Method for preparing polyvinyl alcohol coarse denier monofilament fiber

By modifying PVA powder by cross-linking and xanthation, and combining it with plasticizers and flame retardants, the problem of insufficient tensile strength and flame retardant properties of polyvinyl alcohol monofilament fibers was solved, and high-strength and high-performance Flame retardant polyvinyl alcohol coarse monofilament fiber suitable for high-end applications.

CN118727183AInactive Publication Date: 2024-10-01SHANDONG NANSHAN TEXTILE GARMENT

Patent Information

Application Number
CN202411223020.5
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Filing Date
2024-09-03
Publication Date
2024-10-01
Estimated Expiration
Not applicable · inactive patent

AI Technical Summary

Technical Problem

Traditional polyvinyl alcohol monofilament fibers have low tensile strength and tensile elongation during the preparation process, are flammable, and cannot meet the requirements for high strength, high elasticity and flame retardant properties.

Method used

PVA powder is modified by cross-linking and xanthation, mixed with plasticizers and flame retardants, and then melt-spun and heat-treated to prepare polyvinyl alcohol coarse-denier monofilament fibers with high strength and flame-retardant properties.

Benefits of technology

It significantly improves the tensile strength and flame retardant properties of the fiber and is suitable for high-end applications, meeting the requirements of high strength and high elasticity while reducing the risk of combustion.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure SMS_1
    Figure SMS_1
  • Figure SMS_2
    Figure SMS_2
Patent Text Reader

Abstract

The invention relates to a method for preparing polyvinyl alcohol coarse denier monofilament fibers, and belongs to the technical field of polyvinyl alcohol fiber preparation, the method comprises the following steps: firstly, PVA powder is cross-linked, freeze-dried and crushed to obtain pretreated PVA; carbon disulfide powder reacts with alkali to generate xanthate, and the pretreated PVA is subjected to xanthation modification. And then mixing the modified PVA with a plasticizer and a flame retardant, carrying out melt spinning, extruding through a spinneret plate at a specific temperature, and carrying out side blowing cooling, stretching and heat treatment shaping to finally prepare the polyvinyl alcohol coarse denier monofilament fiber. Through crosslinking and xanthation modification, the physical and chemical properties, such as strength, heat resistance and water resistance, of PVA are significantly improved; the temperature and stretching conditions are accurately controlled in the spinning process, so that the uniformity and high quality of the fibers are ensured; the final product has excellent strength and flame retardance, and is suitable for various high-end application fields.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The invention relates to the technical field of polyvinyl alcohol fiber preparation, and more specifically, to a method for preparing polyvinyl alcohol coarse-denier monofilament fibers. Background Art

[0002] In the field of textile materials, polyvinyl alcohol (PVA) fibers have attracted much attention due to their good hydrophilicity, biocompatibility and degradability. However, traditional polyvinyl alcohol monofilament fibers often face the problem of low tensile strength and tensile elongation during the preparation process. Specifically, during the stretching process, ordinary polyvinyl alcohol monofilament fibers are difficult to form a stable high-strength structure due to the weak interaction between molecular chains, resulting in limited tensile strength. At the same time, its tensile elongation is also low, which limits the performance of the fiber in terms of deformation recovery and elasticity retention. This limits its application in situations requiring high strength and high elasticity. In addition, the polyvinyl alcohol material itself is flammable, and monofilament fibers that have not been specially treated tend to burn rapidly under extreme conditions such as fires, increasing safety hazards. With the increasingly stringent safety standards, the deficiencies of ordinary polyvinyl alcohol monofilament fibers in flame retardancy have gradually become apparent, making it difficult to meet the high requirements for flame retardancy of materials in specific fields such as fire protection and construction.

[0003] Therefore, developing a method for preparing polyvinyl alcohol coarse-denier monofilament fibers that can not only improve tensile strength and tensile elongation but also significantly enhance flame retardancy has become a technical challenge that needs to be urgently addressed in the current field of textile materials. Summary of the invention

[0004] In order to solve the problems raised in the background technology, the present invention provides a method for preparing polyvinyl alcohol coarse denier monofilament fiber. First, PVA powder is cross-linked and freeze-dried, and then crushed to obtain pretreated PVA. Then, carbon disulfide powder is reacted with an alkali to generate xanthate, and the pretreated PVA is xanthated and modified. Subsequently, the modified PVA is mixed with a plasticizer and a flame retardant, melt-spun, extruded through a spinneret at a specific temperature, and shaped by side-blowing cooling, stretching and heat treatment to finally obtain a polyvinyl alcohol coarse denier monofilament fiber. Through cross-linking and xanthate modification, the physical and chemical properties of PVA, such as strength, heat resistance and water resistance, are significantly improved; the temperature and stretching conditions are precisely controlled during the spinning process to ensure the uniformity and high quality of the fiber; the final product has excellent performance in strength and flame retardancy, and is suitable for a variety of high-end application fields.

