High-corrosion-resistance bidirectional pulse nickel plating method
Bidirectional pulse nickel plating technology solves the problems of poor depth capability and high raw material consumption of DC nickel plating technology, achieves refinement and high corrosion resistance of nickel plating, and meets the needs of aerospace and other industries for high corrosion resistance.
Patent Information
- Application Number
- CN202410831668.4
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Filing Date
- 2024-06-26
- Publication Date
- 2024-10-01
Smart Images

Figure CN118727079A_ABST
Abstract
Description
Technical Field
[0001] The invention relates to the technical field of metal surface treatment, in particular to a high-corrosion-resistant bidirectional pulse nickel plating method. Background Art
[0002] Electroplating is a surface treatment technology that deposits a layer of metal or alloy on the surface of a base material (usually metal) through an electrolytic process. This process can enhance the corrosion resistance, wear resistance, decorative properties or conductivity of the base material.
[0003] With the continuous application of electroplating technology in various industries, it has also begun to be used in high-precision industries such as aerospace. Aerospace materials require high corrosion resistance to better resist corrosion in various media and atmospheric environments. Electroplating nickel on the surface of metal materials can enhance the corrosion resistance and wear resistance of metal materials and reduce hydrogen embrittlement problems. In the prior art, nickel plating mostly adopts direct current plating process. Direct current plating is a traditional electroplating technology that uses direct current to drive metal ions to deposit from the plating solution to the surface of the workpiece. Although direct current plating technology has the advantages of high maturity, stable plating solution, and easy control, the existing direct current nickel plating technology has poor depth capability and large raw material consumption, resulting in high cost and poor coating uniformity. Summary of the invention
[0004] Based on the above, the present invention aims to provide a method for bidirectional pulse nickel plating with high corrosion resistance. The method provided by the present invention can refine the grains of the nickel plating layer, achieve uniformity of the nickel plating layer, and achieve high corrosion resistance and good throwing power of the nickel plating layer.
[0005] In order to achieve the above object, the present invention provides the following technical solutions: a method for bidirectional pulse nickel plating with high corrosion resistance, which adopts a bidirectional pulse electroplating method to plate a metal material in an electroplating solution containing nickel elements;
[0006] The double pulse nickel plating process parameters in the plating are: plating temperature is 55±5°C; the forward pulse peak current density range is: 0.1~1.5A / dm 2 ; Reverse pulse peak current density range: 0.025~0.75A / dm 2 ; The frequency range is 50 to 2000 Hz; the duty cycle is set to 2 to 80%, and the plating time is 2 to 8 minutes.
[0007] Preferably, the electroplating solution containing nickel element contains nickel sulfamate, nickel chloride, boric acid and sodium dodecyl sulfate.
[0008] Further preferably, in the nickel-containing electroplating solution, the concentration of nickel sulfamate is 350 g / L, the concentration of nickel chloride is 15 g / L, the concentration of boric acid is 40 g / L, and the concentration of sodium dodecyl sulfate is 0.1 g / L.
[0009] Preferably, the pH of the electroplating solution containing nickel element is 4.15±0.35.
[0010] Preferably, the metal material comprises copper.
[0011] Preferably, before plating the metal material in the electroplating solution containing nickel element, the method further includes a step of pretreating the metal material.
[0012] Further preferably, the pretreatment is: subjecting the metal material to degreasing treatment, weak corrosion treatment, strong corrosion treatment and activation treatment in sequence.
[0013] Further preferably, the degreasing treatment is: immersing the metal material in degreasing powder to remove excess surface material; the weak corrosion treatment is: washing the degreased metal material with water, and immersing it in a dilute hydrochloric acid solution to remove surface oxides; the strong corrosion and activation treatment is: washing the metal material after the weak corrosion treatment with water, and immersing it in a dilute sulfuric acid solution to further remove the oxides on the substrate surface, and then activating it in a dilute hydrochloric acid solution.
[0014] Preferably, after the plating is completed, the process further includes the steps of taking the material out of the vat, washing the material after taking it out of the vat, and drying the material.
[0015] The present invention also provides a method for refining the grains of an electroplated nickel layer, and electroplating nickel is performed using the method described in the above technical solution.
[0016] Beneficial technical effects:
[0017] The method provided by the invention can refine the grains of the nickel plating layer, achieve the uniformity of the nickel plating layer, and achieve the high corrosion resistance and good throwing power of the nickel plating layer.
