Recyclable TPU non-woven fabric high-low temperature film and preparation method thereof

By using the structure of renewable nylon fabric layer, bio-based hot melt adhesive layer and TPU surface film layer in TPU non-woven fabric, combined with modified polymer, the problem of low recycling efficiency and poor quality of TPU material is solved, and high efficiency is achieved , the preparation of environmentally friendly TPU non-woven high and low temperature membranes meets the needs of practical applications.

CN118727463APending Publication Date: 2024-10-01DONGGUAN ZHONGDING PLASTIC PRODUCTION CO LTD
View PDF 0 Cites 0 Cited by

Patent Information

Application Number
CN202410920387.6
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Filing Date
2024-07-10
Publication Date
2024-10-01

AI Technical Summary

Technical Problem

Existing recycling technologies for TPU materials and non-woven fabrics are inefficient and may cause environmental pollution, and the recycled materials are of poor quality and cannot meet actual application needs.

Method used

It adopts the structure of renewable nylon fabric layer, bio-based hot melt adhesive layer and TPU surface film layer. Through the mixed processing of bio-fiber and recycled polyester filament, combined with modified polyurethane emulsion and modified polyester polyol, it forms high adhesion. , high-strength TPU non-woven high and low temperature membrane, which has the characteristics of environmental protection, heat resistance, water resistance and so on.

Benefits of technology

It improves the quality and performance of recycled materials, achieves the goals of environmental protection and sustainable development, meets practical application needs, and reduces the risk of environmental pollution.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure BDA0004936512600000141
    Figure BDA0004936512600000141
Patent Text Reader

Abstract

The invention relates to a recyclable TPU non-woven fabric high and low temperature film and a preparation method thereof, the recyclable TPU non-woven fabric high and low temperature film comprises a regenerated nylon fabric layer, a hot melt adhesive layer and a TPU surface film layer which are arranged in sequence, the non-woven fabric layer is formed by mixing and processing biological fibers and regenerated polyester filament DTY, the hot melt adhesive layer adopts bio-based hot melt adhesive, the TPU surface film layer is formed by coating TPU paint, and the TPU surface film layer is formed by coating TPU paint. The TPU coating is prepared from the following raw materials in parts by weight: 40-60 parts of TUP particles, 10-20 parts of TPSIV particles, 1-3 parts of a moisture absorbent, 1-3 parts of a slipping agent, 1-5 parts of a plasticizer, 1-3 parts of a dispersing agent, 10-15 parts of modified polyurethane emulsion, 5-10 parts of modified polyester polyol, 20-40 parts of a solvent and 0.1-1.0 part of a flatting agent. The recyclable TPU non-woven fabric high-low temperature film is environmentally friendly, the material source is renewable and meets the sustainable development requirement, and the material source adopted by the regenerated nylon fabric layer is renewable and meets the sustainable development requirement.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The invention relates to the technical field of TPU films, and in particular to a recyclable and regenerable TPU non-woven fabric high-low temperature film and a preparation method thereof. Background Art

[0002] Polyurethane (TPU) is a widely used high-performance material. Due to its excellent wear resistance, tear resistance and elasticity, it is widely used in various products such as clothing, shoes, wall coverings, sofas, car seats, etc. However, traditional TPU materials are difficult to recycle and reuse after use, which puts pressure on the environment. In the field of non-woven fabric preparation technology, non-woven fabric is a fabric that does not require spinning and weaving. It has a simple production process, low cost, and good air permeability and hygroscopicity. Therefore, it is widely used in various fields. However, traditional non-woven fabrics are also difficult to recycle and reuse after use, which puts pressure on the environment. In the field of environmental protection material recycling technology, with the improvement of environmental awareness, how to effectively recycle and reuse various materials and reduce environmental pollution is an important research direction at present. Among them, how to effectively recycle and reuse TPU materials and non-woven fabrics is an important research topic. 1) Solutions of the prior art: The existing solutions are mainly to recycle discarded TPU materials and non-woven fabrics through physical or chemical methods, and then convert them into new TPU materials and non-woven fabrics through certain process. Although this method can achieve the recycling and reuse of TPU materials and non-woven fabrics, its recycling efficiency is low, and the recycling process may cause secondary pollution to the environment. 2) Problems with the prior art: The problems existing in the prior art in this field are mainly the following: First, the existing recycling methods have low recycling efficiency, and a large amount of TPU materials and non-woven fabrics are discarded after use and cannot be effectively recycled and reused, which puts pressure on the environment. Secondly, the existing recycling methods may cause secondary pollution to the environment during the recycling process. For example, harmful chemicals may be produced during the chemical recycling process. Finally, the regenerated TPU materials and non-woven fabrics obtained by the existing recycling methods are of poor quality and unstable performance, and cannot meet the needs of practical applications. Summary of the invention

[0003] In order to overcome the shortcomings and deficiencies in the prior art, the purpose of the present invention is to provide a recyclable and regenerated TPU non-woven high and low temperature membrane. The TPU non-woven high and low temperature membrane is environmentally friendly and has a renewable material source, which meets the requirements of sustainable development. The material source used in the recycled nylon fabric layer is renewable and meets the requirements of sustainable development. At the same time, it has low density, softness, high strength, and good resilience. During the curing process, the bio-based hot melt adhesive layer absorbs moisture in the air and reacts with the moisture attached to the surface of the recycled nylon fabric layer to form a partially cross-linked network structure, generating a high molecular polymer with high adhesion, which significantly improves the adhesion, heat resistance, low temperature resistance, etc., so that the prepared fabric has the characteristics of high peel strength, heat resistance, and water washability.

