Homogenizing preparation method for micro-arc oxidation coating of large-size thin-wall part
By installing the inner cavity structure of large-sized thin-walled parts on the stainless steel cathode screen and coinciding with the central axis of the auxiliary device, an additional electric field is constructed, which solves the problem of uneven coating caused by uneven electric field during the micro-arc oxidation process, and achieves large-scale The uniform preparation of micro-arc oxidation coatings on the surface of thin-walled parts improves the uniformity of the electric field and the stability of the coating.
Patent Information
- Application Number
- CN202410996390.6
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Filing Date
- 2024-07-24
- Publication Date
- 2024-10-01
AI Technical Summary
During the micro-arc oxidation process, the coating thickness in the inner cavity area of large-sized thin-walled parts is low and uneven, resulting in uneven electric field distribution and difficulty in achieving uniform surface treatment.
By installing the inner cavity structure of large-sized thin-walled parts on the stainless steel cathode screen and coinciding with the central axis of the auxiliary device, an additional electric field is constructed to ensure uniform distribution of the electric field on the inner and outer surfaces. The auxiliary device assembly and electrolyte circulation pump and filter are used and other devices to improve electric field stability.
It realizes the uniform preparation of micro-arc oxidation coating on the surface of large-sized thin-walled parts, improves the uniformity of electric field on the inner and outer surfaces and the stability of coating thickness, reduces production costs, and is suitable for large-scale industrial applications.
Smart Images

Figure CN118727094A_ABST
Abstract
Description
Technical Field
[0001] The invention belongs to the technical field of micro-arc oxidation, and in particular relates to a method for homogenizing a micro-arc oxidation coating on a large-sized thin-walled component. Background Art
[0002] Micro-arc oxidation (MAO), also known as plasma spark deposition, is a surface treatment process that relies on the instantaneous high temperature and high pressure generated by arc discharge on the surface of aluminum, magnesium, titanium and their alloys by mixing electrolyte and corresponding electrical parameters to grow a ceramic film layer mainly composed of matrix metal oxide. It has extremely broad application prospects in the fields of machinery, automobile, national defense, electronics, aerospace, construction and civil engineering. However, for the integrated and complex parts obtained by additive manufacturing, it is easy to cause problems of uneven surface coating and ablation. For example, the complex thin-walled integrated structure devices prepared by 3D printing, compared with the devices with smooth surface structures of traditional machined surfaces, 3D printed devices often increase the complexity of parts due to the characteristics of rough surface and complex surface structure. Therefore, when micro-arc oxidation is performed on large-sized thin-walled parts, the film thickness of the micro-arc oxidation in the inner cavity of the device is much lower than the film layer on the outer surface, and the inner hole area is often accompanied by uneven film thickness. Usually in the process of micro-arc oxidation, the workpiece to be processed and the corresponding electrode are mostly relatively static and immersed in the electrolyte, so that a ceramic coating is generated on the surface of the workpiece to be processed opposite to the electrode. When the size of the workpiece to be processed increases and the surface becomes more complicated, the electric field distribution in the solution will become uneven, making it difficult to achieve uniform surface treatment over a large area. Summary of the invention
[0003] The technical problem to be solved by the present invention is to provide a method for uniformly preparing micro-arc oxidation coatings for large-sized thin-walled parts in view of the deficiencies of the above-mentioned prior art. The method constructs an additional electric field by adding an auxiliary device, and adopts a placement method in which the inner cavity structure of the large-sized thin-walled parts is mounted on a stainless steel cathode screen and coincides with the central axis of the auxiliary device, thereby improving the electric field strength of the inner cavity structure to ensure that the electric field on the inner and outer surfaces of the large-sized thin-walled parts is uniformly distributed, achieving uniform preparation of micro-arc oxidation coatings on the surfaces of large-sized thin-walled parts, and solving the problem that it is difficult to achieve uniform coating preparation on the surfaces of large-sized workpieces.
