Preparation method and application of high-performance high-flexibility formaldehyde-free impregnated bond paper

Through the layer-by-layer self-assembly technology of polyamide epichlorohydrin resin and polyvinyl alcohol/melamine adhesive, the deficiencies in strength, toughness and wear resistance of impregnated adhesive film paper are solved, and high-performance formaldehyde-free flexible adhesive film paper is realized Preparation, no formaldehyde release and high transparency, suitable for artificial board facing materials.

CN118727501AActive Publication Date: 2024-10-01NORTHEAST FORESTRY UNIV

Patent Information

Application Number
CN202410983897.8
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Filing Date
2024-07-22
Publication Date
2024-10-01
Estimated Expiration
2044-07-22

AI Technical Summary

Technical Problem

Existing impregnated adhesive film paper cannot simultaneously have high strength, high toughness, crack resistance, scratch resistance, abrasion resistance and no formaldehyde release, and the low transparency of the adhesive affects the paper texture.

Method used

Using a layer-by-layer self-assembly strategy of polyamide epichlorohydrin resin and polyvinyl alcohol/melamine adhesive, by adjusting the pH value and solid content of the resin, the preparation of formaldehyde-free flexible impregnated adhesive film paper is achieved, using PAE resin and PVA/MA The cross-linking reaction of the adhesive forms a double cross-linked network structure, which improves the bonding strength and wear resistance.

Benefits of technology

Prepare high-performance and highly flexible formaldehyde-free impregnated adhesive film paper, which has no formaldehyde release, high transparency, strong flexibility, excellent wear resistance, scratch resistance and crack resistance. It is suitable for artificial panel facing materials and replaces melamine impregnated adhesive. Membrane paper.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN118727501A_ABST
    Figure CN118727501A_ABST
Patent Text Reader

Abstract

The invention discloses a preparation method and application of high-performance high-flexibility formaldehyde-free impregnated bond paper, and belongs to the technical field of impregnated bond paper. The invention aims to solve the problems that the existing impregnated bond paper cannot have high strength, high toughness, cracking resistance, scratch resistance, wear resistance and no formaldehyde release at the same time, and the paper texture is influenced by low transparency of an adhesive. The preparation method comprises the following steps: 1, adjusting the pH value of the polyamide epichlorohydrin resin; 2, preparing a polyvinyl alcohol / melamine adhesive; and 3, dipping decorative raw paper in the polyamide epichlorohydrin resin after pH adjustment, then drying to obtain primary impregnated paper, dipping the primary impregnated paper in a polyvinyl alcohol / melamine adhesive at room temperature, and then drying to obtain the high-performance high-flexibility formaldehyde-free impregnated bond paper. The material can be used as an artificial board facing material.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The invention belongs to the technical field of impregnated adhesive film paper. Background Art

[0002] Impregnated film paper is widely used as a finishing material for artificial boards due to its aesthetics and decorative and protective effects on the base materials of artificial boards (fiberboard, particleboard, blockboard, etc.). Among all the finishing materials for artificial boards, impregnated film paper is easy to produce, cheap, and highly efficient, and has the largest market share, accounting for about 60%.

[0003] Since urea-formaldehyde resin and melamine-formaldehyde resin have low raw material cost, good quality, and are aqueous solutions of low molecular weight condensation resins, they can penetrate well into the special facing paper, giving the surface of the artificial board added value, and the impregnated paper obtained has good wear resistance and scratch resistance. Therefore, the current market is dominated by urea-formaldehyde resin and melamine-formaldehyde impregnated film paper. However, since melamine impregnated paper releases free formaldehyde during production and use, it brings great harm to human health. In addition, melamine impregnated paper also has the problem of high brittleness and is not suitable for use on non-planar processing surfaces. And after being compounded with artificial boards, it may cause cracks and other problems due to changes in temperature and humidity. With the improvement of living standards and the implementation of relevant national policies, the formaldehyde-free and toughening of impregnated film paper is of great significance.