[0004] Another object of the present invention is to provide a method for preparing a recyclable TPU non-woven high and low temperature film. The recycled TPU material and non-woven fabric of the present invention are prepared by a special method, and their quality and performance are guaranteed, which can meet the needs of practical applications and solve the problems of poor quality and unstable performance of recycled materials in the prior art.

[0005] The purpose of the present invention is achieved through the following technical scheme: a recyclable and regenerated TPU non-woven high and low temperature film, comprising a recycled nylon fabric layer, a hot melt adhesive layer and a TPU surface film layer arranged in sequence, the non-woven fabric layer is made of a mixture of bio-fiber and recycled polyester filament DTY, the hot melt adhesive layer adopts bio-based hot melt adhesive, and the TPU surface film layer is coated with TPU coating, and the TPU coating comprises the following raw materials in parts by weight: 40-60 parts of TUP particles, 10-20 parts of TPSIV particles, 1-3 parts of hygroscopic agent, 1-3 parts of lubricant, 1-5 parts of plasticizer, 1-3 parts of dispersant, 10-15 parts of modified polyurethane emulsion, 5-10 parts of modified polyester polyol, 20-40 parts of solvent, and 0.1-1.0 parts of leveling agent.

[0006] The PU non-woven high and low temperature film in the present invention is environmentally friendly, the material source is renewable, and it meets the requirements of sustainable development. The material source of the recycled nylon fabric layer is renewable and meets the requirements of sustainable development. At the same time, it has the properties of low density, softness, high strength, and good resilience. During the aging process, the bio-based hot melt adhesive of the hot melt adhesive layer absorbs moisture in the air and reacts with the moisture attached to the surface of the recycled nylon fabric layer to form a partially cross-linked network structure, generating a high molecular polymer with high adhesion, which significantly improves the adhesion, heat resistance, and low temperature resistance, so that the prepared fabric has the characteristics of high peeling strength, heat resistance, and water resistance. The TPU coating used in the TPU surface film layer has good aging resistance, air tightness, antibacterial property, water resistance, impact resistance, and tear resistance, and has high strength, good reliability, long service life, etc., and is not only environmentally friendly, degradable, renewable, and recyclable, but also has better wear resistance than rubber. Among them, TUP particles are mainly divided into polyester type and polyether type, with a wide hardness range, wear resistance, oil resistance, transparency, good elasticity, and can increase the various properties of TPU coating film; by adding TPSIV particles to polyester TUP particles, TPSIV has good hydrolysis resistance and anti-fouling properties, and feels smooth, which makes up for the performance defects of polyester TPU material surface astringency and poor hydrolysis resistance. TPU is an environmentally friendly material with good recyclability. Therefore, the composite TPU non-woven high and low temperature film has a comfortable feel, good hydrolysis resistance and anti-fouling properties, and has green and environmentally friendly functions; modified polyester polyol is the main component of TPU coating, which provides elasticity and plasticity. Modified polyester polyol introduces a large number of hydrophilic groups through hyperbranching technology, which improves the hydrophilicity and stability of the film, and synergizes with other additives to make TPU coating film have better performance.

[0007] Preferably, the TPU particles are one or both of polyether TPU and polyester TPU.

[0008] Preferably, the lubricant is one or both of polyolefin wax and erucamide.

[0009] The above-mentioned specific lubricant used in the present invention can improve the smoothness, surface color, anti-stickiness, anti-fouling, adhesion and chemical resistance of the coating film, is suitable for higher processing temperatures, and has a more lasting lubricating effect, thereby comprehensively improving the film-forming performance of the TPU coating.

[0010] Preferably, the plasticizer is a mixture of dipropylene glycol dibenzoate, polyvinyl pyrrolidone and polyvinyl alcohol in a weight ratio of 0.8-1.2:0.6-1.0:0.4-0.8.

[0011] The plasticizer in the present invention is composed of the above-mentioned raw materials in a specific ratio, so that the TPU coating can form a protective film on the surface of the hot melt adhesive layer to effectively prevent oil pollution from penetrating.

[0012] Preferably, the dispersant is at least one of sodium dodecyl sulfate, methyl amyl alcohol, and guar gum; and the solvent is at least one of isopropanol, methyl ethyl ketone, and N,N-dimethylformamide.