[0004] In order to solve the above technical problems, the technical solution adopted by the present invention is: a method for preparing a uniform micro-arc oxidation coating of a large-sized thin-walled component, characterized in that the method comprises the following steps:
[0005] Step 1, assembling the auxiliary device: installing a pair of cathode plates near opposite tank walls inside the auxiliary electrolyte tank, and the pair of cathode plates are respectively fixed at both ends of the cathode fixing plate located at the bottom of the auxiliary electrolyte tank, fixing the stainless steel cathode screen on the cathode fixing plate, and the upper outlet of the stainless steel cathode screen is connected to the lower inlet through a hose, installing an electrolyte circulation pump on the hose, and adding an electrolyte filter on the hose near the lower inlet, and the electrolyte circulation pump and the electrolyte filter are both located outside the auxiliary electrolyte tank, and then installing an anode fixing frame with an anode conductive wire above the auxiliary electrolyte tank to obtain an assembled auxiliary device;
[0006] Step 2, preparation of micro-arc oxidation coating: placing large-sized thin-walled parts in a mixed solution prepared by deionized water and a detergent for ultrasonic cleaning, and rinsing with deionized water to obtain the treated large-sized thin-walled parts, and then the inner cavity structure of the treated large-sized thin-walled parts is mounted on the stainless steel cathode screen in the auxiliary device assembled in step 1, and the central axis coincides with the central axis of the auxiliary device, and then connected to the anode conductive wire on the anode fixing frame, and the whole is transferred into the electrolyte so that the electrolyte covers the treated large-sized thin-walled parts, and the coating is prepared by micro-arc oxidation. After cleaning with deionized water, the water stains are blown dry with compressed air, and then cleaned with ethanol to obtain large-sized thin-walled parts with a uniform coating.
[0007] Since the large-sized thin-walled parts are larger in size and more complex in structure, the cathode plate in the micro-arc oxidation has a large electric field strength and concentrated distribution around the periphery of the large-sized thin-walled parts. However, as the ceramic coating is generated on the surface of the outer wall of the large-sized thin-walled parts opposite to the cathode, the outer surface of the large-sized thin-walled parts will inevitably shield a part of the electric field of the inner surface, so that the electric field strength of the inner cavity structure area is reduced, resulting in uneven electric field of the parts as a whole, and a large difference in film formation rate, thereby causing the problem of uneven coating. The present invention adopts an auxiliary device in the conventional micro-arc oxidation process, and usually adjusts the position and size of the auxiliary device according to the size of the large-sized thin-walled parts. By putting the inner cavity structure of the processed large-sized thin-walled parts on the stainless steel cathode screen and coinciding with the central axis of the auxiliary device, the uniformity of the distance between the auxiliary device and the inner wall in the inner cavity structure of the large-sized thin-walled parts is achieved, thereby ensuring the uniform distribution and stability of the electric field strength of the inner wall in the inner cavity structure of the large-sized thin-walled parts, and finally realizing the uniform preparation of the surface coating of the large-sized thin-walled parts.
[0008] The above-mentioned method for preparing a uniform micro-arc oxidation coating of a large-sized thin-walled component is characterized in that the interior of the stainless steel cathode screen described in step one is a hollow structure, the size of the stainless steel cathode screen is half the size of the inner cavity structure of the large-sized thin-walled component described in step two, and the upper outlet and lower inlet of the stainless steel cathode screen are both provided with a protruding interface connected to a hose. The present invention ensures that there is enough space between the two by designing the interior of the stainless steel cathode screen as a hollow structure, and the size of the stainless steel cathode screen is usually half the diameter of the inner cavity structure size of the large-sized thin-walled component, so as to facilitate the circulation of the electrolyte in the inner cavity area, facilitate the electrolyte to fully contact the inner cavity of the large-sized thin-walled component mounted thereon through the stainless steel cathode screen, and improve the stability of the electric field; by setting a protruding interface to connect with the hose, it is convenient for the electrolyte to enter and exit the interface for exchange and circulation cooling, and stabilize the electrolyte temperature and solution composition uniformity in the inner cavity area of the component.
[0009] The above-mentioned method for preparing a uniform micro-arc oxidation coating for a large-sized thin-walled component is characterized in that a fixing plate is provided at the lower end of the stainless steel cathode screen in step 1, a stainless steel fixing rod with a long round rod structure is fixedly connected to the cathode fixing plate at the position corresponding to the fixing plate, a threaded interface is provided on the upper side of the stainless steel fixing rod, and the stainless steel fixing rod is fixed to the fixing plate by a stainless steel bolt. The above-mentioned arrangement improves the structural stability of the stainless steel cathode screen and facilitates subsequent disassembly and replacement.
[0010] The above-mentioned method for preparing a uniform micro-arc oxidation coating for a large-sized thin-walled component is characterized in that the hose described in step 1 is a low-density high-pressure polyethylene hose. Usually, the electrolyte used in micro-arc oxidation is alkaline, so a low-density high-pressure polyethylene hose with high chemical stability and good alkali resistance is selected to improve the hose's corrosion resistance to the electrolyte and ensure the long-term stability of the auxiliary equipment.