[0018] The method provided by the invention can change the structure of the coating, making the coating smooth and delicate; it can also improve the dispersion ability, making the coating thickness more uniform and the leveling property better.
[0019] The method provided by the invention can reduce the porosity of the coating, improve the toughness of the coating, improve the hardness and wear resistance of the coating, and reduce the impurity content of the coating.
[0020] The method provided by the invention can improve the bonding strength between the nickel plating layer and the substrate. BRIEF DESCRIPTION OF THE DRAWINGS
[0021] In order to more clearly illustrate the embodiments of the present invention or the technical solutions in the prior art, the drawings required for use in the embodiments will be briefly introduced below. Obviously, the drawings described below are only some embodiments of the present invention. For ordinary technicians in this field, other drawings can be obtained based on these drawings without paying creative work.
[0022] Figure 1 The scanning electron microscope images of the nickel coating obtained in Example 1, wherein A and A' are respectively the peak current density of the forward pulse at different magnifications of 0.75 A / dm 2 , control the reverse pulse peak current density to 0.11A / dm 2 Nickel coating obtained under different magnifications; B and B' are the forward pulse peak current density of 0.75A / dm 2 , control the reverse pulse peak current density to 0.2A / dm 2 Nickel coating obtained under the conditions.
[0023] Figure 2 The scanning electron microscope images of the nickel coating obtained in Example 2, wherein A and A' are respectively the forward current density of 0.75A / dm at different magnifications. 2 , control the reverse current density to 0.2A / dm 2 The nickel coating obtained under the conditions; B and B' are the forward current density of 1.25A / dm under different magnifications. 2 , control the reverse current density to 0.2A / dm 2 Nickel coating obtained under the conditions.
[0024] Figure 3 The scanning electron microscope images of the nickel coating obtained in Comparative Example 1, wherein A and A' are the pulse peak current density of 0.25A / dm at different magnifications. 2 Nickel coating obtained under different magnifications; B and B' are the peak current density of the pulse at 0.75A / dm 2 Nickel coating obtained under different magnifications; C and C' are the peak current density of the pulse at 1.5A / dm 2 Nickel coating obtained under the conditions.
[0025] Figure 4 The scanning electron microscope images of the nickel-plated test piece obtained in Comparative Example 1 after 196 hours of corrosion resistance test, wherein A and A' are the pulse peak current density of 0.25A / dm at different magnifications. 2 Nickel coating obtained under different magnifications; B and B' are the peak current density of the pulse at 1.5A / dm 2 Nickel coating obtained under the conditions.
[0026] Figure 5 The scanning electron microscope images of the nickel-plated test piece obtained in Example 1 after a 196-hour corrosion resistance test, wherein A and A' are respectively the peak current density of the forward pulse at different magnifications of 0.75 A / dm 2 , control the reverse pulse peak current density to 0.11A / dm 2 Nickel coating obtained under different magnifications; B and B' are the forward pulse peak current density of 0.75A / dm 2 , control the reverse pulse peak current density to 0.2A / dm 2 Nickel coating obtained under the conditions. DETAILED DESCRIPTION
[0027] Various exemplary embodiments of the present invention will now be described in detail. This detailed description should not be considered as limiting the present invention, but should be understood as a more detailed description of certain aspects, features, and embodiments of the present invention.
[0028] It should be understood that the terms described in the present invention are only for describing a particular embodiment and are not intended to limit the present invention. In addition, for the numerical range in the present invention, it should be understood that each intermediate value between the upper and lower limits of the scope is also specifically disclosed. The intermediate value in any stated value or stated range, and each smaller range between any other stated value or intermediate value in the described range is also included in the present invention. The upper and lower limits of these smaller ranges can be independently included or excluded in the scope.
[0029] Unless otherwise indicated, all technical and scientific terms used herein have the same meanings as those generally understood by those skilled in the art. Although the present invention describes only preferred methods and materials, any methods and materials similar or equivalent to those described herein may also be used in the implementation or testing of the present invention. All documents mentioned in this specification are incorporated by reference to disclose and describe the methods and / or materials associated with the documents. In the event of a conflict with any incorporated document, the content of this specification shall prevail.