[0004] At present, the formaldehyde-free problem of decorative paper is mainly solved by using formaldehyde-free impregnated adhesives. The formaldehyde-free adhesives are mainly inorganic adhesives, soy protein adhesives, water-based polyurethane resin adhesives and polyacrylic resin adhesives, etc. However, the main problems of decorative paper impregnated with inorganic adhesives are poor paper flexibility and low transparency of adhesives affecting paper texture. The bonding force of decorative paper impregnated with soy protein adhesive is small and the bonding strength is low. Although water-based polyurethane resin adhesives have strong adhesion, their scratch resistance needs to be improved. Although the modified polyacrylic resin adhesive impregnated decorative paper has improved scratch resistance, it has problems such as low physical and mechanical properties, low wear resistance, and low color clarity. Therefore, it is difficult for existing formaldehyde-free impregnated decorative paper to replace melamine impregnated paper. Summary of the invention

[0005] The present invention aims to solve the problem that the existing impregnated adhesive film paper cannot simultaneously have high strength, high toughness, crack resistance, scratch resistance, wear resistance and no formaldehyde release, and the low transparency of the adhesive affects the paper texture, and further provide a preparation method and application of high-performance and high-flexibility formaldehyde-free impregnated adhesive film paper.

[0006] A method for preparing high-performance and high-flexibility formaldehyde-free impregnated film paper is carried out according to the following steps:

[0007] 1. adjusting the pH value of the polyamide epichlorohydrin resin to 7-11 to obtain the pH-adjusted polyamide epichlorohydrin resin;

[0008] 2. Dissolve polyvinyl alcohol in distilled water, then add melamine, react for 1h to 7h at a temperature of 90°C to 100°C and a stirring speed of 300rpm to 600rpm, and finally cool to room temperature to obtain a polyvinyl alcohol / melamine adhesive;

[0009] 3. At room temperature, the decorative base paper is first impregnated in the polyamide epichlorohydrin resin after pH adjustment, and then dried to obtain a primary impregnated paper. At room temperature, the primary impregnated paper is then impregnated in a polyvinyl alcohol / melamine adhesive, and then dried to obtain a high-performance and high-flexibility formaldehyde-free impregnated film paper.

[0010] The invention discloses an application of high-performance and high-flexibility formaldehyde-free impregnated film paper, which is used as a facing material for artificial boards.

[0011] The beneficial effects of the present invention are:

[0012] (1) The raw material of the impregnating adhesive is water as solvent, which is green and environmentally friendly; (2) The preparation process of the impregnating resin is simple, suitable for large-scale production, and the preparation process is pollution-free; (3) The adhesive does not release formaldehyde and is highly transparent; (4) The formaldehyde-free flexible impregnated film paper is formaldehyde-free and has strong flexibility; (5) After water activation, the formaldehyde-free flexible impregnated film paper has excellent surface bonding strength, wear resistance, scratch resistance, crack resistance and other properties of the veneer artificial board. (6) The formaldehyde-free flexible impregnated film paper adopts a layer-by-layer self-assembly preparation process, which is simple and easy to control. It is expected to replace melamine impregnated film paper.

[0013] Instruction Manual

[0014] Figure 1 The actual picture of the flexibility of the high-performance and high-flexibility formaldehyde-free impregnated film paper, decorative base paper and melamine impregnated film paper prepared in Example 4, a is the decorative base paper, b is the melamine impregnated film paper, and c is the high-performance and high-flexibility formaldehyde-free impregnated film paper;

[0015] Figure 2 is an infrared spectrum; a is the decorative base paper, b is the once-impregnated paper prepared in step 3 of Example 4, and c is the high-performance and high-flexibility formaldehyde-free impregnated film paper prepared in step 3 of Example 4;

[0016] Figure 3 This is a physical picture of the polyvinyl alcohol / melamine adhesive prepared in Example 2;

[0017] Figure 4 These are actual pictures of decorative base paper and impregnated film paper, where a is the decorative base paper and b is the high-performance and high-flexibility formaldehyde-free impregnated film paper prepared in Example 2. DETAILED DESCRIPTION

[0018] Specific implementation method 1: This implementation method is a method for preparing high-performance and high-flexibility formaldehyde-free impregnated film paper, which is carried out according to the following steps:

[0019] 1. adjusting the pH value of the polyamide epichlorohydrin resin to 7-11 to obtain the pH-adjusted polyamide epichlorohydrin resin;

[0020] 2. Dissolve polyvinyl alcohol in distilled water, then add melamine, react for 1h to 7h at a temperature of 90°C to 100°C and a stirring speed of 300rpm to 600rpm, and finally cool to room temperature to obtain a polyvinyl alcohol / melamine adhesive;

[0021] 3. At room temperature, the decorative base paper is first impregnated in the polyamide epichlorohydrin resin after pH adjustment, and then dried to obtain a primary impregnated paper. At room temperature, the primary impregnated paper is then impregnated in a polyvinyl alcohol / melamine adhesive, and then dried to obtain a high-performance and high-flexibility formaldehyde-free impregnated film paper.