[0011] The above-mentioned method for preparing a homogenized micro-arc oxidation coating for a large-sized thin-walled component is characterized in that the electrolyte filter in step 1 has a stainless steel filter mesh inside. By setting a stainless steel filter mesh inside the electrolyte filter to filter out impurities in the sent electrolyte and then re-send it to the stainless steel cathode screen to participate in micro-arc oxidation, the purity of the electrolyte in the inner cavity of the large-sized thin-walled component is improved, and impurities are prevented from entering the electrolyte to affect the quality of the micro-arc oxidation film layer formed in the inner cavity.
[0012] The above-mentioned method for preparing a uniform micro-arc oxidation coating for a large-sized thin-walled component is characterized in that the electrolyte circulation pump in step 1 adopts an alkali-resistant motor and is equipped with a solution flow control valve. The solution flow control valve is prepared in the electrolyte circulation pump to adjust the electrolyte flow entering the rusty steel cathode screen to ensure the stability of the electrolyte circulation.
[0013] Compared with the prior art, the present invention has the following advantages:
[0014] 1. Aiming at the problem of uneven coating prepared by micro-arc oxidation due to uneven electric field at the outer wall and inner cavity of large-sized thin-walled parts, the present invention, under the premise of fixing the electrolyte system and micro-arc oxidation process parameters, constructs an additional electric field by adding an auxiliary device, and adopts a placement method in which the inner cavity structure of the large-sized thin-walled parts is sleeved on a stainless steel cathode screen and coincides with the central axis of the auxiliary device, thereby improving the electric field strength of the inner cavity structure to ensure that the electric field on the inner and outer surfaces of the large-sized thin-walled parts is evenly distributed, thereby realizing the uniform preparation of micro-arc oxidation coatings on the surfaces of large-sized thin-walled parts.
[0015] 2. The auxiliary device adopted in the present invention is simple to assemble. By connecting the fixing plate at the lower end of the stainless steel cathode screen to the stainless steel fixing rod of the cathode fixing plate through bolts, the stability of the stainless steel cathode screen in the inner cavity structure of large-sized thin-walled parts is improved, and it is easy to disassemble. Stainless steel cathode screens of different sizes can be replaced according to the different inner cavity structures of large-sized thin-walled parts, thereby improving the electric field distribution in the inner cavity structure area of the large-sized thin-walled parts, making the internal and external current distribution uniform, ensuring the uniformity of the micro-arc oxidation coating in the inner cavity, and then significantly improving the thickness stability of the coating.
[0016] 3. The preparation process of the present invention is simple, operable, and has low production cost, which is conducive to large-scale industrial application.
[0017] The technical solution of the present invention is further described in detail below through the accompanying drawings and embodiments. BRIEF DESCRIPTION OF THE DRAWINGS
[0018] Figure 1 It is a schematic diagram of the assembly of the auxiliary device and the large-sized thin-walled parts in the present invention.
[0019] Figure 2 for Figure 1 Enlarged view of point A in the middle.
[0020] Figure 3 This is a physical picture of the coating prepared on the surface of a large-sized thin-walled component in Example 1 of the present invention.
[0021] Figure 4 This is a physical picture of the coating prepared on the surface of a large-sized thin-walled component in Comparative Example 1 of the present invention.