[0005] The present invention provides a method for preparing a polyvinyl alcohol coarse-denier monofilament fiber, which adopts the following technical scheme: A method for preparing polyvinyl alcohol coarse-denier monofilament fiber comprises the following preparation steps: S1. Add PVA powder to deionized water and stir evenly to obtain a PVA solution; add a crosslinking agent to the PVA solution, adjust the pH value of the system to 2-4, stir again until uniform, freeze-dry, and then crush and sieve to obtain a pretreated PVA powder; S2, adding the pretreated PVA powder obtained in step S1 to deionized water, stirring evenly, adding NaOH powder and carbon disulfide powder, continuing to stir and raising the system temperature to 50-60°C, the reaction time is 100-150 minutes, then filtering the system, washing the filtrate with deionized water until the pH value of the washing liquid is neutral, and finally drying the washed filtrate to obtain modified PVA; S3. The modified PVA, plasticizer and flame retardant obtained in step S2 are mixed at 40-60° C. for 1-3 hours to obtain a mixture; after the mixture is melted, it is metered using a spinning pump with a metering temperature of 170-190° C., and then extruded using a spinneret with a spinneret temperature set to 110-130° C., and then cooled and wound, with a spinneret stretching ratio of 1.5-3 times, the spun fiber is stretched at 160-210° C. with a stretching ratio of 10-20 times, and heat-treated at 200-220° C. for 1-3 minutes to obtain polyvinyl alcohol coarse denier monofilament fiber.

[0006] Furthermore, a method for preparing polyvinyl alcohol coarse denier monofilament fiber comprises the following preparation steps: S1. Add PVA powder to deionized water and stir evenly at room temperature to obtain a PVA solution; add a crosslinking agent to the PVA solution, adjust the pH value of the system to 2-4, stir again until uniform, freeze-dry, and then crush through a 10-30 mesh sieve to obtain a pretreated PVA powder; S2, the pretreated PVA powder obtained in step S1 is added to deionized water according to (1-3) g: 250 mL, and after stirring evenly, NaOH powder and carbon disulfide powder are added, stirring is continued and the system temperature is increased to 50-60° C., the reaction time is 100-150 minutes, and then the system is filtered, and the filtrate is washed with deionized water until the pH value of the washing liquid is neutral, and finally the washed filtrate is dried to obtain modified PVA; In the above reaction process, in step S1, a cross-linking agent is used to cross-link PVA, and a PVA material with a pore size is obtained after freeze drying, and the pre-treated PVA powder is obtained after crushing and sieving. In step S2, carbon disulfide powder can react with an aqueous solution of alkali to generate xanthate, and the following reaction occurs in the system: CS2+ 2NaOH → Na2COS2+ H2O; then the sodium xanthate generated in the system xanthates the pre-treated PVA powder, and the xanthate group is grafted onto the main chain of PVA to prepare a modified PVA.

[0007] S3. The modified PVA, plasticizer and flame retardant obtained in step S2 are mixed at 40-60°C for 1-3 hours to obtain a mixture; after the mixture is melted, it is metered using a spinning pump with a metering temperature of 170-190°C, and then extruded using a spinneret with a spinneret temperature set to 110-130°C, and then cooled with side-blown air at a humidity of 70% and wound up, the spinneret stretching ratio is 1.5-3 times, the spun fiber is stretched at 160-210°C with a stretching ratio of 10-20 times, and heat-treated at 200-220°C for 1-3 minutes to obtain polyvinyl alcohol coarse denier monofilament fiber.

[0008] Furthermore, in step S1, the mass ratio of PVA powder to cross-linking agent is (3-4): (1-3).

[0009] Furthermore, in step S1, the cross-linking agent is a 10-30 wt % glutaraldehyde aqueous solution.

