Polylactic acid fiber and preparation process thereof

Through the modification and polymerization coating technology of CNTs, the problem of insufficient heat resistance and toughness of polylactic acid fiber is solved, its heat resistance and toughness are significantly improved, the compatibility with PLA fiber is improved, and the fiber's Overall performance.

CN118727191APending Publication Date: 2024-10-01ANHUI YUANMENG BIO BASED MATERIAL TECH CO LTD
View PDF 0 Cites 0 Cited by

Patent Information

Application Number
CN202411109117.3
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Filing Date
2024-08-13
Publication Date
2024-10-01

AI Technical Summary

Technical Problem

Polylactic acid fiber has poor heat resistance, toughness and hydrolysis resistance, which limits its marketization process and industrial development.

Method used

By modifying hydroxylated multi-walled carbon nanotubes (CNTs) with a silane coupling agent and long-chain unsaturated olefinic acid, and coating them with lactide ring-opening polymerization, CNTs-coupling agent/long-chain unsaturated olefinic acid is formed. -LA, blended with polylactic acid chips to prepare composite masterbatch, and then polylactic acid fiber was prepared by melt spinning.

Benefits of technology

It improves the dispersion and crystallinity of CNTs in the PLA matrix, enhances the heat resistance and toughness of PLA fiber, improves the compatibility between PLA fiber and CNTs, and improves the hydrolysis resistance of the fiber.

✦ Generated by Eureka AI based on patent content.
Patent Text Reader

Abstract

The invention discloses a polylactic acid fiber and a preparation method thereof, and belongs to the technical field of chemical fiber preparation. The preparation method comprises the following steps: performing surface modification on CNTs by using a silane coupling agent to obtain a CNTs-coupling agent; performing secondary modification on the CNTs-coupling agent by using long-chain unsaturated olefine acid to obtain a CNTs-coupling agent / long-chain unsaturated olefine acid; lactide is subjected to ring opening polymerization to coat the CNTs-coupling agent / long-chain unsaturated olefine acid, and CNTs-coupling agent / long-chain unsaturated olefine acid-LA is prepared; blending the CNTs-coupling agent / long-chain unsaturated olefine acid-LA and the polylactic acid slices to prepare a composite master batch; and blending the composite master batch with polylactic acid slices, and carrying out melt spinning to obtain the CNTs-coupling agent / long-chain unsaturated olefine acid-LA polylactic acid fiber. The polylactic acid fiber prepared by the method has good heat resistance, toughness and hydrolysis resistance, and can be widely applied to textile materials.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The invention relates to the technical field of chemical fiber preparation, and in particular to a polylactic acid fiber and a preparation method thereof. Background Art

[0002] As a necessity for human life, textiles are used in huge quantities, are difficult to recycle, and have a great impact on the environment. Therefore, vigorously developing new biodegradable textile materials has become one of the current trends in the development of world textile technology. In recent years, the new fiber material polylactic acid fiber, referred to as PLA fiber, has attracted the attention and favor of the global textile material industry. PLA fiber is a degradable chemical fiber material made from renewable grains such as corn. It overcomes the disadvantage of polymer materials relying on petrochemical resources, can be completely degraded in water or soil, and will not pollute the environment.

[0003] However, PLA fibers and textile products have problems such as easy hydrolysis, poor heat resistance, poor toughness, poor fabric feel, and poor wear resistance, which seriously hinder their marketization process and drag down the rapid development and growth of the entire industry.

[0004] The patent application with publication number CN111825845A discloses a polylactic acid grafted modified bamboo fiber and a polylactic acid composite material and a preparation method thereof. Functional bamboo fiber and functional polylactic acid are dissolved together in a solvent, and then an initiator is introduced to achieve grafting modification through a chemical reaction. This preparation method not only simplifies the operation steps and is easy to implement, but also significantly optimizes the interface bonding between the two phases of the material, showing good adaptability to industrial production. The obtained bamboo fiber / polylactic acid composite material and its composite fiber show significantly improved performance advantages in terms of breaking strength, impact toughness and heat resistance. However, there is a problem of uneven dispersion of bamboo fiber and polylactic acid in this patent. Summary of the invention

[0005] In order to overcome the deficiencies of the prior art, the object of the present invention is to provide a polylactic acid fiber and a preparation method thereof, so as to solve the technical problems of poor heat resistance, poor toughness and poor hydrolysis resistance of polylactic acid fiber.