[0030] It will be apparent to those skilled in the art that various modifications and variations may be made to the specific embodiments of the present invention description without departing from the scope or spirit of the present invention. Other embodiments derived from the present invention description will be apparent to the skilled artisan. The present invention description and examples are exemplary only.
[0031] The words “include,” “including,” “have,” “contain,” etc. used in this document are open-ended terms, meaning including but not limited to.
[0032] The present invention provides a method for bidirectional pulse nickel plating with high corrosion resistance, which specifically comprises the following steps:
[0033] S1. Preparation of a nickel-containing electroplating solution: the electroplating solution is composed of 350 g / L nickel sulfamate, 15 g / L nickel chloride, 40 g / L boric acid and 0.1 g / L sodium dodecyl sulfate; the pH of the electroplating solution is 4.15 ± 0.35;
[0034] S2. Pre-treat the metal test piece (preferably a copper test piece):
[0035] S2.1. Degreasing: Soak the metal test piece in degreasing powder and clean it for 40 minutes to remove excess material on the surface.
[0036] S2.2. Weak corrosion: After the degreased metal specimen is washed with water, it is immersed in a dilute hydrochloric acid solution to remove the oxide on the surface; the concentration of the dilute hydrochloric acid is 400 ml / L; the immersion time is 45 seconds;
[0037] S2.3. Strong corrosion and activation: After the weak corrosion treatment, the metal test piece is washed with water, immersed in a dilute sulfuric acid solution, and then rinsed with water to further remove the oxide on the surface of the substrate, and then activated in a dilute hydrochloric acid solution; the concentration of the dilute sulfuric acid is 10wt%; the immersion time is 45s; the concentration of the dilute hydrochloric acid is 400ml / L; the activation time is 45s;
[0038] S3. Plating: Plating temperature is 55±5℃, double pulse process parameters: forward pulse peak current density range is: 0.1~1.5A / dm 2 ; Reverse pulse peak current density range: 0.025~0.75A / dm 2 ; The frequency range is 50 to 2000 Hz; the duty cycle is set to 2 to 80%, and the plating time is 2 to 8 minutes; the pretreated metal material is transferred into the nickel-containing electroplating solution for plating.
[0039] S4. Post-treatment after leaving the cylinder: the plating thickness meets 2-5μm. After leaving the cylinder, two cold water washes and one hot water wash are carried out, and the product is obtained after being transferred to a 70℃ oven for drying.
[0040] In order to better understand the present invention, the content of the present invention is further explained below in conjunction with the embodiments, but the content of the present invention is not limited to the following embodiments.
[0041] The metal test pieces described in the embodiments are all Hull cell copper test pieces.
[0042] The degreasing powder used in the embodiments of the present invention is purchased Lcx degreasing agent.
[0043] Example 1
[0044] The method for electroplating nickel on the surface of a copper test piece in this embodiment specifically includes the following steps:
[0045] S1. Preparation of a nickel-containing electroplating solution: the electroplating solution consists of 350 g / L nickel sulfamate, 15 g / L nickel chloride, 40 g / L boric acid and 0.1 g / L sodium dodecyl sulfate; the pH of the electroplating solution is 4.15 (pH is adjusted by adding dilute sulfuric acid);
[0046] S2. Pretreatment of the Hull cell copper test piece:
[0047] S2.1. Degreasing: Soak the Hull cell copper specimen in degreasing powder and clean for 40 minutes to remove excess material on the surface;
[0048] S2.2. Weak corrosion: After the degreased copper specimen is washed with tap water and pure water, it is immersed in a 400 ml / L dilute hydrochloric acid solution for 45 seconds to remove the surface oxide;
[0049] S2.3. Strong corrosion and activation: After the weak corrosion treatment, the metal specimen was washed with tap water and pure water, immersed in a 10wt% dilute sulfuric acid solution for 45s, and then rinsed with tap water to further remove the oxide on the substrate surface, and then activated in a 400ml / L dilute hydrochloric acid solution for 45s;
[0050] S3. Plating: Plating temperature is 50℃, double pulse process parameters: forward pulse peak current density range is: 0.75A / dm 2 ; Reverse pulse peak current density: 0.025, 0.05, 0.08, 0.11, 0.15, 0.2, 0.25, 0.5, 0.75A / dm 2 ; The frequency range is 1000 Hz; The duty cycle is set to 60%, and the plating time is 3 minutes; The pretreated metal material is transferred into the nickel-containing electroplating solution for plating.