[0010] Furthermore, in step S2, the mass ratio of pretreated PVA powder, carbon disulfide powder, and NaOH powder is (1-3): (0.1-1): (0.01-0.018).

[0011] Furthermore, in step S3, the plasticizer is obtained by mixing a brominated polymer material, glycerol, ethylene glycol and an inorganic salt in a mass ratio of (1-3):2:1:(1-2).

[0012] Furthermore, the brominated polymer material is at least one of brominated polystyrene, tetrabromobisphenol A, brominated polyacrylonitrile, and brominated polyolefin.

[0013] Furthermore, the inorganic salt is Mg 2+ and Ca 2+ At least one metal salt.

[0014] Furthermore, in step S3, the flame retardant is ammonium polyphosphate.

[0015] Furthermore, in step S3, during the melting process, the temperature of the feeding zone is set to 150-170°C, the temperature of the compression zone is set to 170-190°C, and the temperature of the homogenization zone is set to 190-210°C.

[0016] Furthermore, in step S3, the mass ratio of modified PVA, plasticizer and flame retardant is 10:(1-3):(0.1-1).

[0017] In summary, the present invention has the following beneficial effects: 1. In the technical solution of the present invention, a cross-linking agent is used to cross-link PVA, and a PVA material with a pore size is obtained after freeze drying, and a pre-treated PVA powder is obtained after crushing and sieving; the rich pores on the pre-treated PVA powder can improve its adsorption effect on flame retardants and plasticizers in the subsequent process, and improve the reinforcing effect of the flame retardants and plasticizers used on PVA fiber products, making them more stable and durable. In addition, pre-treating PVA powder can reveal more functional groups such as hydroxyl groups, enhance its surface activity, increase the modification rate of xanthate on PVA materials, prevent the reaction time from being too long, resulting in the hydrolysis of xanthate, reduce the xanthate degree of the modified PVA, and affect the performance of the finished product.

[0018] 2. In the technical solution of the present invention, the pre-treated PVA powder is subjected to xanthate treatment to prepare modified PVA. The xanthate treatment grafts xanthate groups on the PVA molecular chain, and the xanthate groups cooperate with the hydroxyl groups on the PVA chain, which can improve the binding effect of the metal salt ions in the plasticizer and the PVA material through the interaction of coordination bonds and ion exchange.

[0019] 3. In the technical solution of the present invention, brominated polymer materials, glycerol, ethylene glycol and inorganic salts are used in combination as plasticizers for PVA; the use of glycerol and ethylene glycol components is conducive to reducing the glass transition temperature of PVA materials and improving the flexibility and processability of PVA; the combined use of brominated polymer materials and phosphorus flame retardants can improve the flame retardant properties of the materials, and can be used in combination with glycerol and ethylene glycol components to further improve the mechanical properties of PVA. The inorganic salt component can interact with the xanthate functional group and carboxyl functional group on the modified PVA, weaken the hydrogen bonding between the PVA molecular chains, destroy its crystalline structure, and further improve the flame retardant properties and mechanical properties of the obtained PVA fiber. DETAILED DESCRIPTION

[0020] The following will be combined with the embodiments of the present invention to clearly and completely describe the technical solutions in the embodiments of the present invention. Obviously, the described embodiments are only part of the embodiments of the present invention, not all of the embodiments. Based on the embodiments of the present invention, all other embodiments obtained by ordinary technicians in this field without making creative work are within the scope of protection of the present invention.

[0021] The specific implementation of the present invention involves: PVA powder was provided by Shanghai Chenqi Chemical Technology Co., Ltd., with the product number PVA2488 (100 mesh); NaOH powder and carbon disulfide powder, chemically pure, 80 mesh; Brominated polystyrene, CAS No. 88497-56-7, bromide content ≥ 68%; Tetrabromobisphenol A: CAS number 79-94-7, purity 99%.