[0022] Description of Reference Numerals
[0023] 1—auxiliary electrolyte tank; 2—cathode plate; 3—cathode fixing plate;
[0024] 4—stainless steel fixing rod; 5—anode fixing frame; 6—anode conductive wire;
[0025] 7—Large-size thin-walled parts; 8—Stainless steel cathode screen; 9—Hose;
[0026] 10—electrolyte filter; 11—electrolyte circulation pump; 12—fixed plate;
[0027] 13—Stainless steel bolts. DETAILED DESCRIPTION
[0028] Example 1
[0029] This embodiment includes the following steps:
[0030] Step 1: Assemble auxiliary devices: Figure 1 and Figure 2 As shown, a pair of cathode plates 2 are installed near the opposite tank walls inside the auxiliary electrolyte tank 1, and the pair of cathode plates 2 are respectively fixed at the two ends of the cathode fixing plate 3 located at the bottom of the auxiliary electrolyte tank 1, and a fixing plate 12 is provided at the lower end of the stainless steel cathode screen 8 with a hollow structure inside, and a stainless steel fixing rod 4 with a long round rod structure is fixedly connected at the position corresponding to the fixing plate 12 on the cathode fixing plate 3, and a threaded interface is provided on the upper side of the stainless steel fixing rod 4, and the stainless steel fixing rod 4 and the fixing plate 12 are connected and fixed by stainless steel bolts 13, and the stainless steel cathode screen 8 is fixedly connected to the cathode fixing plate 3 and located between the pair of cathode plates 2, and the size of the stainless steel cathode screen 8 is step The inner cavity structure size of the large-sized thin-walled component 7 in step 2 is half, and the upper outlet and the lower inlet of the stainless steel cathode screen 8 are both provided with protruding interfaces connected with the hose 9, and the hose 9 is a low-density high-pressure polyethylene hose. An electrolyte circulation pump 11 is installed on the hose 9. The electrolyte circulation pump 11 adopts an alkali-resistant motor and is equipped with a solution flow control valve. An electrolyte filter 10 with a stainless steel filter screen inside is installed on the hose 9 near the lower inlet, and the electrolyte circulation pump 11 and the electrolyte filter 10 are both located outside the auxiliary electrolyte tank 1, and then an anode fixing frame 5 with an anode conductive wire 6 is installed above the auxiliary electrolyte tank 1 to obtain an assembled auxiliary device;
[0031] Step 2: Preparation of micro-arc oxidation coating: Place the large-sized thin-walled parts 7 made of TC4 titanium alloy in a mixed solution prepared by deionized water and a detergent for ultrasonic cleaning for 10 minutes, and rinse with deionized water to obtain the treated large-sized thin-walled parts 7, and then Figure 1As shown, the cavity structure of the treated large-sized thin-walled component 7 is mounted on the stainless steel cathode screen 8 in the auxiliary device assembled in step one, and the central axis coincides with the central axis of the auxiliary device, and then connected to the anode conductive wire 6 on the anode fixing frame 5, and the whole is transferred into the electrolyte, so that the electrolyte covers the treated large-sized thin-walled component 7, and micro-arc oxidation is performed to prepare the coating. The components of the electrolyte are: 30g / L sodium silicate, 15g / L sodium hexametaphosphate, 0.6g / L sodium hydroxide, and the rest is deionized water. The process parameters of micro-arc oxidation are: voltage 520V, frequency 300Hz, duty cycle 15%, time 25min, electrolyte temperature 15°C~20°C during micro-arc oxidation, and after the micro-arc oxidation process is completed, the water stains are blown dry with compressed air after washing with deionized water, and washed with ethanol to obtain a large-sized thin-walled component with a uniform coating.
[0032] Comparative Example 1
[0033] This comparative example includes the following process: placing large-sized thin-walled parts made of TC4 titanium alloy in a mixed solution prepared by deionized water and a cleaning agent for ultrasonic cleaning for 10 minutes, and rinsing them with deionized water to obtain the treated large-sized thin-walled parts, and then placing them in the electrolyte of a micro-arc oxidation device so that the electrolyte covers the treated large-sized thin-walled parts, and performing micro-arc oxidation to prepare a coating. The components of the electrolyte are: 30g / L sodium silicate, 15g / L sodium hexametaphosphate, 0.6g / L sodium hydroxide, and the rest is deionized water. The process parameters of micro-arc oxidation are: voltage 520V, frequency 300Hz, duty cycle 15%, time 25min, electrolyte temperature 15°C~20°C during micro-arc oxidation, and after the micro-arc oxidation process is completed, the water stains are blown dry with compressed air after washing with deionized water, and then washed with ethanol to obtain large-sized thin-walled parts with a coating.
[0034] Figure 3 This is a physical picture of the coating prepared on the surface of a large-sized thin-walled component in Example 1 of the present invention. Figure 4 This is a physical picture of the coating prepared on the surface of a large-sized thin-walled component in Comparative Example 1 of the present invention. Figure 3 and Figure 4 By comparison, it can be seen that in Example 1 of the present invention, an auxiliary device is used for micro-arc oxidation, and the coating prepared on the surface of large-sized thin-walled parts with complex structures, including the outer wall and the inner cavity structure, is uniform, while in Comparative Example 1, the coating prepared on the surface of large-sized thin-walled parts with complex structures using conventional micro-arc oxidation equipment is uneven, especially the coating prepared at the inner cavity structure and the corner structure is damaged and uneven, which means that the present invention constructs an additional electric field through an auxiliary device to ensure that the electric field on the inner and outer surfaces of large-sized thin-walled parts is evenly distributed, thereby achieving uniform preparation of micro-arc oxidation coatings on the surfaces of large-sized thin-walled parts.
