Preparation method of colored aramid fiber non-woven fabric with closed structure

By adding pigments and polymers to amide polar organic solvents, and combining multi-stage stretching and heat setting technology, the problem of loose structure and single color of aramid non-woven fabrics is solved, achieving tight sealing and diversified colors. Made of aramid non-woven fabrics with excellent performance.

CN118727263APending Publication Date: 2024-10-01GANZHOU LONGPONT MATERIAL TECH CO LTD
View PDF 6 Cites 0 Cited by

Patent Information

Application Number
CN202411058953.3
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Filing Date
2024-08-02
Publication Date
2024-10-01

AI Technical Summary

Technical Problem

The existing aramid non-woven fabric has a loose structure, cannot form a dense structure, and has a single color, making it difficult to meet the needs of diverse structural appearance.

Method used

Colored pigments and meta-aramid polymers are added to amide polar organic solvents, and through vacuum degassing, spinneret forming, multi-stage stretching, and heat setting, colored aramid fibers are formed. Processed to form a colored aramid non-woven fabric with a closed structure.

Benefits of technology

Aramid non-woven fabrics with tightly closed surface structures and diversified colors are realized, which have excellent thermal stability, flame retardancy, chemical stability and insulation, and achieve a closed structure.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN118727263A_ABST
    Figure CN118727263A_ABST
Patent Text Reader

Abstract

The invention belongs to the technical field of aramid fiber non-woven fabrics, and discloses a preparation method of a colored aramid fiber non-woven fabric with a closed structure, which comprises the following steps: preparing colored aramid fibers, producing the colored aramid fiber non-woven fabric, hot-pressing the colored aramid fiber non-woven fabric, adding sufficient colored pigment and meta-position aramid fiber polymer into an amide polar organic solvent, fully stirring, and drying to obtain the colored aramid fiber non-woven fabric with the closed structure. Then filtering and vacuum defoaming are carried out, a defoamed mixture solution is conveyed into a spinning nozzle through a metering pump to be extruded into filaments, the filaments are sprayed out in coagulating bath forming liquid to form nascent fibers, and the aramid fiber finished product is obtained through multi-stage stretching, multi-section groove type and spraying type water washing, drying and heat setting. The method comprises the following steps: preparing a colored aramid fiber finished product, quantitatively conveying the colored aramid fiber finished product to an opener for carding, carrying out lapping, drafting, spunlace and drying to form a non-woven fabric with a loose structure, preheating the prepared non-woven fabric in a preheating box, and carrying out hot pressing on the non-woven fabric through a large-diameter hot roller to obtain a colored aramid fiber non-woven fabric finished product with a closed structure. The black aramid fiber non-woven fabric is uniform in color and luster and has excellent thermal stability, flame retardance, chemical stability, insulativity and the like, and the black aramid fiber non-woven fabric reaches a structure closed state through detection.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The invention belongs to the technical field of aramid nonwoven fabrics, and in particular relates to a method for preparing a colored aramid nonwoven fabric with a closed structure. Background Art

[0002] Aramid non-woven fabrics made of aramid fibers have excellent thermal stability, flame retardancy, chemical stability, and insulation properties. They are also light in weight and have outstanding mechanical properties. They can be used as insulating materials, heat-insulating materials, packaging materials, and protective materials. They are widely used in aerospace, electronic transportation, medical care, workwear protection, and other industries. As demand continues to increase, diverse requirements are also placed on the structure and appearance of aramid non-woven fabrics.

[0003] Application No. KR20160048676 provides a method for manufacturing aromatic polyamide non-woven fabrics using copolyamide aromatic polyamide membranes to simplify the polymerization steps of aramid polymer solutions. However, this method has strict requirements on the membrane manufacturing process and cannot ensure the industrial production of smooth and dense membrane structures.

[0004] Application No. US201515032804 provides a method for manufacturing aramid stab-proof fabric using a water jetting method, which solves the problem that the stab-proof vest is inevitably heavy and hard, causing the wearer to move slowly, because the multiple layers of stab-proof materials are stacked so that a knife or awl cannot penetrate, and thin metal plates or high-strength plastics and fabrics coated with inorganic particles are used. However, this method has the problem that the process for producing aramid staple fiber webs is too complicated and the production efficiency is low.

