Preparation method of hydrophobic polyester fiber, hydrophobic polyester fiber and fabric

By using supercritical carbon dioxide for waterless dyeing on polyester fiber and attaching a hydrophobic agent, the problem of high water cost and pollution in the traditional water medium dyeing process has been solved, the hydrophobic modification of polyester fiber has been achieved, and the performance of the fiber has been improved. and application areas.

CN118727439APending Publication Date: 2024-10-01陶鹏
View PDF 0 Cites 0 Cited by

Patent Information

Application Number
CN202310325748.8
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Filing Date
2023-03-29
Publication Date
2024-10-01

AI Technical Summary

Technical Problem

The traditional water medium dyeing process involves high water costs, serious wastewater pollution, and polyester fiber does not have hydrophobic properties, which limits its application fields.

Method used

Supercritical carbon dioxide is used as the dyeing medium, and the hydrophobic agent is dissolved in it. The hydrophobic agent is attached to the surface of the polyester fiber through an anhydrous dyeing process to form a hydrophobic polyester fiber, thereby achieving hydrophobic modification of the polyester fiber without adding additives. , simplify the process flow.

Benefits of technology

It achieves the long-lasting hydrophobicity and oleophobicity of polyester fiber, reduces chemical pollution, expands the application fields of the fiber, and improves production efficiency. It has excellent properties such as self-cleaning, anti-adhesion, antifouling, antibacterial, and waterproof.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN118727439A_ABST
    Figure CN118727439A_ABST
Patent Text Reader

Abstract

The invention provides a preparation method of a hydrophobic polyester fiber, the hydrophobic polyester fiber and a fabric, and is suitable for the field of textile dyeing and finishing processes, the preparation method of the hydrophobic polyester fiber comprises the steps that supercritical carbon dioxide is prepared, the temperature of the supercritical carbon dioxide is larger than or equal to 31.1 DEG C, and the pressure of the supercritical carbon dioxide is larger than or equal to 7.39 Mpa; dissolving a water repellent agent in supercritical carbon dioxide; and dissolving the polyester fiber to be dyed in the supercritical carbon dioxide of the water repellent agent for waterless dyeing, so that the water repellent agent is attached to the surface of the polyester fiber to form the hydrophobic polyester fiber.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The invention relates to the technical field of waterless dyeing, and in particular to a preparation method of hydrophobic polyester fiber, the hydrophobic polyester fiber and fabric. Background Art

[0002] In order to solve the problems of high pollution and high energy consumption in traditional water-based dyeing, non-aqueous raw materials such as supercritical carbon dioxide formed from industrial waste gas carbon dioxide are used instead of water as the dyeing medium, and waterless dyeing of textile products is carried out under closed conditions. Compared with the water-based dyeing process, the non-aqueous dyeing process is water-free, which reduces water pollution during dyeing and finishing. Using supercritical carbon dioxide instead of water to dye textiles is an innovation in traditional dyeing processing, which eliminates the generation of wastewater at the source.

[0003] Surfaces with a contact angle greater than 90° with water are usually called hydrophobic surfaces. The larger the contact angle, the better the hydrophobic properties of the surface. Superhydrophobicity refers to a wetting state with a contact angle greater than 150°. The special wettability of superhydrophobic surfaces gives them excellent properties such as self-cleaning, anti-adhesion, anti-fouling and antibacterial, and waterproofing, which has attracted great attention and research interest. Polyester fiber is one of the most widely used synthetic fibers by humans. Polyester fiber is easily wetted by water and does not have water-repellent properties. Therefore, hydrophobic modification of polyester fiber can expand its application field. Since supercritical carbon dioxide technology does not require the participation of water in the textile dyeing process, there is no need for cleaning, drying, and other operations after dyeing, which greatly simplifies the process and improves production efficiency.

[0004] Therefore, inventing a method for preparing hydrophobic polyester fibers has become a technical problem that needs to be solved urgently. Summary of the invention

[0005] The invention aims to solve or improve the technical problems of high water cost and serious wastewater pollution in the traditional water bath dyeing process.

[0006] A first aspect of the present invention is to provide a method for preparing hydrophobic polyester fiber.

[0007] A second aspect of the present invention is to provide a hydrophobic polyester fiber.

[0008] A third aspect of the present invention is to provide a fabric.

[0009] The method for preparing a hydrophobic polyester fiber provided by the present invention comprises: preparing supercritical carbon dioxide, wherein the temperature of the supercritical carbon dioxide is greater than or equal to 31.1° C., and the pressure of the supercritical carbon dioxide is greater than or equal to 7.39 Mpa; dissolving a hydrophobic agent in the supercritical carbon dioxide; and dissolving polyester fibers to be dyed in the supercritical carbon dioxide containing the hydrophobic agent for waterless dyeing, so that the hydrophobic agent is attached to the surface of the polyester fibers, so as to form the hydrophobic polyester fibers.