[0022] Example 1 A method for preparing polyvinyl alcohol coarse-denier monofilament fiber specifically comprises the following preparation steps: S1. PVA powder was added to deionized water at a mass volume ratio of 4 g:100 mL, and stirred at 30 rpm at room temperature to obtain a PVA solution; a cross-linking agent was added to the PVA solution, and the pH value of the system was adjusted to 2. The solution was stirred again until uniform, freeze-dried, and then crushed through a 10-mesh sieve to obtain a pretreated PVA powder; Among them, the mass ratio of PVA powder to cross-linking agent is 3:1; Wherein, the cross-linking agent is a 10wt% glutaraldehyde aqueous solution; S2, the pretreated PVA powder obtained in step S1 is added to deionized water at a ratio of 1 g: 250 mL, and after stirring evenly, NaOH powder and carbon disulfide powder are added, stirring is continued and the system temperature is raised to 50° C. The reaction time is 100 minutes, and then the system is filtered, and the filtered material is washed with deionized water until the pH value of the washing liquid is neutral, and finally the filtered material after washing is dried to obtain modified PVA; Among them, the mass ratio of pretreated PVA powder, carbon disulfide powder, and NaOH powder is 1:0.1:0.01; S3, the modified PVA, plasticizer and flame retardant obtained in step S2 are mixed at a mass ratio of 10:1:0.1 at 40°C for 1 hour to obtain a mixture; the mixture is melted and metered using a spinning pump, the temperature of the feeding zone is set to 150°C during the melting process, the temperature of the compression zone is set to 170°C, the temperature of the homogenization zone is set to 190°C, and the metering temperature is set to 170°C, and then extruded using a spinneret with an aperture of 0.2mm, the spinneret temperature is set to 110°C, and then cooled with side-blown air at a humidity of 70% and wound, the spinneret stretching ratio is 1.5 times, the nascent fiber is stretched at 160°C, the stretching ratio is 10 times, and the polyvinyl alcohol coarse denier monofilament fiber is obtained by heat treatment at 200°C for 1 minute; The plasticizer is obtained by mixing a brominated polymer material, glycerol, ethylene glycol and an inorganic salt in a mass ratio of 1:2:1:1; the brominated polymer material is brominated polystyrene, and the inorganic salt is magnesium sulfate; Wherein, the flame retardant is ammonium polyphosphate.

[0023] Example 2 A method for preparing polyvinyl alcohol coarse-denier monofilament fiber specifically comprises the following preparation steps: S1. PVA powder was added to deionized water at a mass volume ratio of 4 g:100 mL, and stirred at 30 rpm at room temperature to obtain a PVA solution; a cross-linking agent was added to the PVA solution, and the pH value of the system was adjusted to 3. The solution was stirred again until uniform, freeze-dried, and then crushed through a 20-mesh sieve to obtain a pretreated PVA powder; Among them, the mass ratio of PVA powder to cross-linking agent is 3:2; Wherein, the cross-linking agent is a 20wt% glutaraldehyde aqueous solution; S2, the pretreated PVA powder obtained in step S1 is added to deionized water at a ratio of 2 g: 250 mL, and after stirring evenly, NaOH powder and carbon disulfide powder are added, stirring is continued and the system temperature is raised to 55° C. The reaction time is 120 minutes, and then the system is filtered, and the filtered material is washed with deionized water until the pH value of the washing liquid is neutral, and finally the washed filtered material is dried to obtain the modified PVA; Among them, the mass ratio of pretreated PVA powder, carbon disulfide powder, and NaOH powder is 2:0.5:0.015; S3, the modified PVA, plasticizer and flame retardant obtained in step S2 are mixed at a mass ratio of 10:2:0.5 at 50°C for 2 hours to obtain a mixture; after the mixture is melted, it is metered using a spinning pump, the temperature of the feeding zone is set to 160°C during the melting process, the temperature of the compression zone is set to 180°C, the temperature of the homogenization zone is set to 200°C, and the metering temperature is set to 180°C, and then extruded using a spinneret with an aperture of 0.2mm, the spinneret temperature is set to 120°C, and then the side-blown air with a humidity of 70% is cooled and wound, the spinneret stretching ratio is 2 times, the nascent fiber is stretched at 180°C, the stretching ratio is 15 times, and the polyvinyl alcohol coarse denier monofilament fiber is obtained by heat treatment at 210°C for 2 minutes; The plasticizer is obtained by mixing a brominated polymer material, glycerol, ethylene glycol and an inorganic salt in a mass ratio of 2:2:1:1.5; the brominated polymer material is brominated polystyrene, and the inorganic salt is magnesium sulfate; Wherein, the flame retardant is ammonium polyphosphate.