[0013] Preferably, the modified polyester polyol comprises the following raw materials: 10-20 parts of 3-(2-hydroxypropoxy)butanol, 10-15 parts of adipic acid, and 0.5-1.5 parts of antimony trioxide (catalyst).

[0014] Preferably, the modified polyester polyol is prepared by the following method: according to parts by weight, 3-(2-hydroxypropoxy)butanol and adipic acid are placed in a reactor, nitrogen is introduced to expel the air, the mixture is heated to 100-120°C, and stirred for 1-2h; antimony trioxide is then added, and the mixture is stirred at 135-145°C for 1-2h, during which the reaction system is vacuumed every 20-30min to remove small molecular by-products, and the reaction is stopped after there is no significant change in the weight of the reaction system to obtain the modified polyester polyol.

[0015] The modified polyester polyol in the present invention is prepared by adopting the above raw materials and methods. The modified polyester polyol is produced by reacting 3-(2-hydroxypropoxy) butanol with adipic acid, which can improve the low temperature resistance of the TPU coating, that is, improve the low temperature folding resistance, and the modified polyester polyol has good compatibility with other raw materials of the polyurethane stock solution system. By adopting the above technical scheme, in the preparation method of the modified polyester polyol, the citric acid-(2-hydroxypropoxy) butanol and adipic acid used are renewable resources. The modified polyester polyol has the following effects and synergistic effects in the preparation of high-performance polyether TPU film: hydrophilicity and stability: the modified polyester polyol has a large number of hydrophilic groups at the end, which can improve the hydrophilicity and stability of the TPU film, so that it has good air permeability and water washability. Environmentally friendly: the modified polyester polyol prepared from the renewable resources of -(2-hydroxypropoxy) butanol and adipic acid has environmentally friendly characteristics and meets the requirements of sustainable development. High degree of branching: Hyperbranching technology makes the modified polyester polyol have a high degree of branching, which can increase the elasticity and plasticity of the polyether TPU film. Compatibility with other components: The modified polyester polyol has good compatibility with other components. In summary, the modified polyester polyol has multiple functions in the preparation of high-performance TPU film, such as hydrophilicity and stability, environmental friendliness, high degree of branching, and compatibility with other components. The synergistic effect makes the film have better performance.

[0016] Preferably, the modified polyurethane emulsion adopts the water-based polyurethane modified acrylic acid model WX-3200 provided by Foshan Wanxia New Material Technology Co., Ltd.

[0017] Preferably, the leveling agent is a silicone-modified polyether type water-based leveling agent; and the hygroscopic agent is a mixture of chitosan and carbomer.

[0018] Preferably, the TPU coating is prepared by the following steps:

[0019] S1. Mix the dispersant, lubricant and solvent in parts by weight to obtain a mixture A for later use;

[0020] S2, according to weight parts, TUP particles, TPSIV particles, plasticizer, modified polyurethane emulsion and modified polyester polyol are mixed and stirred uniformly to obtain a mixture B for standby use;

[0021] S3. Add mixture B into mixture A, add moisture absorbent and leveling agent at the same time, stir at a speed of 700-900 rpm until uniform, and obtain TPU coating.

[0022] The present invention also provides a method for preparing a recyclable and regenerable TPU non-woven high and low temperature film, comprising the following steps:

[0023] A1. Take the recycled nylon fabric layer, stick the hot melt adhesive on the recycled nylon fabric layer and dry it to form a hot melt adhesive layer for later use;

[0024] A2. Evenly coat the TPU coating on the hot melt adhesive layer, heat it to 90-120°C and dry it for 3-5 hours to obtain a recyclable TPU non-woven high and low temperature film.

[0025] The beneficial effects of the present invention are: the TPU non-woven fabric high and low temperature film of the present invention is environmentally friendly, the material source is renewable, and it meets the requirements of sustainable development. The material source of the recycled nylon fabric layer is renewable and meets the requirements of sustainable development. At the same time, it has low density, softness, high strength, and good resilience. During the curing process, the bio-based hot melt adhesive layer absorbs moisture in the air and reacts with the moisture attached to the surface of the recycled nylon fabric layer to form a partially cross-linked network structure, generating a high molecular polymer with high adhesion, which significantly improves the adhesion, heat resistance, low temperature resistance, etc., so that the prepared fabric has the characteristics of high peel strength, heat resistance, and water washability.

[0026] The preparation method of the recyclable TPU non-woven high and low temperature membrane of the present invention is simple, easy to implement, and is conducive to large-scale production and application. Through a special preparation method, the quality and performance of the membrane are guaranteed, and the needs of practical applications can be met, thus solving the problems of poor quality and unstable performance of recycled materials in the prior art. DETAILED DESCRIPTION

[0027] In order to facilitate the understanding of those skilled in the art, the present invention is further described below in conjunction with embodiments, and the contents mentioned in the implementation modes are not intended to limit the present invention.