[0010] The preparation method of the hydrophobic polyester fiber provided by the present invention uses supercritical carbon dioxide as a medium to modify the polyester fiber to be hydrophobic. Compared with the existing padding process, spraying process, foaming process, washing and other methods, no auxiliary agent needs to be added during the dyeing process, which greatly shortens the modification step, saves costs, reduces the pollution of chemicals to the environment, and has positive significance for the development of polyester fiber products. In addition, the hydrophobic polyester fiber prepared by the present invention has excellent properties such as self-cleaning, anti-adhesion, anti-fouling and antibacterial, and waterproof due to the special wettability of its super-hydrophobic surface. In addition, the present application also broadens the scope of use of supercritical carbon dioxide fluid, is not limited to the dyeing of ordinary dyes, and greatly improves the process flow of preparing hydrophobic polyester fibers.

[0011] In the above technical solution, the hydrophobic agent includes a fluoride with 6 carbon atoms or a bromide with 6 carbon atoms.

[0012] In this technical solution, using fluoride with 6 carbon atoms or bromide with 6 carbon atoms as a hydrophobic agent can make the polyester fiber have lasting hydrophobicity and oleophobicity, and the dyed fiber is harmless to the human body and has good safety in use.

[0013] In the above technical scheme, in the step of dissolving the polyester fiber to be dyed in the supercritical carbon dioxide of the hydrophobic agent for waterless dyeing, the temperature of the supercritical carbon dioxide of the hydrophobic agent is greater than or equal to 60°C and less than or equal to 80°C; the pressure of the supercritical carbon dioxide of the hydrophobic agent is greater than or equal to 15Mpa and less than or equal to 30Mpa; the dyeing time is greater than or equal to 2h and less than or equal to 6h.

[0014] In this technical solution, during the waterless dyeing process, the temperature of the supercritical carbon dioxide in the hydrophobic agent is greater than or equal to 60°C and less than or equal to 80°C, that is, the dyeing temperature is greater than or equal to 60°C and less than or equal to 80°C. Further, the dyeing temperature is 70°C, and the pressure of the supercritical carbon dioxide in the hydrophobic agent is greater than or equal to 15Mpa and less than or equal to 30Mpa, that is, the dyeing pressure is greater than or equal to 15Mpa and less than or equal to 30Mpa. Further, the dyeing pressure is 25Mpa, and the dyeing time is greater than or equal to 2h and less than or equal to 6h. Further, the dyeing time is greater than or equal to 4h. Due to the particularity of the dye of the present application, it is more concerned about the hydrophobicity and oleophobicity of the polyester fiber. Therefore, the dyeing temperature and pressure of the present application are lower than those of the existing dyes, and the dyeing time is longer, thereby ensuring the dyeing effect, so that the surface of the polyester fiber is evenly dyed, and the hydrophobic agent can better adhere to the surface of the polyester fiber and is not easy to fall off.

[0015] In the above technical scheme, the temperature of the supercritical carbon dioxide is greater than or equal to 60°C and less than or equal to 80°C, the pressure of the supercritical carbon dioxide is greater than or equal to 15Mpa and less than or equal to 30Mpa, and the step of preparing supercritical carbon dioxide includes: opening the carbon dioxide storage tank to continuously introduce carbon dioxide into the first space, turning on the heating device to heat the carbon dioxide in the first space, when the temperature reaches the first preset temperature and the pressure reaches the first preset pressure, pressurizing the first space through the boosting device, closing the carbon dioxide storage tank when the pressure reaches the second preset pressure, and heating the carbon dioxide in the first space to the second preset temperature through the heating device to obtain supercritical carbon dioxide.

[0016] In this technical solution, using supercritical carbon dioxide with a temperature of 60°C to 80°C and a pressure of 15Mpa to 30Mpa as the dyeing environment can ensure uniform dyeing effect and improve the durability of the hydrophobic agent. In addition, in the step of preparing supercritical carbon dioxide, carbon dioxide is first introduced into the first space through a carbon dioxide storage tank, and when the temperature of the carbon dioxide in the first space reaches a first preset temperature and the pressure reaches a first preset pressure, the boosting device is turned on to boost the first space, so that the preparation efficiency of supercritical carbon dioxide can be improved.

[0017] In the above technical solution, the first preset temperature is greater than or equal to 40°C and less than or equal to 60°C; the first preset pressure is greater than or equal to 8Mpa and less than or equal to 15Mpa; the second preset temperature is greater than or equal to 60°C and less than or equal to 80°C; the second preset pressure is greater than or equal to 15Mpa and less than or equal to 30Mpa.