[0005] Application No. US3869428 provides a method for preparing an aramid staple fiber non-woven fabric, comprising adding isophthaloyl chloride in an equal molar amount to the above-mentioned metaphenylenediamine to an organic solvent containing metaphenylenediamine, polymerizing to prepare an aramid polymer, then dissolving the prepared polymer in a concentrated sulfuric acid solution, preparing fine fibers by spinning and other methods to manufacture aramid yarns, then cutting the manufactured aramid yarns to manufacture aramid staple fibers, then supplying and processing the above-mentioned aramid staple fibers on a card punching machine to manufacture an aramid staple fiber web, then making the above-mentioned aramid staple fiber web into pinholes to manufacture an aramid staple fiber non-woven fabric. The aramid non-woven fabric provided by this scheme has a loose structure and cannot form a dense structure, and the non-woven fabric has a single color. Summary of the invention

[0006] The object of the present invention is to provide a method for preparing a colored aramid non-woven fabric with a closed structure, so as to solve the problems in the prior art that the aramid non-woven fabric has a loose structure and cannot form a dense structure, and the non-woven fabric has a single color.

[0007] In order to achieve the above object, the present invention provides the following technical solution: a method for preparing a colored aramid non-woven fabric with a closed structure, the method for preparing an aramid non-woven fabric with a tightly closed surface structure and diversified colors, comprising the following steps: Sp1: To prepare colored aramid fiber, sufficient colored pigment and meta-aramid polymer are added to an amide polar organic solvent, and the three are fully stirred and dispersed into a uniform solution. The solution is then filtered through a filter medium, and vacuum degassing is performed at 60-80°C for no more than 5 hours to form a mixture solution. The degassed mixture solution is transported to a spinneret through a metering pump to be extruded into filaments, and then sprayed out in a coagulation bath forming liquid to form primary fibers. The coagulant in the coagulation bath diffuses into the stock solution stream, and the solvent in the stock solution diffuses into the coagulation bath forming liquid. In wet spinning, when the spinning stock solution is extruded from the spinneret hole, the stock solution has not yet solidified, and the tensile strength of the spinning line is very low, and it cannot withstand excessive spinneret stretching. Therefore, wet forming usually adopts spinneret negative stretching, zero stretching or small positive stretching; and then after multi-stage stretching, multi-stage trough and shower washing, drying and heat setting, the aramid fiber product is finally obtained; The purpose of multi-stage stretching is to improve the physical properties of the primary fiber. The stretching process is not only a process of changing the fiber geometry, but also a process of reorganizing and forming the fiber structure, which increases the orientation degree of the macromolecular chains in the low-order region of the fiber along the fiber axis, accompanied by some structural changes. In production, under the premise of low tensile stress (to avoid the formation of hair), the stretching temperature, the degree of plasticization of the fiber, the stretching speed, the length of the fiber between the stretching rollers, or the use of multi-stage stretching should be changed to ensure that the high elastic shape develops smoothly during stretching. The heat setting temperature is 320-350℃, and it is divided into three stages, including the relaxation stage, the setting stage and the structural fixing stage. The relaxation stage makes the loose and disordered intermolecular forces in the amorphous area of ​​the fiber weaken rapidly and the internal stress relaxes; the setting stage increases the intermolecular forces in the relaxed area of ​​the fiber and makes the structure more compact and orderly; the structural fixing stage makes the structure formed in the setting stage be fixed rapidly; Sp2: Produce colored aramid non-woven fabrics. The finished colored aramid fibers are quantitatively transported to the opening machine for combing. After laying, drawing, spunlacing, and drying, the non-woven fabrics with loose structure are formed. Sp3: Hot pressing colored aramid non-woven fabric. The non-woven fabric is preheated in a preheating box, and then hot pressed by a large-diameter hot rolling roller to obtain a finished colored aramid non-woven fabric with a closed structure. The preheating is to provide heat in the thickness direction of the non-woven fabric to facilitate the heat transfer inside the non-woven fabric during subsequent hot pressing.

[0008] Preferably, the amide polar organic solvent is dimethylacetamide, and the concentration of the amide polar organic solvent is not less than 80-90%.

[0009] Preferably, the colored pigment is an organic pigment, and the colored pigment is mixed and ground with an amide polar organic solvent by a fine grinder, and the inherent viscosity of the meta-aramid polymer is set to between 6-10.

[0010] Preferably, the pore size of the filter medium is set to 10-20 μm.