[0028] Example 1

[0029] A recyclable and regenerated TPU non-woven high and low temperature membrane, comprising a recycled nylon fabric layer, a hot melt adhesive layer and a TPU surface film layer which are arranged in sequence, wherein the non-woven fabric layer is made by mixing biological fibers and recycled polyester filaments DTY, the hot melt adhesive layer adopts bio-based hot melt adhesive, and the TPU surface film layer is coated with TPU coating, wherein the TPU coating comprises the following raw materials in parts by weight: 40 parts of TUP particles, 10 parts of TPSIV particles, 1 part of moisture absorbent, 1 part of lubricant, 1 part of plasticizer, 1 part of dispersant, 10 parts of modified polyurethane emulsion, 5 parts of modified polyester polyol, 20 parts of solvent, and 0.1 part of leveling agent.

[0030] The TUP particles are polyether TPU.

[0031] The lubricant is polyolefin wax.

[0032] The plasticizer is a mixture of dipropylene glycol dibenzoate, polyvinyl pyrrolidone and polyvinyl alcohol in a weight ratio of 0.8:0.6:0.4.

[0033] The dispersant is sodium dodecyl sulfate; the solvent is methyl ethyl ketone.

[0034] The modified polyester polyol comprises the following raw materials: 10 parts of 3-(2-hydroxypropoxy)butanol, 10 parts of adipic acid, and 0.5 parts of antimony trioxide.

[0035] The modified polyester polyol is prepared by the following method: according to parts by weight, 3-(2-hydroxypropoxy)butanol and adipic acid are put into a reactor, nitrogen is introduced to expel air, the reaction mixture is heated to 100° C., and stirred for 2 hours; antimony trioxide is then added, and the mixture is stirred at 135° C. for 2 hours, during which the reaction system is vacuumed once every 20 minutes to remove small molecular by-products, and the reaction is stopped after there is no obvious change in the weight of the reaction system to obtain the modified polyester polyol.

[0036] The modified polyurethane emulsion adopts the model of water-based polyurethane modified acrylic WX-3200 provided by Foshan Wanxia New Material Technology Co., Ltd.

[0037] The leveling agent is a silicone-modified polyether type water-based leveling agent, and the silicone-modified polyether type water-based leveling agent adopts German BYK-345 polyether-modified silicone leveling agent; the hygroscopic agent is a mixture of chitosan and carbomer in a weight ratio of 1:1.

[0038] The TPU coating is prepared by the following steps:

[0039] S1. Mix the dispersant, lubricant and solvent in parts by weight to obtain a mixture A for later use;

[0040] S2, according to weight parts, TUP particles, TPSIV particles, plasticizer, modified polyurethane emulsion and modified polyester polyol are mixed and stirred uniformly to obtain a mixture B for standby use;

[0041] S3. Add mixture B into mixture A, and add a moisture absorbent and a leveling agent at the same time, and stir at a speed of 700 rpm until the mixture is uniform to obtain a TPU coating.

[0042] A recyclable TPU nonwoven high and low temperature membrane is prepared by the following steps:

[0043] A1. Take the recycled nylon fabric layer, stick the hot melt adhesive on the recycled nylon fabric layer and dry it to form a hot melt adhesive layer for later use;

[0044] A2. Evenly coat the TPU coating on the hot melt adhesive layer, heat it to 90°C and dry it for 5 hours to obtain a recyclable TPU non-woven high and low temperature film.

[0045] Example 2

[0046] A recyclable and regenerated TPU non-woven high and low temperature membrane, comprising a recycled nylon fabric layer, a hot melt adhesive layer and a TPU surface film layer which are arranged in sequence, wherein the hot melt adhesive layer adopts a bio-based hot melt adhesive, the non-woven fabric layer is processed by mixing bio-fiber and recycled polyester filament DTY, and the TPU surface film layer is coated with TPU coating, and the TPU coating comprises the following raw materials in parts by weight: 45 parts of TUP particles, 13 parts of TPSIV particles, 1.5 parts of moisture absorbent, 1.5 parts of lubricant, 2 parts of plasticizer, 1.5 parts of dispersant, 11 parts of modified polyurethane emulsion, 6 parts of modified polyester polyol, 25 parts of solvent, and 0.3 parts of leveling agent.

[0047] The TUP particles are polyester TPU.

[0048] The lubricant is erucamide.

[0049] The plasticizer is a mixture of dipropylene glycol dibenzoate, polyvinyl pyrrolidone and polyvinyl alcohol in a weight ratio of 0.9:0.7:0.5.

[0050] The dispersant is sodium dodecyl sulfate; the solvent is methyl ethyl ketone.

[0051] The modified polyester polyol comprises the following raw materials: 13 parts of 3-(2-hydroxypropoxy)butanol, 11 parts of adipic acid, and 0.8 parts of antimony trioxide.