[0018] In the above technical scheme, before the step of dissolving the polyester fiber to be dyed in the supercritical carbon dioxide of the hydrophobic agent for waterless dyeing, the step also includes: continuously introducing supercritical carbon dioxide into the surface of the polyester fiber to remove the oil in the polyester fiber by the supercritical carbon dioxide, wherein the continuous introduction time of the supercritical carbon dioxide is greater than or equal to 5 minutes and less than or equal to 25 minutes.

[0019] In this technical solution, before dissolving the polyester fiber to be dyed in the supercritical carbon dioxide of the hydrophobic agent for anhydrous dyeing, supercritical carbon dioxide is first continuously introduced into the surface of the polyester fiber to remove the oil in the polyester fiber through the supercritical carbon dioxide, which can improve the dyeing effect in the later stage and improve the binding force between the hydrophobic agent and the surface of the polyester fiber. On the other hand, deoiling by supercritical carbon dioxide is green and environmentally friendly compared to traditional deoiling methods and has high deoiling efficiency. In addition, the deoiling time is controlled to be greater than or equal to 5 minutes and less than or equal to 25 minutes, which can ensure that the polyester fiber can be fully deoiled and avoid too long time and reduced efficiency.

[0020] In the above technical solution, before the step of dissolving the polyester fiber to be dyed in the supercritical carbon dioxide of the hydrophobic agent for waterless dyeing, the step also includes: continuously introducing carbon dioxide into the space where the polyester fiber is located to remove the air in the space where the polyester fiber is located.

[0021] In this technical solution, before the step of dissolving the polyester fiber to be dyed in the supercritical carbon dioxide of the hydrophobic agent for waterless dyeing, carbon dioxide is continuously introduced into the space where the polyester fiber is located to remove the air in the space where the polyester fiber is located. This ensures that the supercritical carbon dioxide is in full contact with the polyester fiber, thereby improving the dyeing efficiency and the bonding force between the hydrophobic agent and the surface of the polyester fiber.

[0022] In the above technical solution, the method for preparing the hydrophobic polyester fiber further includes: separating the hydrophobic agent that has not been used to anhydrous dye the polyester fiber from the supercritical carbon dioxide; and recovering the supercritical carbon dioxide after the hydrophobic agent is separated.

[0023] In this technical solution, after waterless dyeing, the hydrophobic agent that has not been used to dye the polyester fiber is separated from the supercritical carbon dioxide, and the supercritical carbon dioxide after the hydrophobic agent is separated is recovered, so that the carbon dioxide can be recycled and the energy utilization rate can be improved.

[0024] The second aspect of the present invention provides a hydrophobic polyester fiber. The hydrophobic polyester fiber provided by the present invention is prepared by the preparation method of the hydrophobic polyester fiber according to any technical solution of the first aspect of the present application.

[0025] The third aspect of the present invention provides a fabric, and the material of the fabric provided by the present invention includes the hydrophobic polyester fiber of the technical solution of the second aspect of the present application.

[0026] Additional aspects and advantages of the present invention will become apparent in the following description or may be learned through practice of the present invention. BRIEF DESCRIPTION OF THE DRAWINGS

[0027] The above and / or additional aspects and advantages of the embodiments of the present invention will become apparent and easily understood from the description of the embodiments in conjunction with the following drawings, in which:

[0028] Figure 1 A schematic flow chart of a method for preparing polyester fiber provided by an embodiment of the present invention is shown;

[0029] Figure 2 A schematic flow chart of a method for preparing polyester fiber provided by another embodiment of the present invention is shown;

[0030] Figure 3A schematic flow chart of a method for preparing polyester fiber provided by another embodiment of the present invention is shown;

[0031] Figure 4 A schematic flow chart of a method for preparing polyester fiber provided in yet another embodiment of the present invention is shown;

[0032] Figure 5 A schematic structural diagram of a waterless dyeing device for polyester fibers provided in an embodiment of the present invention is shown;

[0033] Figure 6 Another schematic structural diagram of the waterless dyeing device for polyester fibers provided in an embodiment of the present invention is shown.

[0034] in, Figure 5 and Figure 6 The corresponding relationship between the component names and numbers in is as follows:

[0035] 1 dye kettle, 2 dyeing kettle, 3 separation and recovery device, 4 heating device, 5 condenser, 6 carbon dioxide storage tank, 7 circulation pump, 8 compression pump, 9 valve, 10 carbon dioxide steel tank, 11 refrigeration unit, 12 refrigerant tank, 13 ethylene glycol pump, 14 thermal oil heater. DETAILED DESCRIPTION

[0036] In order to more clearly understand the above aspects, features and advantages of the embodiments of the present invention, the embodiments of the present invention are further described in detail below in conjunction with the accompanying drawings and specific implementation methods. It should be noted that the embodiments of the present application and the features in the embodiments can be combined with each other without conflict.