[0011] Preferably, the coagulation bath molding liquid is an aqueous solution containing an organic solvent, the organic solvent is DMSO, DMF or DMAC, and the concentration of the organic solvent is 20-60%wt.

[0012] Preferably, the heat setting temperature is set at 320-350°C.

[0013] Preferably, the opener uses a large cylinder to improve the raising efficiency and lightness, and the opener speed is set to 1200-1400m / min. The spunlace process adopts a three-pass spunlace process, the spunlace pressure of the first pass is set to 4-8MPa, the spunlace pressure of the second pass is set to 8-10MPa, and the spunlace pressure of the third pass is set to 10-15MPa. In order to achieve heat setting without destroying the structure of the aramid fiber, the drying temperature is 300-330°C.

[0014] Preferably, the preheating box temperature is set to 180-200° C., the hot rolling roller diameter is set to 700-900 mm, the hot rolling temperature is set to 290-320° C., and the hot rolling roller pressure is set to 4-10 MPa.

[0015] The beneficial effects of the present invention are as follows: The invention comprises the following steps: adding sufficient amount of colored pigment and meta-aramid polymer into an amide polar organic solvent, fully stirring and dispersing the three into a uniform solution, filtering and vacuum degassing, conveying the degassed mixture solution into a spinneret through a metering pump for extrusion into filaments, spraying out in a coagulation bath forming liquid to form primary fibers, and finally obtaining aramid fiber finished products through multi-stage stretching, multi-section trough-type and shower-type water washing, drying and heat setting. Finally, the colored aramid fiber finished products are quantitatively conveyed to an opener for combing, and are formed into a non-woven fabric with a loose structure after web laying, drawing, water spunlacing and drying. Finally, the prepared non-woven fabric is preheated in a preheating box, and then the non-woven fabric is heat-pressed by a large-diameter hot rolling roller to obtain a colored aramid non-woven fabric finished product with a closed structure. The black aramid non-woven fabric has uniform color and excellent thermal stability, flame retardancy, chemical stability, insulation and other properties. According to detection, the black aramid non-woven fabric reaches a closed structure state. BRIEF DESCRIPTION OF THE DRAWINGS

[0016] Figure 1 It is a flow chart of the present invention. DETAILED DESCRIPTION

[0017] The following will be combined with the drawings in the embodiments of the present invention to clearly and completely describe the technical solutions in the embodiments of the present invention. Obviously, the described embodiments are only part of the embodiments of the present invention, not all of the embodiments. Based on the embodiments of the present invention, all other embodiments obtained by ordinary technicians in this field without creative work are within the scope of protection of the present invention.

[0018] Example: like Figure 1 As shown, an embodiment of the present invention provides a method for preparing a colored aramid non-woven fabric with a closed structure. First, a black organic pigment is mixed and ground with a dimethylacetamide organic solvent through a fine grinder until the particle size is 5um, and then a meta-aramid polymer with an inherent viscosity of 7 and a black organic pigment are added to a coagulation bath molding liquid with a DMAC content of 85% in a ratio of 1:100, and mixed and stirred for 2 hours, wherein the mixture accounts for 20% and the pH is 6.5.

[0019] The mixed solution is then filtered through a 10um filter medium, vacuum degassed, and transported to a spinneret through a metering pump for extrusion into filaments, which are then sprayed out into a coagulation bath molding liquid with a DMAC concentration of 50% to become primary fibers. After three-stage stretching (stretching ratio 3:4), three-stage trough water washing and six-stage jet water washing, 200°C drying, and 330°C high-temperature shaping, the finished aramid fiber with high color fastness and uniform black color is finally obtained.

[0020] The finished black aramid fiber products are then quantitatively transported to the large cylinder opening machine for combing. The speed of the large cylinder opening machine is set to 1300m / min. After a series of processes such as laying, stretching, spunlace, and drying at 300℃, a loosely structured black aramid non-woven fabric is formed. The pressure of the first spunlace is set to 6MPa, the second spunlace pressure is set to 8MPa, and the third spunlace pressure is set to 12MPa.

[0021] Finally, the black aramid nonwoven fabric is preheated at 180°C in a preheating box, and then hot-pressed at 320°C, 8MPa, and 5m / min by a hot-rolling roller with a diameter of 800mm to obtain a black aramid nonwoven fabric product with a compact structure.