[0024] Example 3 A method for preparing polyvinyl alcohol coarse-denier monofilament fiber specifically comprises the following preparation steps: S1. PVA powder was added to deionized water at a mass volume ratio of 4 g:100 mL, and stirred at 30 rpm at room temperature to obtain a PVA solution; a cross-linking agent was added to the PVA solution, and the pH value of the system was adjusted to 4. The solution was stirred again until uniform, freeze-dried, and then crushed through a 30-mesh sieve to obtain a pretreated PVA powder; Among them, the mass ratio of PVA powder to cross-linking agent is 4:3; Wherein, the cross-linking agent is a 30wt% glutaraldehyde aqueous solution; S2. The pretreated PVA powder obtained in step S1 is added to deionized water at a ratio of 3 g: 250 mL. After stirring evenly, NaOH powder and carbon disulfide powder are added. Stirring is continued and the system temperature is raised to 60° C. The reaction time is 150 minutes. The system is then filtered and the filtered material is washed with deionized water until the pH value of the washing liquid is neutral. Finally, the washed filtered material is dried to obtain modified PVA. Among them, the mass ratio of pretreated PVA powder, carbon disulfide powder, and NaOH powder is 3:1:0.018; S3, the modified PVA, plasticizer and flame retardant obtained in step S2 are mixed at a mass ratio of 10:3:1 at 60°C for 3 hours to obtain a mixture; the mixture is melted and metered using a spinning pump, the temperature of the feeding zone is set to 170°C during the melting process, the temperature of the compression zone is set to 190°C, the temperature of the homogenization zone is set to 210°C, and the metering temperature is set to 190°C, and then extruded using a spinneret with an aperture of 0.2mm, the spinneret temperature is set to 130°C, and then cooled with side-blown air at a humidity of 70% and wound, the spinneret stretching ratio is 3 times, the nascent fiber is stretched at 210°C, the stretching ratio is 20 times, and the polyvinyl alcohol coarse denier monofilament fiber is obtained by heat treatment at 220°C for 3 minutes; The plasticizer is obtained by mixing a brominated polymer material, glycerol, ethylene glycol and an inorganic salt in a mass ratio of 3:2:1:2; the brominated polymer material is tetrabromobisphenol A, and the inorganic salt is calcium sulfate; Wherein, the flame retardant is ammonium polyphosphate.

[0025] Comparative Example 1 The difference between this comparative example and Example 1 is that in step S3, polystyrene is used instead of brominated polystyrene material.

[0026] Comparative Example 2 The difference between this comparative example and Example 1 is that in step S3, the inorganic salt used is copper sulfate; Comparative Example 3 The difference between this comparative example and Example 1 is that the flame retardant used in step S3 is decabromodiphenylethane.

[0027] Comparative Example 4 The difference between this comparative example and Example 1 is that the pretreated PVA powder is prepared by the following steps: PVA powder was added into deionized water at a mass volume ratio of 4 g:100 mL, stirred at 30 rpm at room temperature, the pH value of the system was adjusted to 2, stirred again until uniform, freeze-dried, and then crushed through a 10-mesh sieve to obtain pretreated PVA powder.

[0028] Comparative Example 5 A method for preparing polyvinyl alcohol coarse-denier monofilament fiber specifically comprises the following preparation steps: S1. PVA powder was added to deionized water at a mass volume ratio of 4 g:100 mL, and stirred at 30 rpm at room temperature to obtain a PVA solution; a cross-linking agent was added to the PVA solution, and the pH value of the system was adjusted to 2. The solution was stirred again until uniform, freeze-dried, and then crushed through a 10-mesh sieve to obtain a pretreated PVA powder; Among them, the mass ratio of PVA powder to cross-linking agent is 3:1; Wherein, the cross-linking agent is a 10wt% glutaraldehyde aqueous solution; S2. The pretreated PVA powder, plasticizer and flame retardant obtained in step S1 are mixed at a mass ratio of 10:1:0.1 at 40°C for 1 hour to obtain a mixture; the mixture is melted and metered using a spinning pump, the temperature of the feeding zone is set to 150°C during the melting process, the temperature of the compression zone is set to 170°C, the temperature of the homogenization zone is set to 190°C, and the metering temperature is set to 170°C, and then extruded using a spinneret with an aperture of 0.2 mm, the spinneret temperature is set to 110°C, and then cooled with side-blown air at a humidity of 70% and wound, the spinneret stretching ratio is 1.5 times, the nascent fiber is stretched at 160°C, the stretching ratio is 10 times, and the polyvinyl alcohol coarse denier monofilament fiber is obtained by heat treatment at 200°C for 1 minute; The plasticizer is obtained by mixing a brominated polymer material, glycerol, ethylene glycol and an inorganic salt in a mass ratio of 1:2:1:1; the brominated polymer material is brominated polystyrene, and the inorganic salt is magnesium sulfate; Wherein, the flame retardant is ammonium polyphosphate.