[0037] In the following description, many specific details are set forth to facilitate a full understanding of the embodiments according to the present invention. However, the embodiments according to the present invention may also be implemented in other ways different from those described herein. Therefore, the protection scope of the embodiments according to the present invention is not limited to the specific embodiments disclosed below.

[0038] like Figure 1 As shown, a method for preparing polyester fiber provided by one embodiment of the present invention comprises the following steps:

[0039] S102; preparing supercritical carbon dioxide, wherein the temperature of the supercritical carbon dioxide is greater than or equal to 31.1°C, and the pressure of the supercritical carbon dioxide is greater than or equal to 7.39Mpa;

[0040] S104: dissolving a hydrophobic agent in supercritical carbon dioxide;

[0041] S106: dissolving the polyester fiber to be dyed in supercritical carbon dioxide of a hydrophobic agent for waterless dyeing, so that the hydrophobic agent adheres to the surface of the polyester fiber to form a hydrophobic polyester fiber.

[0042] The preparation method of the hydrophobic polyester fiber provided by the present invention first prepares supercritical carbon dioxide, wherein the temperature of the supercritical carbon dioxide is greater than or equal to 31.1°C, and the pressure of the supercritical carbon dioxide is greater than or equal to 7.39Mpa, then the hydrophobic agent is dissolved in the supercritical carbon dioxide, and then the polyester fiber to be dyed is dissolved in the supercritical carbon dioxide of the hydrophobic agent for anhydrous dyeing, so that the hydrophobic agent is attached to the surface of the polyester fiber to form the hydrophobic polyester fiber. The preparation method of the hydrophobic polyester fiber provided by the present invention uses supercritical carbon dioxide as a medium to modify the polyester fiber to be hydrophobic. Compared with the existing padding processing, spray processing, foam processing, water washing and other methods, no auxiliary agent needs to be added during the dyeing process, which greatly shortens the modification step, saves costs, reduces the pollution of chemicals to the environment, and has positive significance for the development of polyester fiber products. In addition, the hydrophobic polyester fiber prepared by the present invention has excellent properties such as self-cleaning, anti-adhesion, anti-fouling and antibacterial, and waterproof due to the special wettability of its super-hydrophobic surface.

[0043] In the above technical solution, the hydrophobic agent includes a fluoride with 6 carbon atoms or a bromide with 6 carbon atoms. Using a fluoride with 6 carbon atoms or a bromide with 6 carbon atoms as a hydrophobic agent can make the polyester fiber have a lasting hydrophobic and oleophobic property, and the dyed fiber is harmless to the human body and has good safety in use.

[0044] In the above technical scheme, during the waterless dyeing process, the temperature of the supercritical carbon dioxide in the hydrophobic agent is greater than or equal to 60°C and less than or equal to 80°C, that is, the dyeing temperature is greater than or equal to 60°C and less than or equal to 80°C, further, the dyeing temperature is 70°C, and the pressure of the supercritical carbon dioxide in the hydrophobic agent is greater than or equal to 15Mpa and less than or equal to 30Mpa, that is, the dyeing pressure is greater than or equal to 15Mpa and less than or equal to 30Mpa, further, the dyeing pressure is 25Mpa, and the dyeing time is greater than or equal to 2h and less than or equal to 6h, further, the dyeing time is greater than or equal to 4h. Due to the particularity of the dye of the present application, it is more concerned about the hydrophobicity and oleophobicity of the polyester fiber. Therefore, the dyeing temperature and pressure of the present application are lower than the dyeing temperature and pressure of the existing dyes, and the dyeing time is longer, thereby ensuring the dyeing effect, so that the surface of the polyester fiber is evenly dyed, and the hydrophobic agent can better adhere to the surface of the polyester fiber and is not easy to fall off.

[0045] In the above technical scheme, the temperature of the supercritical carbon dioxide is greater than or equal to 60°C and less than or equal to 80°C, the pressure of the supercritical carbon dioxide is greater than or equal to 15Mpa and less than or equal to 30Mpa, and the step of preparing the supercritical carbon dioxide includes: opening the carbon dioxide storage tank 6 to continuously introduce carbon dioxide into the first space, opening the heating device 4 to heat the carbon dioxide in the first space, when the temperature reaches the first preset temperature and the pressure reaches the first preset pressure, pressurizing the first space by the supercharging device, closing the carbon dioxide storage tank 6 when the pressure reaches the second preset pressure, and heating the carbon dioxide in the first space to the second preset temperature by the heating device 4 to obtain supercritical carbon dioxide. Using supercritical carbon dioxide with a temperature of 60°C to 80°C and a pressure of 15Mpa to 30Mpa as the dyeing environment can ensure uniform dyeing effect and improve the durability of the hydrophobic agent.