[0022] The black aramid nonwoven fabric has uniform color and excellent thermal stability, flame retardancy, chemical stability and insulation properties. After testing, the black aramid nonwoven fabric has a quantitative weight of 95g / , thickness 0.11mm, tightness 0.86g / , air permeability 0.03um / pa.s, has reached a closed structural state.

[0023] It should be noted that, in this article, relational terms such as first and second, etc. are only used to distinguish one entity or operation from another entity or operation, and do not necessarily require or imply any such actual relationship or order between these entities or operations. Moreover, the terms "include", "comprise" or any other variants thereof are intended to cover non-exclusive inclusion, so that a process, method, article or device including a series of elements includes not only those elements, but also other elements not explicitly listed, or also includes elements inherent to such process, method, article or device.

[0024] Although embodiments of the present invention have been shown and described, it will be appreciated by those skilled in the art that various changes, modifications, substitutions and variations may be made to the embodiments without departing from the principles and spirit of the present invention, and that the scope of the present invention is defined by the appended claims and their equivalents.

Claims

1. A method for preparing a colored aramid nonwoven fabric with a closed structure, the method being used to prepare an aramid nonwoven fabric with a tightly closed surface structure and diversified colors. It is characterized in that The following steps are involved: Sp1: Preparation of colored aramid fiber: adding a sufficient amount of colored pigment and meta-aramid polymer to an amide polar organic solvent, fully stirring and dispersing the three into a uniform solution, filtering the solution through a filter medium, vacuum degassing at 60-80°C for no more than 5 hours to form a mixture solution, conveying the degassed mixture solution to a spinneret through a metering pump for extrusion into filaments, spraying out in a coagulation bath forming liquid to form primary fibers, and finally obtaining aramid fiber products after multi-stage stretching, multi-stage tank and shower washing, drying and heat setting; Sp2: Produce colored aramid non-woven fabrics. The finished colored aramid fibers are quantitatively transported to the opening machine for combing. After laying, drawing, spunlacing, and drying, the non-woven fabrics with loose structure are formed. Sp3: Hot pressing colored aramid non-woven fabric, preheating the prepared non-woven fabric in a preheating box, and then hot pressing the non-woven fabric through a large-diameter hot rolling roller to obtain a finished colored aramid non-woven fabric with a closed structure.

2. A method for preparing a structurally closed colored aramid nonwoven fabric according to claim 1, Features: The amide polar organic solvent is dimethylacetamide, and the concentration of the amide polar organic solvent is not less than 80-90%.

3. The method for preparing a structurally closed colored aramid nonwoven fabric according to claim 1, Features: The colored pigment is an organic pigment, and the colored pigment is mixed and ground with an amide polar organic solvent by a fine grinder, and the inherent viscosity of the meta-aramid polymer is set to be between 6 and 10.

4. The method for preparing a structurally closed colored aramid nonwoven fabric according to claim 1, Features: The pore size of the filter medium is set to 10-20 μm.

5. The method for preparing a structurally closed colored aramid nonwoven fabric according to claim 1, Features: The coagulation bath molding liquid is set as an aqueous solution containing an organic solvent, the organic solvent is set as DMSO, DMF or DMAC, and the concentration of the organic solvent is set to 20-60%wt.

6. The method for preparing a structurally closed colored aramid nonwoven fabric according to claim 1, Features: The heat setting temperature is set at 320-350°C.

7. The method for preparing a structurally closed colored aramid nonwoven fabric according to claim 1, Features: The opening machine uses a large cylinder, and the opening machine speed is set to 1200-1400m / min. The spunlace process adopts a three-pass spunlace process. The spunlace pressure of the first pass is set to 4-8MPa, the spunlace pressure of the second pass is set to 8-10MPa, and the spunlace pressure of the third pass is set to 10-15MPa.

8. The method for preparing a structurally closed colored aramid nonwoven fabric according to claim 1, Features: The preheating box temperature is set to 180-200° C., the hot rolling roller diameter is set to 700-900 mm, the hot rolling temperature is set to 290-320° C., and the hot rolling roller pressure is set to 4-10 MPa.

Citation Information

Patent Citations

  • Method for preparing colored meta-aramid fiber by one-step process

    CN113355764A

  • Preparation method of aramid fiber lithium battery diaphragm

    CN116334837A

  • Papermaking-grade meta-position aramid fiber surface brooming preparation method

    CN117306013A

  • Aramid nonwoven fabric and its production

    JP1995331570A

  • Composition of freeze-dried formulation for tissue repair treatment