[0006] The purpose of the present invention can be achieved through the following technical solutions:

[0007] A method for preparing polylactic acid fiber, characterized in that it is prepared by the following steps:

[0008] 1) Silane coupling agent is used to modify the surface of CNTs to obtain CNTs-coupling agent;

[0009] 2) The long-chain unsaturated olefinic acid performs secondary modification on the CNTs-coupling agent to obtain CNTs-coupling agent / long-chain unsaturated olefinic acid;

[0010] 3) Lactide is ring-opening polymerized to coat CNTs-coupling agent / long-chain unsaturated olefinic acid to obtain CNTs-coupling agent / long-chain unsaturated olefinic acid-LA;

[0011] 4) CNTs-coupling agent / long-chain unsaturated olefinic acid-LA is blended with polylactic acid chips to prepare composite masterbatch;

[0012] 5) After the composite masterbatch and the polylactic acid chips are dried, they are blended and melt-spun to obtain a polylactic acid fiber.

[0013] Furthermore, the CNTs are hydroxylated multi-walled carbon nanotubes, the silane coupling agent is KH550, and the long-chain unsaturated olefinic acid is one of oleic acid, linoleic acid, 5-hexenoic acid, and erucic acid.

[0014] Furthermore, the step of surface modification of CNTs by the silane coupling agent is as follows: weigh CNTs and the hydrolyzed silane coupling agent solution, heat the solution to 70-80°C and stir for 4-5h; dry the mixed solution at 120-130°C for 8-10h, take it out, grind, wash, vacuum filter, and dry at 70-80°C for 10-12h to obtain CNTs with surface modification by the silane coupling agent.

[0015] Furthermore, the mass fraction of the silane coupling agent in CNTs is 3-5wt%; the silane coupling agent is diluted with methanol and water before use, and the mass ratio of water: methanol: silane coupling agent is 10:70:20; hydrochloric acid is added dropwise to adjust the pH value to 3-4, and hydrolysis is carried out at room temperature for 0.5-1h to obtain a pre-hydrolyzed silane coupling agent solution.

[0016] Furthermore, the secondary modification comprises the following steps: adding CNTs-coupling agent into deionized water, then adding long-chain unsaturated olefinic acid dropwise, heating the solution to 70-80° C. and stirring for 8-10 hours, washing and drying after the reaction to obtain CNTs secondary-modified with long-chain unsaturated olefinic acid;

[0017] The mass ratio of CNTs-coupling agent, long-chain unsaturated olefinic acid and deionized water is 1:2:50.

[0018] Furthermore, the step of encapsulating CNTs by ring-opening polymerization of lactide is as follows: adding the dried lactide to DMF, and simultaneously adding CNTs-coupling agent / long-chain unsaturated olefinic acid and stannous octoate catalyst, heating to 130-140° C. under a nitrogen atmosphere, stirring and reacting for 20-24 hours, and after the reaction is completed, centrifuging, washing with dichloromethane, washing with distilled water, and drying at 70-80° C. for 4-6 hours to obtain lactide-modified CNTs-coupling agent / long-chain unsaturated olefinic acid-LA.

[0019] Furthermore, the mass ratio of the CNTs-coupling agent / long-chain unsaturated olefinic acid to lactide is 1:10;

[0020] The mass ratio of stannous octoate catalyst to lactide is 1:150.

[0021] Furthermore, the preparation steps of the composite masterbatch in step 4) are as follows: polylactic acid chips, polylactic acid powder and CNTs-coupling agent / long-chain unsaturated olefinic acid-LA are dried at 100-110° C. for 10-12 hours, melt blended, cooled and pelletized to form the composite masterbatch;

[0022] The blending temperature is 160°C-190°C;

[0023] The amount of CNTs-coupling agent / long-chain unsaturated olefinic acid-LA used is 0.25-2wt% of the total mass of the composite masterbatch.