[0046] In the above technical solution, the first preset temperature is greater than or equal to 40°C and less than or equal to 60°C; the first preset pressure is greater than or equal to 8Mpa and less than or equal to 15Mpa; the second preset temperature is greater than or equal to 60°C and less than or equal to 80°C; the second preset pressure is greater than or equal to 15Mpa and less than or equal to 30Mpa. That is, in the process of continuously introducing carbon dioxide into the first space through the carbon dioxide storage tank 6, when the temperature is between 40°C and 60°C and the pressure is between 15Mpa and 30Mpa, the first space is further pressurized by the compression pump 8, so that the preparation efficiency of supercritical carbon dioxide can be improved.

[0047] In the above technical solution, before dissolving the polyester fiber to be dyed in the supercritical carbon dioxide of the hydrophobic agent for waterless dyeing, supercritical carbon dioxide is first continuously introduced into the surface of the polyester fiber to remove the oil in the polyester fiber through the supercritical carbon dioxide, which can improve the dyeing effect in the later stage and improve the binding force between the hydrophobic agent and the surface of the polyester fiber. On the other hand, deoiling by supercritical carbon dioxide is green and environmentally friendly compared to traditional deoiling methods and has high deoiling efficiency. In addition, the deoiling time is controlled to be greater than or equal to 5 minutes and less than or equal to 25 minutes, which can ensure that the polyester fiber can be fully deoiled and avoid too long time and reduced efficiency.

[0048] In the above technical solution, before the step of dissolving the polyester fiber to be dyed in the supercritical carbon dioxide of the hydrophobic agent for waterless dyeing, carbon dioxide is continuously introduced into the space where the polyester fiber is located to remove the air in the space where the polyester fiber is located. This ensures that the supercritical carbon dioxide is in full contact with the polyester fiber, thereby improving the dyeing efficiency and the bonding force between the hydrophobic agent and the surface of the polyester fiber.

[0049] In the above technical scheme, after waterless dyeing, the hydrophobic agent that has not been used to dye the polyester fiber is separated from the supercritical carbon dioxide, and the supercritical carbon dioxide after the hydrophobic agent is separated is recovered, so that the carbon dioxide can be recycled and the energy utilization rate can be improved.

[0050] like Figure 2 and Figure 5 As shown, another embodiment of the present invention provides a method for preparing polyester fiber, comprising the following steps:

[0051] S202: loading;

[0052] Specifically, a hydrophobic agent is placed in a dye kettle 1, polyester fibers are wound into cheese yarns of a specified density, and after oil extraction, they are loaded into a dye kettle 2, and the dye kettle 2 is a high-pressure dyeing kettle with a sealed kettle body.

[0053] S204: preparing CO2 into supercritical CO2;

[0054] Specifically, the temperature and pressure values ​​of the dyeing kettle 2 are set, the carbon dioxide storage tank 6 is opened to supply gas to the dye kettle 1 and the dyeing kettle 2, and the heating device 4 is turned on to heat the CO2. When the temperature and pressure reach the set values, the CO2 in the carbon dioxide storage tank 6 is filled into the entire system through the compression pump 8. When the pressure reaches the second preset pressure, the pressurization is turned off. After being pressurized by the compression pump 8, the CO2 is heated to a supercritical state under the action of the heating device 4.

[0055] S206: heat preservation and hydrophobic modification cycle;

[0056] Specifically, the circulation system including the dyeing kettle 2 and the circulation pump 7 is turned on, and the supercritical carbon dioxide is subjected to heat-insulating and hydrophobic modification circulation treatment in the circulation system under the action of the airflow.

[0057] S208: pressure reduction, separation and recovery;

[0058] Specifically, the compression pump 8, the circulation pump 7 and the heating device 4 are turned off, and the valve 9 is opened to release the pressure, so that the fluid passes through the separation and recovery device 3, is cooled by the condenser 5, and then the pressure is released to discharge the carbon dioxide and the hydrophobic agent.

[0059] The specific recycling process is as follows: Figure 6 As shown, first, the ethylene glycol in the refrigerant tank 12 is cooled by the refrigeration unit 11, and the cooled ethylene glycol is used as a coolant. Then, the low-temperature ethylene glycol is transported to the inside of the condenser 5 by the ethylene glycol pump 13. After the supercritical carbon dioxide passes through the separation and recovery device 3, it can exchange heat with the low-temperature ethylene glycol in the condenser 5 and then be cooled into liquid carbon dioxide. The liquid carbon dioxide flows back to the carbon dioxide storage tank 6 to complete the recovery.