[0029] Performance Testing The mechanical properties of the samples prepared in Examples 1-3 and Comparative Examples 1-5 are now tested. 20 cm of the polyvinyl alcohol coarse denier monofilament fibers prepared in Examples 1-3 and Comparative Examples 1-5 of the present invention are taken out as samples. The linear density of the fibers is measured using a denier meter at room temperature, and the samples are weighed to calculate their deniers.

[0030] Using a tensile testing machine, the fiber samples prepared in different groups were clamped in a fixture, and the samples were stretched at a tensile rate of 50 mm / min until the samples broke. The elongation at break and elongation at break of the samples were calculated. Each sample was tested 5 times and the average value was recorded.

[0031] The specific performance test results are shown in Table 1: Table 1. Mechanical properties of samples tested

[0032] As shown in the results of Table 1 above, the polyvinyl alcohol coarse denier monofilament fiber prepared in Example 2 has the best breaking strength and elongation at break, and exhibits the best mechanical properties. As shown in the results of Comparative Example 1, the introduction of bromine elements can interact with the PVA molecular chain, strengthen the molecular chain structure, increase the interaction force between molecules, prevent the expansion of cracks, and make the fiber more difficult to break under stress, thereby improving the overall strength. As shown in the results of Comparative Example 2, calcium ions and magnesium ions can form more cross-linking points compared to other metal ions, showing better breaking strength and elongation at break. As shown in the results of Comparative Example 3, compared with flame retardants with good flame retardant effects such as decabromodiphenylethane, ammonium polyphosphate has less effect on the movement of PVA molecular chains, making the mechanical properties in Example 1 better than the data in Comparative Example 3. As shown in the results of Comparative Examples 4 and 5, the mechanical properties of the obtained PVA fiber can be improved by cross-linking pretreatment and xanthogenic treatment of PVA powder.

[0033] The flame retardant effect of the polyvinyl alcohol coarse denier monofilament fibers prepared in Examples 1-3 and Comparative Examples 1-5 is now tested. Take 30 cm of the monofilament fibers prepared in different groups. Under the conditions of an ambient temperature of 2°C, a relative humidity of 45±2%, and an air oxygen concentration of 20±2%, ignite the sample from the top. After confirming that the top of the sample is completely on fire, immediately remove the igniter and record the burning time and the burning length of the sample. When igniting the sample, the longest time the flame acts is 30 seconds. If it cannot be ignited within 30 seconds, continue to ignite after increasing the oxygen concentration until it ignites within 30 seconds. Each sample is tested 15 times, and the average value is recorded. The test results are shown in Table 2 below.

[0034] Table 2. Flame retardant effect test

[0035] From the results in Table 2, it can be seen that the polyvinyl alcohol coarse denier monofilament fiber prepared in Example 2 has the best flame retardant effect. From the results in the comparative example, it can be seen that the combined use of brominated polymer materials and phosphorus flame retardants can improve the flame retardant properties of the material. The comprehensive performance of the polyvinyl alcohol coarse denier monofilament fibers prepared in Examples 1-3 of the present invention is better than that of the products prepared in Comparative Examples 1-5, that is, within the technical solution defined in the present invention, the comprehensive performance of the polyvinyl alcohol coarse denier monofilament fibers prepared is excellent.

[0036] In the description of the specification, the description with reference to the terms "one embodiment", "example", "specific example", etc. means that the specific features, structures, materials or characteristics described in conjunction with the embodiment or example are included in at least one embodiment or example of the present invention. In this specification, the schematic representation of the above terms does not necessarily refer to the same embodiment or example. Moreover, the specific features, structures, materials or characteristics described can be combined in any one or more embodiments or examples in a suitable manner.

[0037] The above contents are merely examples and explanations of the present invention. Those skilled in the art may make various modifications or additions to the specific embodiments described or replace them in a similar manner. As long as they do not deviate from the invention or exceed the scope defined by the claims, they shall all fall within the protection scope of the present invention.