[0024] Furthermore, in step 5), the drying temperature of the polylactic acid chips and the composite masterbatch is 110-120° C., and the drying time is 10-12 hours;

[0025] The melt spinning temperature is 180-200°C.

[0026] A polylactic acid fiber is prepared by the preparation method.

[0027] Beneficial effects of the present invention:

[0028] (1) The present invention prepares CNTs-coupling agent / long-chain unsaturated olefinic acid modified with a silane coupling agent, thereby improving the dispersibility of CNTs in a PLA matrix, thereby being able to better play a heterogeneous nucleation role, improving the crystallinity of PLA, and thus improving the heat resistance of PLA fibers.

[0029] (2) The present invention prepares lactide-modified CNTs-coupling agent / long-chain unsaturated olefinic acid-LA, and the C=C bond in the long-chain unsaturated olefinic acid easily reacts with the hydrogen on the relatively active tertiary carbon atom in the PLA molecule, and a PLA shell is coated on the surface of the CNTs-coupling agent / long-chain unsaturated olefinic acid, thereby solving the compatibility problem between CNTs and PLA fibers; at the same time, the long-chain unsaturated olefinic acid also helps to improve the compatibility between CNTs and PLA fibers and improve the hydrolysis resistance of PLA fibers; and because the PLA shell and CNTs are chemically connected by the coupling agent and the long-chain unsaturated olefinic acid, the coupling agent soft segment layer has a certain flexibility, thickness and deformation ability, thereby improving the toughness of the PLA fiber.

[0030] (3) The present invention prepares a CNTs-coupling agent / long-chain unsaturated olefinic acid-LA suitable for melt spinning of PLA fibers, and individually encapsulates CNTs in a core-shell structure, thereby improving the dispersibility of CNTs in the PLA matrix and the crystallinity of PLA, thereby improving the heat resistance of PLA fibers. DETAILED DESCRIPTION

[0031] The following will be combined with the embodiments of the present invention to clearly and completely describe the technical solutions in the embodiments of the present invention. Obviously, the described embodiments are only part of the embodiments of the present invention, not all of the embodiments. Based on the embodiments of the present invention, all other embodiments obtained by ordinary technicians in this field without creative work are within the scope of protection of the present invention.

[0032] Example 1

[0033] This embodiment provides a polylactic acid fiber, which is prepared by the following steps:

[0034] 1) Silane coupling agent surface modification of CNTs

[0035] The silane coupling agent KH550 was diluted with methanol and water, with the mass ratio of water: methanol: silane coupling agent being 10:70:20, and hydrochloric acid was added dropwise to adjust the pH value to 3-4, and hydrolyzed at room temperature for 1 hour to obtain a pre-hydrolyzed KH550 solution; 2g of pure CNTs and the hydrolyzed KH550 solution were weighed, with the mass fraction of the added KH550 in the pure CNTs being 3wt%, and the solution was heated to 70°C and stirred for 4h; the mixed solution was dried at 130°C for 8h, then taken out, ground, washed, vacuum filtered, and dried at 80°C for 12h to obtain CNTs with KH550 surface modification, which was recorded as CNTs-K (CNTs-coupling agent).

[0036] 2) Secondary modification of CNTs-coupling agent by long-chain unsaturated olefinic acid

[0037] Take 1 g of the dried CNTs-K and add it into 50 mL of deionized water, then add 2 g of oleic acid dropwise, heat the solution to 80 °C and stir for 10 h, take it out and wash it after the reaction is completed, and obtain CNTs modified with oleic acid for the second time, which is recorded as CNTs-KO (CNTs-coupling agent / long-chain unsaturated olefinic acid).