[0060] Furthermore, the main heating principle of the heating device 4 is to heat the thermal oil through the thermal oil heater 14, and the thermal oil and carbon dioxide exchange heat in the heating device 4, thereby achieving the heating of carbon dioxide.

[0061] Furthermore, the carbon dioxide steel tank 10 is an external device used to replenish carbon dioxide for the carbon dioxide steel tank 6 .

[0062] S210: obtaining a hydrophobically modified polyester fiber;

[0063] Specifically, the gaseous CO2 is condensed by the condenser 5 and then returns to the carbon dioxide storage tank 6, where it continues to be depressurized and cooled to normal temperature and pressure, thereby completing the hydrophobic modification of the polyester fiber.

[0064] Further, the hydrophobic agent is a C6 fluorine compound functional finishing agent, that is, a fluorine compound with 6 carbon atoms, or a C6 bromine compound functional finishing agent, that is, a bromine compound with 6 carbon atoms;

[0065] Furthermore, the step of extracting the oil agent in step S202 is as follows: turning on the circulation pump 7 to extract the fiber oil agent through supercritical carbon dioxide, releasing the pressure to discharge the supercritical carbon dioxide containing the oil agent after the treatment is completed, the supercritical carbon dioxide containing the oil agent flows into the separation recovery device 3 and becomes gaseous, the oil agent precipitates from the CO2 and sinks in the separation recovery device 3, and the CO2 gas separated from the oil agent flows into the condenser 5 and becomes liquid CO2 and flows back to the carbon dioxide storage tank 6;

[0066] Furthermore, the time of oil extraction was 10 min;

[0067] Furthermore, after the kettle is sealed in step S202, CO2 is introduced to exhaust the air in the kettle;

[0068] Further, in step S204, the set values ​​of temperature and pressure are: temperature is 40°C to 60°C, and pressure is 8Mpa to 15Mpa;

[0069] Furthermore, in step S206, the conditions for the hydrophobic modification cycle treatment are: temperature 70°C, pressure 15 MPa to 30 MPa.

[0070] Furthermore, in step S208, the pressure is reduced and the temperature is lowered. When the fluid pressure reaches below 7.2 MPa and the temperature reaches below 20° C., the supercritical carbon dioxide entrained with the hydrophobic agent can be discharged;

[0071] Furthermore, the supercritical carbon dioxide entrained with the hydrophobic agent is subjected to a separation and recovery step after being released from the pressure, and the hydrophobic agent is separated and the gaseous carbon dioxide is recovered through the separation and recovery step;

[0072] Furthermore, the separation and recovery device 3 is a separation kettle.

[0073] The technical solution of the present invention has the following advantages over the prior art solutions: the processing methods for making the product hydrophobic generally include padding, spraying, foaming, and garment washing, and CO2 is used instead of water as a medium to achieve hydrophobic modification of polyester fibers. Due to the introduction of fluorine elements, polyester fibers are endowed with hydrophobic and oleophobic characteristics, and the modification process does not require the addition of any additives, which greatly shortens the modification steps, saves costs, and reduces the environmental pollution caused by chemical surface super-hydrophobic modification, which has positive significance for the development of polyester fiber products.

[0074] like Figure 3 As shown, another embodiment of the present invention provides a method for preparing polyester fiber, comprising the following steps:

[0075] S302: polyester fiber degreasing;

[0076] S304: Hydrophobic modification of deoiled polyester fibers.

[0077] Further, if Figure 4 and Figure 5 As shown, S302: the step of degreasing polyester fibers specifically includes:

[0078] S3022: Loading polyester fiber into dyeing kettle;

[0079] Specifically, the polyester fiber is wound into a cheese yarn of a specified density and then loaded into a dyeing kettle 2, the dyeing kettle 2 is sealed, CO2 is introduced, and the air in the kettle is exhausted;

[0080] S3024: preparing CO2 into supercritical CO2;

[0081] Specifically, turn on the heating device 4 connected to the dyeing kettle 2, open the carbon dioxide storage tank 6, open the valve 9, fill CO2 into the entire system through the compression pump 8, turn off the pressurization when the pressure reaches the preset value, and after being pressurized by the compression pump 8, the CO2 is heated to a supercritical state under the action of the heating device 4.

[0082] S3026: Oil extraction;

[0083] Specifically, the circulation pump 7 is turned on to extract the oil in the polyester fiber, and the oil in the polyester fiber is extracted, and the extraction time is 10 minutes to 20 minutes.