[0051] S4. Post-treatment after leaving the cylinder: the plating thickness meets 2-5μm. After leaving the cylinder, two cold water washes and one hot water wash are carried out, and the product is obtained after being transferred to a 70℃ oven for drying.
[0052] Example 2
[0053] The method for electroplating nickel on the surface of a copper test piece in this embodiment specifically includes the following steps:
[0054] S1. Preparation of a nickel-containing electroplating solution: the electroplating solution consists of 350 g / L nickel sulfamate, 15 g / L nickel chloride, 40 g / L boric acid and 0.1 g / L sodium dodecyl sulfate; the pH of the electroplating solution is 3.8 (pH is adjusted by dropping dilute sulfuric acid);
[0055] S2. Pre-treatment of the Hull cell copper test piece:
[0056] S2.1. Degreasing: Soak the Hull cell copper specimen in degreasing powder and clean for 40 minutes to remove excess material on the surface;
[0057] S2.2. Weak corrosion: After the degreased copper specimen is washed with tap water and pure water, it is immersed in a 400 ml / L dilute hydrochloric acid solution for 45 seconds to remove the surface oxide;
[0058] S2.3. Strong corrosion and activation: After the weak corrosion treatment, the metal specimen was washed with tap water and pure water, immersed in a 10wt% dilute sulfuric acid solution for 45s, and then rinsed with tap water to further remove the oxide on the substrate surface, and then activated in a 400ml / L dilute hydrochloric acid solution for 45s;
[0059] S3. Plating: Plating temperature is 55°C, double pulse process parameters: forward pulse peak current density is: 0.1, 0.3, 0.5, 0.75, 1, 1.25, 1.5A / dm 2 ; Reverse pulse peak current density range: 0.2A / dm 2 ; The frequency range is 800 Hz; The duty cycle is set to 2%, and the plating time is 4 minutes; The pretreated metal material is transferred into the nickel-containing electroplating solution for plating.
[0060] S4. Post-treatment after leaving the cylinder: the plating thickness meets 2-5μm. After leaving the cylinder, two cold water washes and one hot water wash are carried out, and the product is obtained after being transferred to a 70℃ oven for drying.
[0061] Example 3
[0062] The method for electroplating nickel on the surface of a copper test piece in this embodiment specifically includes the following steps:
[0063] S1. Preparation of a nickel-containing electroplating solution: the electroplating solution consists of 350 g / L nickel sulfamate, 15 g / L nickel chloride, 40 g / L boric acid and 0.1 g / L sodium dodecyl sulfate; the pH of the electroplating solution is 3.8 (pH is adjusted by dropping dilute sulfuric acid);
[0064] S2. Pre-treatment of the Hull cell copper test piece:
[0065] S2.1. Degreasing: Soak the Hull cell copper specimen in degreasing powder and clean for 40 minutes to remove excess material on the surface;
[0066] S2.2. Weak corrosion: After the degreased copper specimen is washed with tap water and pure water, it is immersed in a 400 ml / L dilute hydrochloric acid solution for 45 seconds to remove the surface oxide;
[0067] S2.3. Strong corrosion and activation: After the weak corrosion treatment, the metal specimen was washed with tap water and pure water, immersed in a 10wt% dilute sulfuric acid solution for 45s, and then rinsed with tap water to further remove the oxide on the substrate surface, and then activated in a 400ml / L dilute hydrochloric acid solution for 45s;
[0068] S3. Plating: Plating temperature is 50℃, double pulse process parameters: forward pulse peak current density range is: 0.75A / dm 2 ; Reverse pulse peak current density range: 0.11A / dm 2 The frequency range is 1000 Hz; the duty cycle is set to 2%, 5%, 7%, 10%, 15%, 20%, 25%, 30%, 40%, 60%, 70%, 80%, and the plating time is 3 minutes; the pretreated metal material is transferred into the nickel-containing electroplating solution for plating.
[0069] S4. Post-treatment after leaving the cylinder: the plating thickness meets 2-5μm. After leaving the cylinder, two cold water washes and one hot water wash are carried out, and the product is obtained after being transferred to a 70℃ oven for drying.