[0038] 3) Lactide ring-opening polymerization coating CNTs-coupling agent / long-chain unsaturated olefinic acid

[0039] Lactide was dried at 50 °C for 10 h, 0.4 g of the dried lactide was added into 100 mL of DMF, and 0.04 g of the above CNTs-KO was added at the same time, 0.0027 g of stannous octoate catalyst was added dropwise, and the temperature was raised to 140 °C under a nitrogen atmosphere and stirred for 20 h. After the reaction was completed, the polylactic acid not grafted to the CNTs was removed by centrifugation and washing with dichloromethane; the final product was washed with distilled water and dried at 80 °C for 6 h to obtain lactide-modified CNTs-KO-LA (CNTs-coupling agent / long-chain unsaturated olefinic acid-LA).

[0040] 4) Preparation of composite masterbatch

[0041] The polylactic acid chips, polylactic acid powder and CNTs-KO-LA were dried at 100°C for 12 hours, melt-blended, cooled and pelletized to prepare composite masterbatch. The amount of CNTs-KO-LA was 0.25wt% of the total mass of the composite masterbatch.

[0042] 5) Preparation of polylactic acid fibers

[0043] The polylactic acid chips and composite master batches are dried at 120° C. for 12 hours, blended, and melt-spun at 180-200° C. to obtain a polylactic acid fiber.

[0044] Example 2

[0045] The difference between this embodiment and Example 1 is that "the amount of CNTs-KO-LA is 0.25wt% of the total mass of the composite masterbatch." is changed to "the amount of CNTs-KO-LA is 0.5wt% of the total mass of the composite masterbatch."; the other raw materials and preparation process remain the same as in Example 1.

[0046] Example 3

[0047] The difference between this embodiment and Example 1 is that "the amount of CNTs-KO-LA is 0.25wt% of the total mass of the composite masterbatch." is changed to "the amount of CNTs-KO-LA is 1wt% of the total mass of the composite masterbatch."; the other raw materials and preparation process remain the same as in Example 1.

[0048] Example 4

[0049] The difference between this embodiment and Example 1 is that "the amount of CNTs-KO-LA is 0.25wt% of the total mass of the composite masterbatch." is changed to "the amount of CNTs-KO-LA is 2wt% of the total mass of the composite masterbatch."; the other raw materials and preparation process remain the same as in Example 1.

[0050] Example 5

[0051] The difference between this embodiment and embodiment 2 is that "the mass fraction of the added KH550 in the pure CNTs is 3wt%" is changed to "the mass fraction of the added KH550 in the pure CNTs is 4wt%"; the other raw materials and preparation process remain the same as in embodiment 2.

[0052] Example 6

[0053] The difference between this embodiment and embodiment 2 is that "the mass fraction of the added KH550 in the pure CNTs is 3wt%" is changed to "the mass fraction of the added KH550 in the pure CNTs is 5wt%"; the other raw materials and preparation process remain the same as in embodiment 2.

[0054] Example 7

[0055] Compared with Example 2, this example replaces oleic acid with linoleic acid, and the remaining raw materials and preparation steps remain the same as those in Example 2.

[0056] Example 8

[0057] Compared with Example 2, this example replaces oleic acid with 5-hexenoic acid, and the remaining raw materials and preparation steps remain the same as those in Example 2.

[0058] Example 9

[0059] Compared with Example 2, this example replaces oleic acid with erucic acid, and the remaining raw materials and preparation steps remain the same as those in Example 2.

[0060] Comparative Example 1

[0061] Compared with Example 1, the difference between this comparative example is that step 1), step 2) and step 3) are removed, and "CNTs-KO-LA" is changed to "CNTs"; the remaining raw materials and preparation process remain the same as Example 2.

[0062] Comparative Example 2

[0063] The difference between this comparative example and Example 1 is that step 3) is removed and "CNTs-KO-LA" is changed to "CNTs-KO"; the remaining raw materials and preparation process remain the same as Example 2.

[0064] Comparative Example 3

[0065] The difference between this comparative example and Example 1 is that step 1) and step 2) are removed, "CNTs-KO" is changed to "CNTs", and "CNTs-KO-LA" is changed to "CNTs-LA"; the remaining raw materials and preparation process remain the same as Example 2.