[0022] The polyvinyl alcohol / melamine adhesive prepared in step 2 of this specific implementation method is a flexible long-chain adhesive with high flexibility and good transparency.

[0023] In step three of this specific implementation method, polyamide epichlorohydrin resin (PAE resin, wet strength agent) and polyvinyl alcohol / melamine adhesive are used for two-step impregnation to achieve a layer-by-layer self-assembly strategy.

[0024] The excellent performance of the impregnated adhesive film paper of this specific embodiment depends on the influence of pH on the activity of the polyamide epichlorohydrin resin on the one hand, and the influence of the solid content control of the polyvinyl alcohol / melamine adhesive on the other hand. The impregnation of these two resins is used to perform layer-by-layer self-assembly and coordinated control, so that the performance of the impregnated adhesive film paper prepared by it is the best. Finally, after water activation, it is applied to the surface of the artificial board, so that the surface bonding performance, surface wear resistance, surface scratch resistance and surface crack resistance all meet the national standard requirements.

[0025] Principle: Traditionally, PAE / PVA / MA blends are highly active, have high viscosity, and are prone to gelation. In order to make the wet strength agent of PAE resin and the toughening agent of PVA / MA work together, a layer-by-layer self-assembly strategy is innovatively adopted. The impregnated film paper uses the special paper for decoration as the base paper. The first layer is impregnated with PAE resin. The PAE resin undergoes a self-crosslinking reaction in the decorative base paper, and the first layer of network structure is formed through ester bonds. After drying, some active molecules are sealed to obtain impregnated paper, thereby improving the water resistance of the paper. The second layer is loaded on the impregnated paper with PVA / MA adhesive. The PVA / MA adhesive forms the second layer of network structure through hydrogen bond supramolecular crosslinking, and then dried to obtain formaldehyde-free flexible impregnated film paper. Polyamide epichlorohydrin resin and polyvinyl alcohol / melamine adhesive are combined in the paper network structure to form covalent bonds and hydrogen bonds. Through layer-by-layer self-assembly, a chemically and physically combined double crosslinking network is formed on the decorative base paper, so that the impregnated film paper has formaldehyde-free, flexibility and bonding strength. After applying a layer of tap water (water activation) on the surface of the formaldehyde-free flexible impregnated film paper, the active groups (hydrogen bonds) of the formaldehyde-free flexible impregnated film paper are efficiently activated, and the paper is hot-pressed with the artificial board on one side at a certain temperature and pressure for a period of time. During the hot-pressing, hydrogen bonds, chemical bonds and mechanical interlocking forces are generated, forming excellent bonding forces. The formaldehyde-free flexible impregnated film paper facing artificial board can be obtained.

[0026] The beneficial effects of this embodiment are:

[0027] (1) The raw material of the impregnating adhesive is water as solvent, which is green and environmentally friendly; (2) The preparation process of the impregnating resin is simple, suitable for large-scale production, and the preparation process is pollution-free; (3) The adhesive does not release formaldehyde and is highly transparent; (4) The formaldehyde-free flexible impregnated film paper is formaldehyde-free and has strong flexibility; (5) After water activation, the formaldehyde-free flexible impregnated film paper has excellent surface bonding strength, wear resistance, scratch resistance, crack resistance and other properties of the veneer artificial board. (6) The formaldehyde-free flexible impregnated film paper adopts a layer-by-layer self-assembly preparation process, which is simple and easy to control. It is expected to replace melamine impregnated film paper.

[0028] Specific embodiment 2: This embodiment differs from specific embodiment 1 in that in step 1, a NaOH solution with a concentration of 1 mol / L to 3 mol / L is added dropwise to the polyamide epichlorohydrin resin at a rotation speed of 500 rpm to 1000 rpm until the pH value reaches 7 to 11. The rest is the same as specific embodiment 1.

[0029] Specific implementation method 3: This implementation method is different from specific implementation method 1 or 2 in that the solid content of the polyamide epichlorohydrin resin in step 1 is 5% to 20%. Other aspects are the same as specific implementation method 1 or 2.