[0052] The modified polyester polyol is prepared by the following method: according to parts by weight, 3-(2-hydroxypropoxy)butanol and adipic acid are placed in a reactor, nitrogen is introduced to expel air, the reaction mixture is heated to 105° C., and stirred for 1.3 hours; antimony trioxide is then added, and the mixture is stirred at 138° C. for 1.3 hours, during which the reaction system is vacuumed once every 20-30 minutes to remove small molecular by-products, and the reaction is stopped after there is no significant change in the weight of the reaction system to obtain the modified polyester polyol.

[0053] The modified polyurethane emulsion adopts the model of water-based polyurethane modified acrylic WX-3200 provided by Foshan Wanxia New Material Technology Co., Ltd.

[0054] The leveling agent is a silicone-modified polyether type water-based leveling agent, and the silicone-modified polyether type water-based leveling agent adopts German BYK-345 polyether-modified silicone leveling agent; the hygroscopic agent is a mixture of chitosan and carbomer in a weight ratio of 1:1.

[0055] The TPU coating is prepared by the following steps:

[0056] S1. Mix the dispersant, lubricant and solvent in parts by weight to obtain a mixture A for later use;

[0057] S2, according to weight parts, TUP particles, TPSIV particles, plasticizer, modified polyurethane emulsion and modified polyester polyol are mixed and stirred uniformly to obtain a mixture B for standby use;

[0058] S3. Add mixture B into mixture A, add moisture absorbent and leveling agent at the same time, stir at 750 rpm until the mixture is uniform, and obtain TPU coating.

[0059] A recyclable TPU nonwoven high and low temperature membrane is prepared by the following steps:

[0060] A1. Take the recycled nylon fabric layer, stick the hot melt adhesive on the recycled nylon fabric layer and dry it to form a hot melt adhesive layer for later use;

[0061] A2. Evenly coat the TPU coating on the hot melt adhesive layer, heat it to 100°C and dry it for 3.5 hours to obtain a recyclable TPU non-woven high and low temperature film.

[0062] Example 3

[0063] A recyclable and regenerated TPU non-woven high and low temperature membrane, comprising a recycled nylon fabric layer, a hot melt adhesive layer and a TPU surface film layer which are arranged in sequence, wherein the hot melt adhesive layer adopts a bio-based hot melt adhesive, the non-woven fabric layer is processed by mixing bio-fiber and recycled polyester filament DTY, and the TPU surface film layer is coated with TPU coating, and the TPU coating comprises the following raw materials in parts by weight: 50 parts of TUP particles, 15 parts of TPSIV particles, 2 parts of moisture absorbent, 2 parts of lubricant, 3 parts of plasticizer, 2 parts of dispersant, 13 parts of modified polyurethane emulsion, 8 parts of modified polyester polyol, 30 parts of solvent, and 0.5 parts of leveling agent.

[0064] The TUP particles are polyether TPU.

[0065] The lubricant is polyolefin wax.

[0066] The plasticizer is a mixture of dipropylene glycol dibenzoate, polyvinyl pyrrolidone and polyvinyl alcohol in a weight ratio of 1.0:0.8:0.6.

[0067] The dispersant is a mixture of sodium lauryl sulfate, methyl amyl alcohol and guar gum in a weight ratio of 0.8:0.7:0.4; and the solvent is isopropanol.

[0068] The modified polyester polyol comprises the following raw materials: 15 parts of 3-(2-hydroxypropoxy)butanol, 13 parts of adipic acid, and 1.0 part of antimony trioxide.

[0069] The modified polyester polyol is prepared by the following method: according to parts by weight, 3-(2-hydroxypropoxy)butanol and adipic acid are put into a reactor, nitrogen is introduced to exhaust the air, the reaction mixture is heated to 110° C., and stirred for 1.5 hours; antimony trioxide is then added, and the mixture is stirred at 140° C. for 1.5 hours, during which the reaction system is vacuumed once every 25 minutes to remove small molecular by-products, and the reaction is stopped after there is no obvious change in the weight of the reaction system to obtain the modified polyester polyol.

[0070] The modified polyurethane emulsion adopts the model of water-based polyurethane modified acrylic WX-3200 provided by Foshan Wanxia New Material Technology Co., Ltd.

[0071] The leveling agent is a silicone-modified polyether type water-based leveling agent, and the silicone-modified polyether type water-based leveling agent adopts German BYK-345 polyether-modified silicone leveling agent; the hygroscopic agent is a mixture of chitosan and carbomer in a weight ratio of 1:1.

[0072] The TPU coating is prepared by the following steps:

[0073] S1. Mix the dispersant, lubricant and solvent in parts by weight to obtain a mixture A for later use;

[0074] S2, according to weight parts, TUP particles, TPSIV particles, plasticizer, modified polyurethane emulsion and modified polyester polyol are mixed and stirred uniformly to obtain a mixture B for standby use;

[0075] S3. Add mixture B into mixture A, and add moisture absorbent and leveling agent at the same time, and stir at a speed of 800 rpm until the mixture is uniform to obtain TPU coating.