[0084] S3028: Separation and recovery;

[0085] Specifically, after the oil extraction is completed, the supercritical CO2 is cooled and depressurized in advance, and the supercritical carbon dioxide fluid containing the oil agent flows into the separation and recovery device 3 through the valve 9 and becomes gaseous. The oil agent precipitates from the CO2 and sinks in the separation and recovery device 3. The CO2 gas separated from the oil agent flows into the condenser 5 and becomes liquid CO2 and flows back to the carbon dioxide storage tank 6, thereby completing the deoiling of the polyester fiber fabric.

[0086] Further, S304: the step of hydrophobic modification of the deoiled polyester fiber specifically comprises:

[0087] S3042: loading;

[0088] Specifically, a C6 fluorine compound functional finishing agent is placed in a dye kettle 1, polyester fibers are wound into cheese yarns of a specified density and then loaded into a dye kettle 2, and the kettle body is sealed.

[0089] S3044: preparing CO2 into supercritical CO2;

[0090] Specifically, the temperature and pressure values ​​of the dyeing kettle 2 are set, the carbon dioxide storage tank 6 is opened to supply gas to the dye kettle 1 and the dyeing kettle 2, and the heating device 4 is turned on to heat the CO2. When the temperature and pressure reach the set values, the CO2 is filled into the entire system through the compression pump 8. When the pressure reaches the preset value, the pressurization is turned off. After being pressurized by the compression pump 8, the CO2 is heated to a supercritical state under the action of the heating device 4.

[0091] S3046: Insulation, hydrophobic modification cycle;

[0092] Specifically, the circulation system including the dyeing kettle 2 and the circulation pump 7 is turned on, and the supercritical carbon dioxide is subjected to heat preservation and hydrophobic modification circulation treatment in the circulation system under the action of airflow, with a temperature of 70° C., a pressure of 15 MPa, and a time of 4 hours.

[0093] S3048: Pressure reduction, separation, and recovery;

[0094] Specifically, the compression pump 8, the circulation pump 7 and the heating device 4 are turned off, and the valve 9 is opened to release the pressure, so that the fluid passes through the separation and recovery device 3. When the fluid pressure reaches below 7.2 MPa and the temperature reaches below 20°C, the pressure is released to discharge carbon dioxide and hydrophobic agent, and then a separation and recovery step is performed to separate the hydrophobic agent and recover the gaseous carbon dioxide.

[0095] S30410: obtaining a hydrophobically modified polyester fiber;

[0096] Specifically, the gaseous CO2 is condensed by the condenser 5 and then returns to the carbon dioxide storage tank 6, where it continues to be depressurized and cooled to normal temperature and pressure, thereby completing the hydrophobic modification of the polyester fiber.

[0097] Another embodiment of the present invention provides a waterless dyeing method for polyester fiber fabric for shoes, and the specific process is basically the same as the steps of the previous embodiment, except that the pressure of supercritical carbon dioxide in the circulation system for heat preservation and hydrophobic modification circulation treatment is 30 MPa.

[0098] An embodiment of the second aspect of the present invention provides a hydrophobic polyester fiber. The hydrophobic polyester fiber provided by this embodiment is prepared by the method for preparing the polyester fiber of any embodiment of the first aspect of the present application.

[0099] An embodiment of the third aspect of the present invention provides a fabric, and the material of the fabric provided by this embodiment includes the hydrophobic polyester fiber of the embodiment of the second aspect of the present application.

[0100] In the embodiments according to the present invention, the terms "first", "second", and "third" are only used for description and cannot be understood as indicating or implying relative importance; the term "plurality" refers to two or more, unless otherwise clearly defined. The terms "installed", "connected", "connected", "fixed" and the like should be understood in a broad sense. For example, "connected" can be a fixed connection, a detachable connection, or an integral connection; "connected" can be a direct connection or an indirect connection through an intermediate medium. For those of ordinary skill in the art, the specific meanings of the above terms in the embodiments according to the present invention can be understood according to specific circumstances.

[0101] In addition, although each operation is described in a specific order, this should be understood as requiring such operation to be performed in a specific order or in a sequential order, or requiring that all illustrated operations should be performed to obtain desired results. Under certain circumstances, multitasking and parallel processing may be advantageous. Similarly, although some specific implementation details are included in the above discussion, these should not be interpreted as limiting the scope of the present invention. Some features described in the context of a separate embodiment can also be implemented in a single implementation in combination. On the contrary, the various features described in the context of a single implementation can also be implemented in multiple implementations individually or in any suitable sub-combination mode.