[0066] Performance tests were performed on Examples 1 to 9 and Comparative Examples 1 to 3. The heat resistance of the polylactic acid fiber samples was tested using a thermogravimetric analyzer. The breaking strength of the polylactic acid fiber was tested according to GB / T14337-2022 using an electronic single yarn strength tester. The obtained polylactic acid was placed in a NaOH aqueous solution with a pH of 12, and its mass loss rate was measured after being placed in a water bath environment in a constant temperature shaker for 144 hours. The results are shown in Table 1:

[0067] Table 1

[0068] project Initial decomposition temperature (℃) Breaking strength (cN / Tex) Mass loss rate (%) Example 1 304.2 13.7 18.3 Example 2 323.6 15.6 15.7 Example 3 320.8 15.0 16.5 Example 4 314.5 14.4 17.5 Example 5 318.8 14.6 16.7 Example 6 319.3 14.9 16.6 Example 7 326.8 16.3 14.9 Example 8 318.7 14.5 16.8 Example 9 324.5 16.0 15.3 Comparative Example 1 296.7 12.1 21.2 Comparative Example 2 300.5 13.1 20.1 Comparative Example 3 298.6 12.8 20.5

[0069] As can be seen from Table 1, the initial decomposition temperature of the polylactic acid fiber sample prepared in Example 2 is 323.6°C, the breaking strength is 15.6 cN / Tex, and the mass loss rate is 15.7%. Compared with Example 2, the initial decomposition temperature and breaking strength of the polylactic acid fiber samples prepared in Example 1, Example 3 and Example 4 are slightly reduced, and the mass loss rate is slightly increased, indicating that the amount of CNTs-coupling agent / long-chain unsaturated olefin acid-LA should not be too low or too high, and the optimal amount is 0.5wt%; compared with Example 2, the initial decomposition temperature and breaking strength of the polylactic acid fiber samples prepared in Example 5 and Example 6 are slightly reduced, and the mass loss rate is slightly increased, indicating that the mass fraction of the added silane coupling agent KH550 in pure CNTs should not be too high, and the optimal amount is 3wt%.

[0070] Compared with Example 2, the initial decomposition temperature and breaking strength of the polylactic acid fiber sample in Example 7 are improved, and the mass loss rate is reduced. This may be because the unsaturated olefinic acid linoleic acid has one more C=C double bond in its structure than oleic acid, which better solves the compatibility problem between CNTs and PLA; Compared with Example 2, the initial decomposition temperature and breaking strength of the polylactic acid fiber sample in Example 8 are reduced, and the mass loss rate is increased. Compared with Example 2, the initial decomposition temperature and breaking strength of the polylactic acid fiber sample in Example 9 are improved, and the mass loss rate is reduced, indicating that long-chain unsaturated olefinic acid helps to improve the compatibility between CNTs and PLA fibers and improve the hydrolysis resistance of PLA fibers.

[0071] Compared with Example 1, the initial decomposition temperature and breaking strength of the polylactic acid fiber sample in Comparative Example 1 are reduced, and the mass loss rate is increased, indicating that the addition of CNTs-coupling agent / long-chain unsaturated olefinic acid-LA helps to improve the heat resistance, toughness and hydrolysis resistance of the polylactic acid fiber; Compared with Comparative Example 1, after adding silane coupling agent and long-chain unsaturated olefinic acid to modify CNTs, the initial decomposition temperature and breaking strength of the polylactic acid fiber sample are increased, and the mass loss rate is reduced, which may be because the addition of silane coupling agent and long-chain unsaturated olefinic acid to modify CNTs improves the dispersibility of CNTs in the PLA matrix; Compared with Comparative Example 1, after adding lactide to modify CNTs, the initial decomposition temperature and breaking strength of the polylactic acid fiber sample are increased, and the mass loss rate is reduced.

[0072] It should be noted that, in this article, relational terms such as first and second, etc. are only used to distinguish one entity or operation from another entity or operation, and do not necessarily require or imply any such actual relationship or order between these entities or operations. Moreover, the terms "include", "comprise" or any other variants thereof are intended to cover non-exclusive inclusion, so that a process, method, article or device including a series of elements includes not only those elements, but also other elements not explicitly listed, or also includes elements inherent to such process, method, article or device.