[0076] A recyclable TPU nonwoven high and low temperature membrane is prepared by the following steps:

[0077] A1. Take the recycled nylon fabric layer, stick the hot melt adhesive on the recycled nylon fabric layer and dry it to form a hot melt adhesive layer for later use;

[0078] A2. Evenly coat the TPU coating on the hot melt adhesive layer, heat it to 100°C and dry it for 4 hours to obtain a recyclable TPU non-woven high and low temperature film.

[0079] Example 4

[0080] A recyclable and regenerated TPU non-woven high and low temperature membrane comprises a recycled nylon fabric layer, a hot melt adhesive layer and a TPU surface film layer which are arranged in sequence, wherein the hot melt adhesive layer adopts a bio-based hot melt adhesive, the non-woven fabric layer is processed by mixing biofiber and recycled polyester filament DTY, and the TPU surface film layer is coated with a TPU coating, wherein the TPU coating comprises the following raw materials in parts by weight: 55 parts of TUP particles, 18 parts of TPSIV particles, 2.5 parts of a hygroscopic agent, 2.5 parts of a lubricant, 4 parts of a plasticizer, 2.5 parts of a dispersant, 14 parts of a modified polyurethane emulsion, 8 parts of a modified polyester polyol, 35 parts of a solvent, and 0.1-1.0 parts of a leveling agent.

[0081] The TUP particles are polyether TPU.

[0082] The lubricant is polyolefin wax.

[0083] The plasticizer is a mixture of dipropylene glycol dibenzoate, polyvinyl pyrrolidone and polyvinyl alcohol in a weight ratio of 1.1:0.9:0.7.

[0084] The dispersant is N,N-dimethylformamide.

[0085] The modified polyester polyol comprises the following raw materials: 18 parts of 3-(2-hydroxypropoxy)butanol, 14 parts of adipic acid, and 1.3 parts of antimony trioxide.

[0086] The modified polyester polyol is prepared by the following method: according to parts by weight, 3-(2-hydroxypropoxy)butanol and adipic acid are put into a reactor, nitrogen is introduced to expel air, the reaction mixture is heated to 115° C., and stirred for 1.8 hours; antimony trioxide is then added, and the mixture is stirred at 140° C. for 1.8 hours, during which the reaction system is vacuumed once every 28 minutes to remove small molecular by-products, and the reaction is stopped after there is no obvious change in the weight of the reaction system to obtain the modified polyester polyol.

[0087] The modified polyurethane emulsion adopts the model of water-based polyurethane modified acrylic WX-3200 provided by Foshan Wanxia New Material Technology Co., Ltd.

[0088] The leveling agent is a silicone-modified polyether type water-based leveling agent, and the silicone-modified polyether type water-based leveling agent adopts German BYK-345 polyether-modified silicone leveling agent; the hygroscopic agent is a mixture of chitosan and carbomer.

[0089] The TPU coating is prepared by the following steps:

[0090] S1. Mix the dispersant, lubricant and solvent in parts by weight to obtain a mixture A for later use;

[0091] S2, according to weight parts, TUP particles, TPSIV particles, plasticizer, modified polyurethane emulsion and modified polyester polyol are mixed and stirred uniformly to obtain a mixture B for standby use;

[0092] S3. Add mixture B into mixture A, add moisture absorbent and leveling agent at the same time, stir at 850 rpm until the mixture is uniform, and obtain TPU coating.

[0093] A recyclable TPU nonwoven high and low temperature membrane is prepared by the following steps:

[0094] A1. Take the recycled nylon fabric layer, stick the hot melt adhesive on the recycled nylon fabric layer and dry it to form a hot melt adhesive layer for later use;

[0095] A2. Evenly coat the TPU coating on the hot melt adhesive layer, heat it to 115°C and dry it for 4.5 hours to obtain a recyclable TPU non-woven high and low temperature film.

[0096] Example 5

[0097] A recyclable and regenerated TPU non-woven high and low temperature membrane, comprising a recycled nylon fabric layer, a hot melt adhesive layer and a TPU surface film layer which are arranged in sequence, wherein the hot melt adhesive layer adopts a bio-based hot melt adhesive, the non-woven fabric layer is processed by mixing bio-fiber and recycled polyester filament DTY, and the TPU surface film layer is coated with TPU coating, and the TPU coating comprises the following raw materials in parts by weight: 60 parts of TUP particles, 20 parts of TPSIV particles, 3 parts of moisture absorbent, 3 parts of lubricant, 5 parts of plasticizer, 3 parts of dispersant, 15 parts of modified polyurethane emulsion, 10 parts of modified polyester polyol, 40 parts of solvent, and 1.0 part of leveling agent.

[0098] The TUP particles are polyether TPU.

