 1.0 mol / L KOH electrolyte saturated with N2. When the pH of the KOH electrolyte was 14, the FeS2-CNT catalyst only needed 179 mV to reach 10 mA cm -2 of current density.

[0018] The beneficial effects of the present invention are:

[0019] The present invention uses cheap transition metals as raw materials, which solves the problem of high cost of precious metals. At the same time, the synthesis method is simple, the process is stable and reliable, and the operability is strong. The catalyst prepared according to this method shows excellent HER catalytic activity and stability, has certain application prospects, and can also be extended to other transition metals, providing new ideas for synthesizing catalysts for hydrogen production by electrolysis of water. BRIEF DESCRIPTION OF THE DRAWINGS

[0020] In order to more clearly illustrate the technical solutions of the embodiments of the present invention, the drawings required for describing the embodiments are briefly introduced below. Obviously, the drawings described below are only some embodiments of the present invention. For ordinary technicians in this field, other drawings can be obtained based on these drawings without creative work.

[0021] Figure 1 is an electron microscope image of the catalyst of Example 1 of the present invention;

[0022] Figure 2 is an electron microscope image of the catalyst of Example 2 of the present invention;

[0023] Figure 3 This is an electron microscope image of the catalyst of Example 3 of the present invention;

[0024] Figure 4 This is the X-ray diffraction pattern of the catalyst prepared in Example 1 of the present invention;

[0025] Figure 5 This is the X-ray diffraction pattern of the catalyst prepared in Example 2 of the present invention;

[0026] Figure 6 This is the X-ray diffraction pattern of the catalyst prepared in Example 3 of the present invention;

[0027] Figure 7 The LSV polarization curves of the three-electrode system described in Examples 1, 2 and 3 of the present invention. DETAILED DESCRIPTION

[0028] The following will be combined with the drawings in the embodiments of the present invention to clearly and completely describe the technical solutions in the embodiments of the present invention. Obviously, the described embodiments are only part of the embodiments of the present invention, not all of the embodiments. Based on the embodiments of the present invention, all other embodiments obtained by ordinary technicians in this field without creative work are within the scope of protection of the present invention.

[0029] Example 1

[0030] A method for preparing an iron sulfide catalyst (FeS2-CNT), the specific steps are as follows:

[0031] (1) Dissolve 0.1 g of ferric acetate, 0.1 g of sodium sulfite and 0.5 g of carbon nanotubes in 60 ml of deionized water and stir to mix well.

[0032] (2) Thereafter, the resulting solution was transferred into a 100 ml hydrothermal kettle and placed in an oven set at 180°C for 12 hours.

[0033] (3) Next, the product is filtered and dried.

[0034] (5) The product is washed with deionized water and ethanol to obtain a catalyst in which iron sulfide is supported on carbon nanotubes (FeS2-CNT).

[0035] Example 2

[0036] A method for preparing a cobalt sulfide catalyst (CoS-CNT), the specific steps are as follows:

[0037] (1) Dissolve 0.1 g of ferric acetate, 0.1 g of sodium sulfite and 0.5 g of carbon nanotubes in 60 ml of deionized water and stir to mix well.

[0038] (2) Thereafter, the resulting solution was transferred into a 100 ml hydrothermal kettle and placed in an oven set at 180°C for 12 hours.

[0039] (3) Next, the product is filtered and dried.

[0040] (5) The product is washed with deionized water and ethanol to obtain a catalyst in which cobalt sulfide is supported on carbon nanotubes (CoS-CNT).

[0041] Example 3

[0042] A method for preparing a copper sulfide catalyst (CuS-CNT), the specific steps are as follows:

[0043] (1) Dissolve 0.1 g of copper acetate, 0.1 g of sodium sulfite and 0.5 g of carbon nanotubes in 60 ml of deionized water and stir to mix well.

[0044] (2) Thereafter, the resulting solution was transferred into a 100 ml hydrothermal kettle and placed in an oven set at 180°C for 12 hours.

[0045] (3) Next, the product is filtered and dried.

[0046] (5) The product is washed with deionized water and ethanol to obtain a copper sulfide-supported carbon nanotube catalyst (CuS-CNT).

[0047] Example 4

[0048] The specific applications of FeS2-CNT, CoS-CNT and CuS-CNT prepared in Examples 1 to 3 were studied, and the electrochemical performance was tested using a three-electrode system. The specific method is as follows:

[0049] (1) The catalyst samples FeS2-CNT, CoS-CNT and CuS-CNT obtained in Examples 1, 2 and 3 were respectively used for experiments.