[0070] Example 4
[0071] The method for electroplating nickel on the surface of a copper test piece in this embodiment specifically includes the following steps:
[0072] S1. Preparation of a nickel-containing electroplating solution: the electroplating solution is composed of 350 g / L nickel sulfamate, 15 g / L nickel chloride, 40 g / L boric acid and 0.1 g / L sodium dodecyl sulfate; the pH of the electroplating solution is 4.45 (pH is adjusted by dropping a dilute sodium hydroxide solution);
[0073] S2. Pretreatment of the Hull cell copper test piece:
[0074] S2.1. Degreasing: Soak the Hull cell copper specimen in degreasing powder and clean for 40 minutes to remove excess material on the surface;
[0075] S2.2. Weak corrosion: After the degreased copper specimen is washed with tap water and pure water, it is immersed in a 400 ml / L dilute hydrochloric acid solution for 45 seconds to remove the surface oxide;
[0076] S2.3. Strong corrosion and activation: After the weak corrosion treatment, the metal specimen was washed with tap water and pure water, immersed in a 10wt% dilute sulfuric acid solution for 45s, and then rinsed with tap water to further remove the oxide on the substrate surface, and then activated in a 400ml / L dilute hydrochloric acid solution for 45s;
[0077] S3. Plating: Plating temperature is 60℃, double pulse process parameters: forward pulse peak current density range is: 0.75A / dm 2 ; Reverse pulse peak current density range: 0.11A / dm 2 The frequencies are 50, 100, 200, 500, 800, 1000 and 2000 Hz respectively; the duty cycle is set to 2% and the plating time is 4 min; the pretreated metal material is transferred into the nickel-containing electroplating solution for plating.
[0078] S4. Post-treatment after leaving the cylinder: the plating thickness meets 2-5μm. After leaving the cylinder, two cold water washes and one hot water wash are carried out, and the product is obtained after being transferred to a 70℃ oven for drying.
[0079] Comparative Example 1
[0080] The method for electroplating nickel on the surface of the copper test piece in this comparative example specifically comprises the following steps:
[0081] S1. Preparation of a nickel-containing electroplating solution: the electroplating solution consists of 350 g / L nickel sulfamate, 15 g / L nickel chloride, 40 g / L boric acid and 0.1 g / L sodium dodecyl sulfate; the pH of the electroplating solution is 3.8 (pH is adjusted by dropping dilute sulfuric acid);
[0082] S2. Pre-treatment of the Hull cell copper test piece:
[0083] S2.1. Degreasing: Soak the Hull cell copper specimen in degreasing powder and clean for 40 minutes to remove excess material on the surface;
[0084] S2.2. Weak corrosion: After the degreased copper specimen is washed with tap water and pure water, it is immersed in a 400 ml / L dilute hydrochloric acid solution for 45 seconds to remove the surface oxide;
[0085] S2.3. Strong corrosion and activation: After the weak corrosion treatment, the metal specimen was washed with tap water and pure water, immersed in a 10wt% dilute sulfuric acid solution for 45s, and then rinsed with tap water to further remove the oxide on the substrate surface, and then activated in a 400ml / L dilute hydrochloric acid solution for 45s;
[0086] S3. Plating: Plating temperature is 60°C, single pulse process parameters: pulse peak current density is 0.25, 0.75, 1.5A / dm 2 ; The frequency is 2000 Hz; The duty cycle is set to 60%, and the plating time is 8 minutes; The pretreated metal material is transferred into the nickel-containing electroplating solution for plating.
[0087] S4. Post-treatment after leaving the cylinder: the plating thickness meets 2-5μm. After leaving the cylinder, two cold water washes and one hot water wash are carried out, and the product is obtained after being transferred to a 70℃ oven for drying.
[0088] The coatings obtained in Examples 1, 2 and Comparative Example 1 were analyzed by scanning electron microscope. Figure 1-3 As shown in the figure, it can be seen that the coating thickness increases first and then decreases with the increase of the reverse average current density. The thickness is uniform and less than 5μm. The density increases with the increase of the reverse average current density, and the grains are fine. As the forward average current density increases from 0.75A / dm 2 Increase to 1.25A / dm 2 As the coating thickness increases, the grain size increases, and the surface density decreases. The shape of the Ni grains shows a classic cone. As the average current density increases from 0.25A / dm 2 Increase to 1.5A / dm 2 As the coating thickness increases, the grain size increases, and the surface density decreases; the shape of the Ni grains shows a classic cone. 2+ Consumption rate and Ni content in bulk solution 2+ The difference in diffusion rate forms local ion-deficient areas.