[0099] The lubricant is polyolefin wax.

[0100] The plasticizer is a mixture of dipropylene glycol dibenzoate, polyvinyl pyrrolidone and polyvinyl alcohol in a weight ratio of 1.2:1.0:0.8.

[0101] The dispersant is sodium lauryl sulfate.

[0102] The modified polyester polyol comprises the following raw materials: 20 parts of 3-(2-hydroxypropoxy)butanol, 15 parts of adipic acid, and 1.5 parts of antimony trioxide.

[0103] The modified polyester polyol is prepared by the following method: according to parts by weight, 3-(2-hydroxypropoxy)butanol and adipic acid are put into a reactor, nitrogen is introduced to exhaust air, the reaction mixture is heated to 120° C., and stirred for 1 hour; antimony trioxide is then added, and the mixture is stirred at 145° C. for 1 hour, during which the reaction system is vacuumed once every 30 minutes to remove small molecular by-products, and the reaction is stopped after there is no significant change in the weight of the reaction system to obtain the modified polyester polyol.

[0104] The modified polyurethane emulsion adopts the model of water-based polyurethane modified acrylic WX-3200 provided by Foshan Wanxia New Material Technology Co., Ltd.

[0105] The leveling agent is a silicone-modified polyether type water-based leveling agent, and the silicone-modified polyether type water-based leveling agent adopts German BYK-345 polyether-modified silicone leveling agent; the hygroscopic agent is a mixture of chitosan and carbomer.

[0106] The TPU coating is prepared by the following steps:

[0107] S1. Mix the dispersant, lubricant and solvent in parts by weight to obtain a mixture A for later use;

[0108] S2, according to weight parts, TUP particles, TPSIV particles, plasticizer, modified polyurethane emulsion and modified polyester polyol are mixed and stirred uniformly to obtain a mixture B for standby use;

[0109] S3. Add mixture B into mixture A, and add moisture absorbent and leveling agent at the same time, and stir at a speed of 900 rpm until the mixture is uniform to obtain TPU coating.

[0110] A recyclable TPU nonwoven high and low temperature membrane is prepared by the following steps:

[0111] A1. Take the recycled nylon fabric layer, stick the hot melt adhesive on the recycled nylon fabric layer and dry it to form a hot melt adhesive layer for later use;

[0112] A2. Evenly coat the TPU coating on the hot melt adhesive layer, heat it to 120°C and dry it for 3 hours to obtain a recyclable TPU non-woven high and low temperature film.

[0113] Comparative Example 1

[0114] The difference between this comparative example and the above-mentioned Example 3 is that no modified polyurethane emulsion and modified polyester polyol are added to the raw materials of the TPU non-woven high and low temperature membrane of this comparative example. The rest of the contents of this comparative example are the same as those of Example 3 and will not be repeated here.

[0115] Comparative Example 2

[0116] The difference between this comparative example and the above-mentioned Example 3 is that no TPSIV particles and film-forming agent are added to the raw materials of the TPU non-woven high and low temperature membrane of this comparative example. The rest of the contents of this comparative example are the same as those of Example 3 and will not be repeated here.

[0117] The performance of the high and low temperature films of the TPU non-woven fabrics prepared in Example 2 and Comparative Examples 1-2 was tested after film formation, and the results are shown in Table 1:

[0118] Wear resistance: The wear resistance of the waterborne polyurethane in each embodiment and comparative example was tested with reference to GB / T1768-2006 "Testing the Wear Resistance of Paint and Varnish by Rotating Rubber Grinding Wheel Method". The specific operation is as follows: Take the TPU non-woven high and low temperature films in each embodiment 2 and comparative examples 1-2, and evenly coat them on the circular organic glass plate required by the national standard, respectively, with a coating thickness of 100 μm, dry and form a film, and cool at room temperature, one group is placed for one day for wear resistance test, and the other group is placed for 180 days for wear resistance test. When testing the wear resistance, first weigh the organic glass plate with an analytical balance, then put the organic glass plate on the TABER wear tester and rub it for 500 turns, then remove the organic glass plate and weigh it again. Among them, the grinding wheel speed is 72r / min, the surface load weight of the paint film is 1000g, and the average value is taken after three repetitions. The mass difference before and after wear is the wear amount, and the size of the wear amount is used to represent the wear resistance of the waterborne polyurethane. The lower the abrasion loss, the better the wear resistance of the waterborne polyurethane. The smaller the difference between the abrasion loss at 180d and 1d, the better the long-term wear resistance of the waterborne polyurethane.

[0119] Peel strength test: The peel strength of the high and low temperature films of the TPU nonwoven fabrics prepared in Example 2 and Comparative Examples 1-2 was measured according to GB / T3923 standard;

[0120] Water vapor permeability test: Referring to GB / T 12704-1991 standard, a water vapor permeability tester was used to test the water vapor permeability of high-performance polyether TPU membrane. The experimental test parameters were set at a temperature of 38°C, a relative humidity of 2%, and an airflow of 0.5m / s. Each sample was tested three times and the average value was taken.