Claims

1. A method for preparing polyvinyl alcohol high-denier monofilament fiber, characterized in that: The method comprises the following preparation steps: S1. Add PVA powder to deionized water and stir evenly to obtain a PVA solution; add a crosslinking agent to the PVA solution, adjust the pH value of the system to 2-4, stir again until uniform, freeze-dry, and then crush and sieve to obtain a pretreated PVA powder; S2, adding the pretreated PVA powder obtained in step S1 to deionized water, stirring evenly, adding NaOH powder and carbon disulfide powder, continuing to stir and raising the system temperature to 50-60°C, the reaction time is 100-150 minutes, then filtering the system, washing the filtrate with deionized water until the pH value of the washing liquid is neutral, and finally drying the washed filtrate to obtain modified PVA; S3. The modified PVA, plasticizer and flame retardant obtained in step S2 are mixed at 40-60° C. for 1-3 hours to obtain a mixture; after the mixture is melted, it is metered using a spinning pump with a metering temperature of 170-190° C., and then extruded using a spinneret with a spinneret temperature set to 110-130° C., and then cooled and wound, with a spinneret stretching ratio of 1.5-3 times, the spun fiber is stretched at 160-210° C. with a stretching ratio of 10-20 times, and heat-treated at 200-220° C. for 1-3 minutes to obtain polyvinyl alcohol coarse denier monofilament fiber.

2. The method for preparing polyvinyl alcohol high-denier monofilament fiber according to claim 1, characterized in that: In step S1, the mass ratio of PVA powder to cross-linking agent is (3-4): (1-3).

3. The method for preparing polyvinyl alcohol high-denier monofilament fiber according to claim 1, characterized in that: In step S1, the cross-linking agent is a 10-30 wt % glutaraldehyde aqueous solution.

4. The method for preparing polyvinyl alcohol high-denier monofilament fiber according to claim 1, characterized in that: In step S2, the mass ratio of pretreated PVA powder, carbon disulfide powder, and NaOH powder is (1-3): (0.1-1): (0.01-0.018).

5. The method for preparing polyvinyl alcohol high-denier monofilament fiber according to claim 1, characterized in that: In step S3, the plasticizer is obtained by mixing a brominated polymer material, glycerol, ethylene glycol and an inorganic salt in a mass ratio of (1-3):2:1:(1-2).

6. The method for preparing polyvinyl alcohol high-denier monofilament fiber according to claim 5, characterized in that: The brominated polymer material is at least one of brominated polystyrene, tetrabromobisphenol A, brominated polyacrylonitrile and brominated polyolefin.

7. The method for preparing polyvinyl alcohol high-denier monofilament fiber according to claim 5, characterized in that: The inorganic salt is Mg 2+ and Ca 2+ At least one metal salt.

8. The method for preparing polyvinyl alcohol high-denier monofilament fiber according to claim 1, characterized in that: In step S3, the flame retardant is ammonium polyphosphate.

9. The method for preparing polyvinyl alcohol high-denier monofilament fiber according to claim 1, characterized in that: In step S3, during the melting process, the temperature of the feeding zone is set to 150-170°C, the temperature of the compression zone is set to 170-190°C, and the temperature of the homogenization zone is set to 190-210°C.

10. The method for preparing polyvinyl alcohol high-denier monofilament fiber according to claim 1, characterized in that: In step S3, the mass ratio of modified PVA, plasticizer and flame retardant is 10:(1-3):(0.1-1).

Citation Information

Patent Citations

  • Polyvinyl alcohol composition capable of melt processing and preparation method thereof

    CN105086306A

  • PVA fiber reinforced flame-retardant PBT-PC alloy composite material and preparation method and application thereof

    CN109294178A

  • Method for preparing polyvinyl alcohol coarse denier fiber through melt spinning

    CN110205696A

  • Flame-retardant polyvinyl alcohol aerogel and preparation method thereof

    CN110607046A

  • Preparation method of microporous polyvinyl alcohol fibers

    CN112921431A

Cited By

  • Preparation method of high-concentration polyvinyl alcohol hydrogel particles capable of being subjected to melt processing

    CN122277947A

  • Production process of micron-sized polyvinyl alcohol fiber

    CN122358345A