[0050] (2) Ultrapure water and Nafion solution (5%) were mixed in a ratio of 9:1 to prepare a dispersed environmental solution, and the sample and the dispersed solution were mixed in a ratio of 3 mg / ml to obtain a dispersed solution. The dispersed solution was ultrasonically dispersed for 1 h to obtain a homogeneous catalyst ink. 30 μL of the dispersed solution was taken and dropped on the surface of a glassy carbon electrode to prepare a working electrode. After natural drying, it was used for hydrogen evolution reaction.

[0051] (3) The hydrogen evolution reaction was carried out in a 1.0 mol / L KOH electrolyte saturated with N2, and the pH of the KOH electrolyte was 14.

[0052] (4) When the current density reaches 10 mA cm -2 When , the FeS2-CNT catalyst has the smallest starting potential and overpotential, which are 0.179 mV and 0.23 mV respectively. The starting points and overpotentials of the other two catalysts are greater than those of the FeS2-CNT catalyst.

[0053] 1. Electron Microscope Image Analysis

[0054] Figure 1 , 2 3 are electron microscope images of the transition metal sulfide catalysts prepared in Examples 1, 2 and 3 of the present invention. As can be seen from the figure, from the microscopic morphology analysis, the catalyst forms a small spherical shape, which increases the specific surface area.

[0055] 2. X-ray diffraction analysis

[0056] Figure 4 , 56 are X-ray diffraction patterns of the catalyst samples prepared in Examples 1, 2 and 3 of the present invention. As can be seen from the figure, the obtained catalytic material has both characteristic diffraction peaks of amorphous carbon materials and characteristic diffraction peaks of transition metal sulfides.

[0057] 3. Performance Analysis

[0058] Figure 7 The electrochemical performance diagram of the catalyst sample prepared by the present invention is shown in the figure. It can be seen from the figure that among the three catalysts prepared by the present invention, the electrochemical performance of the FeS2-CNT catalyst is the best, and it is the best catalyst among the samples.

Claims

1. A method for preparing a transition metal sulfide catalyst, characterized in that: The following steps are involved: S1. Weighing metal acetate, sodium thiosulfate, carbon nanotubes and deionized water as raw materials in a mass ratio of 1-2:1-2:5-10:50-100 = metal acetate: sodium thiosulfate: carbon nanotubes: deionized water; S2. Add the obtained raw materials into a beaker and mix them evenly to obtain M x S y -CNT catalyst precursor solution; S3, 50-100 ml of the precursor solution is transferred to a high-pressure reactor, and in an air atmosphere, a blast drying oven is used to reach a temperature of 160-200° C., and the reaction is carried out for 11-13 hours. After the reaction is completed, the temperature is cooled to room temperature, the solid part is filtered out and dried, and M x S y -CNT transition metal sulfide catalyst; wherein M = Fe, Co or Cu; x = 1, 2; y = 1, 2.

2. The method for preparing a transition metal sulfide catalyst according to claim 1, characterized in that: In S1, the metal acetate salt is one or more of ferric acetate, cobalt acetate or copper acetate.

3. The method for preparing a transition metal sulfide catalyst according to claim 1, characterized in that: In S3, the obtained M x S y The metal element content in the CNT transition metal sulfide catalyst is not less than 20%, the sulfur element exists in the form of sulfide with the metal element, and the catalyst morphology is spherical.

4. An application of a transition metal sulfide catalyst, characterized in that: The transition metal sulfide catalyst is used to prepare a working electrode and is applied in a hydrogen evolution reaction.

5. The use of a transition metal sulfide catalyst according to claim 4, characterized in that: The transition metal sulfide catalyst is used to prepare a working electrode and is applied in a hydrogen evolution reaction, and the steps are as follows: A. Mix ultrapure water and 5% Nafion solution in a volume ratio of 9-18:1-2 to prepare a dispersed environment solution, and mix the prepared M x S y - The CNT transition metal sulfide catalyst sample is mixed with a dispersion environment solution to obtain a dispersion solution; B. Ultrasonic dispersion of the dispersed solution for 1 hour to obtain a homogeneous catalyst ink. 30 μL of the dispersed solution was dropped on the surface of a glassy carbon electrode to form a working electrode. After natural drying, it was used for hydrogen evolution reaction. C. The hydrogen evolution reaction was carried out in a 1.0 mol / L KOH electrolyte saturated with N2. When the pH of the KOH electrolyte was 14, the FeS2-CNT catalyst only needed 179 mV to reach 10 mA cm -2 of current density.