[0073] Although embodiments of the present invention have been shown and described, it will be appreciated by those skilled in the art that various changes, modifications, substitutions and variations may be made to the embodiments without departing from the principles and spirit of the present invention, and that the scope of the present invention is defined by the appended claims and their equivalents.

Claims

1. A method for preparing polylactic acid fiber, characterized in that: Prepared by the following steps: 1) Silane coupling agent is used to modify the surface of CNTs to obtain CNTs-coupling agent; 2) The long-chain unsaturated olefinic acid performs secondary modification on the CNTs-coupling agent to obtain CNTs-coupling agent / long-chain unsaturated olefinic acid; 3) Lactide is ring-opening polymerized to coat CNTs-coupling agent / long-chain unsaturated olefinic acid to obtain CNTs-coupling agent / long-chain unsaturated olefinic acid-LA; 4) CNTs-coupling agent / long-chain unsaturated olefinic acid-LA is blended with polylactic acid chips to prepare composite masterbatch; 5) After the composite masterbatch and the polylactic acid chips are dried, they are blended and melt-spun to obtain a polylactic acid fiber.

2. The method for preparing polylactic acid fiber according to claim 1, characterized in that: CNTs are hydroxylated multi-walled carbon nanotubes, the silane coupling agent is KH550, and the long-chain unsaturated olefinic acid is one of oleic acid, linoleic acid, 5-hexenoic acid, and erucic acid.

3. The method for preparing polylactic acid fiber according to claim 1, characterized in that: The step of surface modification of CNTs by using silane coupling agent is as follows: adding CNTs to the hydrolyzed silane coupling agent solution to obtain a mixed solution, heating and stirring the mixed solution, drying the mixed solution, taking it out and grinding, washing, vacuum filtering, and drying to obtain CNTs with surface modification by silane coupling agent.

4. The method for preparing polylactic acid fiber according to claim 3, characterized in that: The mass fraction of the silane coupling agent in the CNTs is 3-5wt%.

5. The method for preparing polylactic acid fiber according to claim 1, characterized in that: The secondary modification of CNTs-coupling agent by long-chain unsaturated olefinic acid comprises the following steps: adding CNTs-coupling agent into deionized water, then adding long-chain unsaturated olefinic acid dropwise, heating and stirring the solution, washing and drying after the reaction is completed, and obtaining CNTs secondary modified with long-chain unsaturated olefinic acid.

6. The method for preparing polylactic acid fiber according to claim 1, characterized in that: The steps of encapsulating CNTs by ring-opening polymerization of lactide are as follows: adding dried lactide into DMF, adding CNTs-coupling agent / long-chain unsaturated olefinic acid and stannous octoate catalyst at the same time, heating to 130-140° C. under nitrogen atmosphere, stirring and reacting for 20-24 hours, and after the reaction is completed, centrifuging, washing with dichloromethane, washing with distilled water, and drying to obtain lactide-modified CNTs-coupling agent / long-chain unsaturated olefinic acid-LA.

7. The method for preparing polylactic acid fiber according to claim 6, characterized in that: The mass ratio of CNTs-coupling agent / long-chain unsaturated olefinic acid to lactide was 1:10; The mass ratio of stannous octoate catalyst to lactide is 1:

150.

8. The method for preparing polylactic acid fiber according to claim 1, characterized in that: The blending temperature in step 4) is 160°C-190°C; The amount of CNTs-coupling agent / long-chain unsaturated olefinic acid-LA used is 0.25-2wt% of the total mass of the composite masterbatch.

9. The method for preparing polylactic acid fiber according to claim 1, characterized in that: The drying temperature of the polylactic acid chips and the composite masterbatch in step 5) is 110-120° C. and the drying time is 10-12 hours; The melt spinning temperature is 180-200°C.

10. A polylactic acid fiber, characterized in that: Prepared by the preparation method according to any one of claims 1 to 9.