[0089] Corrosion resistance test: Electroplated test pieces under different conditions (Comparative Example 1 and Example 1) were immersed in a 3.5% sodium chloride solution for 196 hours, and then photographed with a scanning electron microscope to observe whether there were other impurities on the surface. The results are shown in Figure 4 and Figure 5 As can be seen from the figure, fine particles appear around the grains on the surface of the single-pulse plated part, and no obvious grain precipitation is observed in the double-pulse process coating, indicating that the corrosion resistance of the double-pulse plated part is better.
[0090] The coating performance of Examples 1-4 was tested: the coating performance test included scanning electron microscope photos of the coating, corrosion resistance scanning pictures, etc. The test pieces used in the test were all made of brass, with a specification of 65×100×0.3mm, and three test pieces were used for each test item. At the same time, it was compared with the unidirectional pulse nickel plating sample (Comparative Example 1). The corrosion potential of the unidirectional pulse nickel plating is between 0.3-0.45V; the corrosion potential of the bidirectional pulse nickel plating is between 0.2-0.35V. Therefore, bidirectional pulse nickel plating can improve the corrosion resistance of the coating.
[0091] The above is only a preferred embodiment of the present invention. It should be pointed out that for ordinary technicians in this technical field, several improvements and modifications can be made without departing from the principle of the present invention. These improvements and modifications should also be regarded as the scope of protection of the present invention.
Claims
1. A method for bidirectional pulse nickel plating with high corrosion resistance, characterized in that: A bidirectional pulse electroplating method is used to plate the metal material in an electroplating solution containing nickel elements; The double pulse nickel plating process parameters in the plating are: plating temperature is 55±5°C; the forward pulse peak current density range is: 0.1~1.5A / dm 2 ; Reverse pulse peak current density range: 0.025~0.75A / dm 2 ; The frequency range is 50 to 2000 Hz; the duty cycle is set to 2 to 80%, and the plating time is 2 to 8 minutes.
2. The method for bidirectional pulse nickel plating with high corrosion resistance according to claim 1, characterized in that: The electroplating solution containing nickel element contains nickel sulfamate, nickel chloride, boric acid and sodium dodecyl sulfate.
3. The method for bidirectional pulse nickel plating with high corrosion resistance according to claim 2, characterized in that: In the nickel-containing electroplating solution, the concentration of nickel sulfamate is 350 g / L, the concentration of nickel chloride is 15 g / L, the concentration of boric acid is 40 g / L, and the concentration of sodium dodecyl sulfate is 0.1 g / L.
4. The method for bidirectional pulse nickel plating with high corrosion resistance according to claim 1, characterized in that: The pH of the electroplating solution containing nickel element is 4.15±0.
35.
5. The method for bidirectional pulse nickel plating with high corrosion resistance according to claim 1, characterized in that: The metal material includes copper.
6. The method for bidirectional pulse nickel plating with high corrosion resistance according to claim 1, characterized in that: Before plating the metal material in the electroplating solution containing nickel element, the method also includes the step of pre-treating the metal material.
7. The method for bidirectional pulse nickel plating with high corrosion resistance according to claim 6, characterized in that: The pretreatment is: subjecting the metal material to degreasing treatment, weak corrosion treatment, strong corrosion treatment and activation treatment in sequence.
8. The method for bidirectional pulse nickel plating with high corrosion resistance according to claim 7, characterized in that: The degreasing treatment is as follows: immersing the metal material in degreasing powder to remove excess material on the surface; the weak corrosion treatment is as follows: washing the degreasing metal material with water, and then immersing it in a dilute hydrochloric acid solution to remove surface oxides; the strong corrosion and activation treatment is as follows: washing the metal material after the weak corrosion treatment with water, and then immersing it in a dilute sulfuric acid solution to further remove oxides on the substrate surface, and then activating it in a dilute hydrochloric acid solution.
9. The method for bidirectional pulse nickel plating with high corrosion resistance according to claim 1, characterized in that: After the plating is completed, the process also includes the steps of taking the material out of the vat, washing it with water and drying it.
10. A method for refining the grain size of an electroplated nickel layer, characterized in that: The method according to claim 1 is used for nickel electroplating.
Citation Information
Cited By
Method for preparing pulse gold-quantum dot composite coating with low cost and high corrosion resistance and wear resistance
CN122669447A