[0035] Example 2
[0036] The difference between this embodiment and embodiment 1 is that the material of the large-sized thin-walled parts is TC6 titanium alloy.
[0037] After testing, it was found that the coating prepared in this embodiment on the surface of large-sized thin-walled parts with complex structures, including the outer wall and inner cavity structure, was uniform.
[0038] Comparative Example 2
[0039] The difference between this comparative example and comparative example 1 is that the material of the large-sized thin-walled parts is TC6 titanium alloy.
[0040] After testing, it was found that the coating prepared on the surface of large-sized thin-walled parts with complex structures in this comparative example was uneven, especially the coating prepared on the inner cavity structure and the corner structure was damaged and uneven.
[0041] The above is only a preferred embodiment of the present invention and does not limit the present invention in any way. Any simple modification, change and equivalent change made to the above embodiment according to the technical essence of the invention still falls within the protection scope of the technical solution of the present invention.
Claims
1. A method for homogenizing a micro-arc oxidation coating on a large-sized thin-walled component, characterized in that: The method comprises the following steps: Step 1, assembling the auxiliary device: a pair of cathode plates (2) are installed near opposite tank walls inside the auxiliary electrolyte tank (1), and the pair of cathode plates (2) are respectively fixed to the two ends of the cathode fixing plate (3) located at the bottom of the auxiliary electrolyte tank (1), a stainless steel cathode screen (8) is fixedly connected to the cathode fixing plate (3), and the upper outlet and the lower inlet of the stainless steel cathode screen (8) are connected through a hose (9), an electrolyte circulation pump (11) is installed on the hose (9), and an electrolyte filter (10) is added to the hose (9) near the lower inlet, and the electrolyte circulation pump (11) and the electrolyte filter (10) are both located outside the auxiliary electrolyte tank (1), and then an anode fixing frame (5) with an anode conductive wire (6) is installed above the auxiliary electrolyte tank (1) to obtain an assembled auxiliary device; Step 2, preparation of micro-arc oxidation coating: placing the large-sized thin-walled component (7) in a mixed solution prepared by deionized water and a detergent for ultrasonic cleaning, and rinsing with deionized water to obtain the treated large-sized thin-walled component (7), and then the inner cavity structure of the treated large-sized thin-walled component (7) is mounted on the stainless steel cathode screen (8) in the auxiliary device assembled in step 1, and the central axis coincides with the central axis of the auxiliary device, and then connected to the anode conductive wire (6) on the anode fixing frame (5), and the whole is transferred into the electrolyte so that the electrolyte covers the treated large-sized thin-walled component (7), and the coating is prepared by micro-arc oxidation, and after washing with deionized water, the water stains are blown away with compressed air, and then washed with ethanol to obtain a large-sized thin-walled component with a uniform coating.
2. The method for homogenizing a micro-arc oxidation coating on a large-sized thin-walled component according to claim 1, characterized in that: The interior of the stainless steel cathode screen (8) described in step one is a hollow structure, and the size of the stainless steel cathode screen (8) is half the size of the inner cavity structure of the large-sized thin-walled component (7) described in step two. The upper outlet and the lower inlet of the stainless steel cathode screen (8) are both provided with protruding interfaces connected to the hose (9).
3. The method for homogenizing a micro-arc oxidation coating on a large-sized thin-walled component according to claim 1, characterized in that: The lower end of the stainless steel cathode screen (8) described in step 1 is provided with a fixing plate (12), and a stainless steel fixing rod (4) with a long round rod structure is fixedly connected to the position of the cathode fixing plate (3) corresponding to the fixing plate (12), a threaded interface is provided on the upper side of the stainless steel fixing rod (4), and the stainless steel fixing rod (4) and the fixing plate (12) are connected and fixed by a stainless steel bolt (13).
4. The method for homogenizing a micro-arc oxidation coating on a large-sized thin-walled component according to claim 1, characterized in that: The hose (9) described in step 1 is a low-density high-pressure polyethylene hose.
5. The method for homogenizing a micro-arc oxidation coating on a large-sized thin-walled component according to claim 1, characterized in that: The electrolyte filter (10) described in step 1 has a filter screen made of stainless steel inside.
6. The method for homogenizing a micro-arc oxidation coating on a large-sized thin-walled component according to claim 1, characterized in that: The electrolyte circulation pump (11) described in step 1 adopts an alkali-resistant motor and is equipped with a solution flow control valve.