[0121] Table 1

[0122]

[0123] It can be seen from Example 2 that the wear-resistant TPU high and low temperature film prepared in the present invention has the advantages of good wear resistance, moisture permeability and mechanical properties.

[0124] From the comparison between Example 2 and Comparative Examples 1-2, it can be seen that under the same conditions, the addition of modified polyurethane emulsion, modified polyester multi-element, TPSIV particles and film-forming agent in the formula makes the prepared wear-resistant TPU high and low temperature film have better wear resistance, moisture permeability and mechanical properties, etc., and has broad market prospects and application value.

[0125] The above embodiments are preferred implementation schemes of the present invention. In addition, the present invention may also be implemented in other ways. Any obvious replacement without departing from the concept of the present invention is within the protection scope of the present invention.

Claims

1. A recyclable TPU non-woven high and low temperature film, Features: It comprises a recycled nylon fabric layer, a hot melt adhesive layer and a TPU surface film layer which are arranged in sequence. The non-woven fabric layer is made of a mixture of bio-fiber and recycled polyester filament DTY. The hot melt adhesive layer adopts bio-based hot melt adhesive. The TPU surface film layer is coated with TPU coating. The TPU coating comprises the following raw materials in parts by weight: 40-60 parts of TUP particles, 10-20 parts of TPSIV particles, 1-3 parts of hygroscopic agent, 1-3 parts of lubricant, 1-5 parts of plasticizer, 1-3 parts of dispersant, 10-15 parts of modified polyurethane emulsion, 5-10 parts of modified polyester polyol, 20-40 parts of solvent and 0.1-1.0 parts of leveling agent.

2. A recyclable TPU nonwoven high and low temperature membrane according to claim 1, Features: The TPU particles are one or both of polyether TPU and polyester TPU.

3. A recyclable TPU nonwoven high and low temperature membrane according to claim 1, Features: The lubricant is one or both of polyolefin wax and erucamide.

4. The recyclable TPU nonwoven high and low temperature membrane according to claim 1, Features: The plasticizer is a mixture of dipropylene glycol dibenzoate, polyvinyl pyrrolidone and polyvinyl alcohol in a weight ratio of 0.8-1.2:0.6-1.0:0.4-0.

8.

5. The recyclable TPU nonwoven high and low temperature membrane according to claim 1, Features: The dispersant is at least one of sodium dodecyl sulfate, methyl amyl alcohol and guar gum; the solvent is at least one of isopropanol, methyl ethyl ketone and N,N-dimethylformamide.

6. The recyclable TPU nonwoven high and low temperature membrane according to claim 1, Features: The modified polyester polyol comprises the following raw materials: 10-20 parts of 3-(2-hydroxypropoxy)butanol, 10-15 parts of adipic acid, and 0.5-1.5 parts of antimony trioxide.

7. The recyclable TPU nonwoven high and low temperature membrane according to claim 1, Features: The modified polyester polyol is prepared by the following method: according to parts by weight, 3-(2-hydroxypropoxy)butanol and adipic acid are placed in a reactor, nitrogen is introduced to exhaust air, the reaction mixture is heated to 100-120° C., and stirred for 1-2 hours; antimony trioxide is then added, and the mixture is stirred at 135-145° C. for 1-2 hours, during which the reaction system is vacuumed once every 20-30 minutes to remove small molecular by-products, and the reaction is stopped after there is no significant change in the weight of the reaction system to obtain the modified polyester polyol.

8. The recyclable TPU nonwoven high and low temperature membrane according to claim 1, Features: The leveling agent is a silicone-modified polyether type water-based leveling agent; and the hygroscopic agent is a mixture of chitosan and carbomer.

9. A recyclable TPU nonwoven high and low temperature membrane according to any one of claims 1 to 8, Features: The TPU coating is prepared by the following steps: S1. Mix the dispersant, lubricant and solvent in parts by weight to obtain a mixture A for later use; S2, according to weight parts, TUP particles, TPSIV particles, plasticizer, modified polyurethane emulsion and modified polyester polyol are mixed and stirred uniformly to obtain a mixture B for standby use; S3. Add mixture B into mixture A, add moisture absorbent and leveling agent at the same time, stir at a speed of 700-900 rpm until uniform, and obtain TPU coating.

10. A method for preparing a recyclable TPU nonwoven high and low temperature membrane according to any one of claims 1 to 8, Features: The steps include: A1. Take the recycled nylon fabric layer, stick the hot melt adhesive on the recycled nylon fabric layer and dry it to form a hot melt adhesive layer for later use; A2. Evenly coat the TPU coating on the hot melt adhesive layer, heat it to 90-120°C and dry it for 3-5 hours to obtain a recyclable TPU non-woven high and low temperature film.