[0102] Although the subject matter has been described in the language of specific structural features and / or method logical actions, it should be understood that the subject matter defined in the appended claims is not necessarily limited to the specific features or actions described above. On the contrary, the specific features and actions described above are merely example forms of implementing the claims.

[0103] The above are only preferred embodiments according to the embodiments of the present invention, and are not intended to limit the embodiments of the present invention. For those skilled in the art, various modifications and changes may be made according to the embodiments of the present invention. Any modification, equivalent replacement, improvement, etc. made within the spirit and principle of the embodiments of the present invention shall be included in the protection scope of the embodiments of the present invention.

Claims

1. A method for preparing a hydrophobic polyester fiber, characterized in that: include: Preparing supercritical carbon dioxide, wherein the temperature of the supercritical carbon dioxide is greater than or equal to 31.1° C., and the pressure of the supercritical carbon dioxide is greater than or equal to 7.39 MPa; dissolving a hydrophobic agent in the supercritical carbon dioxide; The polyester fiber to be dyed is dissolved in supercritical carbon dioxide of a hydrophobic agent for waterless dyeing, so that the hydrophobic agent adheres to the surface of the polyester fiber to form the hydrophobic polyester fiber.

2. The method for preparing the hydrophobic polyester fiber according to claim 1, characterized in that: The hydrophobic agent includes a fluoride with 6 carbon atoms; or The hydrophobic agent includes a bromide having 6 carbon atoms.

3. The method for preparing the hydrophobic polyester fiber according to claim 1, characterized in that: In the step of dissolving the polyester fiber to be dyed in the supercritical carbon dioxide of the hydrophobic agent for waterless dyeing, The temperature of the supercritical carbon dioxide of the hydrophobic agent is greater than or equal to 60° C. and less than or equal to 80° C.; The pressure of the supercritical carbon dioxide in the hydrophobic agent is greater than or equal to 15 MPa and less than or equal to 30 MPa; The dyeing time is greater than or equal to 2h and less than or equal to 6h.

4. The method for preparing the hydrophobic polyester fiber according to claim 1, characterized in that: The temperature of the supercritical carbon dioxide is greater than or equal to 60° C. and less than or equal to 80° C., the pressure of the supercritical carbon dioxide is greater than or equal to 15 MPa and less than or equal to 30 MPa, and the step of preparing the supercritical carbon dioxide comprises: The carbon dioxide storage tank is opened to continuously introduce carbon dioxide into the first space, and the heating device is turned on to heat the carbon dioxide in the first space. When the temperature reaches the first preset temperature and the pressure reaches the first preset pressure, the first space is pressurized by the boosting device. When the pressure reaches the second preset pressure, the carbon dioxide storage tank is closed, and the carbon dioxide in the first space is heated to the second preset temperature by the heating device to obtain the supercritical carbon dioxide.

5. The method for preparing the hydrophobic polyester fiber according to claim 4, characterized in that: The first preset temperature is greater than or equal to 40° C. and less than or equal to 60° C.; The first preset pressure is greater than or equal to 8 MPa and less than or equal to 15 MPa; The second preset temperature is greater than or equal to 60° C. and less than or equal to 80° C.; The second preset pressure is greater than or equal to 15 MPa and less than or equal to 30 MPa.

6. The method for preparing the hydrophobic polyester fiber according to claim 1, characterized in that: Before the step of dissolving the polyester fiber to be dyed in the supercritical carbon dioxide of the hydrophobic agent for anhydrous dyeing, the method further comprises: Supercritical carbon dioxide is continuously introduced into the surface of the polyester fiber to remove the oil in the polyester fiber through the supercritical carbon dioxide, wherein the duration of continuous introduction of the supercritical carbon dioxide is greater than or equal to 5 minutes and less than or equal to 25 minutes.

7. The method for preparing the hydrophobic polyester fiber according to claim 1, characterized in that: Before the step of dissolving the polyester fiber to be dyed in the supercritical carbon dioxide of the hydrophobic agent for anhydrous dyeing, the method further comprises: Carbon dioxide is continuously introduced into the space where the polyester fibers are located to remove the air in the space where the polyester fibers are located.

8. The method for preparing the hydrophobic polyester fiber according to any one of claims 1 to 7, characterized in that: Also includes: separating the hydrophobic agent that has not been used to anhydrous dye the polyester fiber from the supercritical carbon dioxide; The supercritical carbon dioxide is recovered after the hydrophobic agent is separated.

9. A hydrophobic polyester fiber, characterized in that: The hydrophobic polyester fiber is prepared by the method for preparing the hydrophobic polyester fiber according to any one of claims 1 to 8.

10. A fabric, characterized in that: The material of the fabric includes the hydrophobic polyester fiber as claimed in claim 9.