[0030] Specific embodiment 4: This embodiment differs from specific embodiments 1 to 3 in that: the mass percentage of polyvinyl alcohol in the polyvinyl alcohol / melamine adhesive described in step 2 is 5% to 20%; the mass percentage of melamine in the polyvinyl alcohol / melamine adhesive described in step 2 is 0.1% to 2%. Other aspects are the same as specific embodiments 1 to 3.

[0031] Specific embodiment 5: This embodiment differs from specific embodiments 1 to 4 in that: in step 3, the decorative base paper is first immersed in the polyamide epichlorohydrin resin after pH adjustment for 2 to 10 minutes at room temperature. The rest is the same as specific embodiments 1 to 4.

[0032] Specific implementation method 6: This implementation method is different from specific implementation methods 1 to 5 in that: in step 3, the primary impregnated paper is further impregnated in the polyvinyl alcohol / melamine adhesive at room temperature for 2 to 5 minutes. The rest is the same as specific implementation methods 1 to 5.

[0033] Specific embodiment 7: This embodiment is different from Specific embodiments 1 to 6 in that the drying described in step 3 is carried out at a temperature of 50° C. to 90° C. for 10 to 15 minutes. The rest is the same as Specific embodiments 1 to 6.

[0034] Specific implementation method eight: This implementation method is an application of high-performance and high-flexibility formaldehyde-free impregnated film paper, which is used as a facing material for artificial boards.

[0035] Specific embodiment 9: This embodiment is different from specific embodiment 8 in that when it is used as a facing material for artificial boards, it is specifically carried out according to the following steps:

[0036] The high-performance and high-flexibility formaldehyde-free impregnated film paper is water-activated to obtain activated impregnated film paper, and then the activated impregnated film paper is applied to the surface of the artificial board, and finally hot-pressed to obtain the veneered artificial board. The rest is the same as the eighth embodiment.

[0037] Specific embodiment 10: This embodiment is different from specific embodiment 8 or 9 in that the water activation treatment is specifically carried out according to the following steps: at room temperature, the coating amount is 0.1 g / cm 2 ~1g / cm 2 Apply water to the surface of the high-performance, high-flexibility, formaldehyde-free impregnated adhesive film paper to be pasted, and let it stand for 1 to 3 minutes; the hot pressing is specifically performed at a hot pressing temperature of 170°C to 230°C and a hot pressing pressure of 1MPa to 3MPa for 10s to 3min. The rest is the same as the eighth or ninth embodiment.

[0038] The following examples are used to verify the beneficial effects of the present invention:

[0039] Embodiment 1:

[0040] A method for preparing high-performance and high-flexibility formaldehyde-free impregnated film paper is carried out according to the following steps:

[0041] 1. Under the condition of a rotation speed of 800 rpm, a NaOH solution with a concentration of 2 mol / L was added dropwise to the polyamide epichlorohydrin resin until the pH value reached 7, thereby obtaining a polyamide epichlorohydrin resin after pH adjustment;

[0042] The solid content of the polyamide epichlorohydrin resin is 12.5%;

[0043] 2. Dissolve polyvinyl alcohol in distilled water, then add melamine, react for 6 hours at a temperature of 95°C and a stirring speed of 500 rpm, and finally cool to room temperature to obtain a polyvinyl alcohol / melamine adhesive;

[0044] The mass percentage of polyvinyl alcohol in the polyvinyl alcohol / melamine adhesive is 7%; the mass percentage of melamine in the polyvinyl alcohol / melamine adhesive is 0.75%;

[0045] 3. At room temperature, the decorative base paper is first immersed in the polyamide epichlorohydrin resin after pH adjustment for 5 minutes, and then dried to obtain a primary impregnated paper. At room temperature, the primary impregnated paper is then immersed in the polyvinyl alcohol / melamine adhesive for 2 minutes, and then dried to obtain a high-performance and high-flexibility formaldehyde-free impregnated adhesive film paper;

[0046] The decorative base paper is made of fiber, the manufacturer is Qifeng New Materials Co., Ltd., the model is 9027-83g, the thickness is 0.09mm, and the area is 30×30cm 2 ; The drying is specifically carried out at a temperature of 60°C for 12 minutes; the thickness of the high-performance and high-flexibility formaldehyde-free impregnated film paper is 0.25mm;

[0047] Fourth, subjecting the high-performance and high-flexibility formaldehyde-free impregnated film paper to water activation treatment to obtain activated impregnated film paper, and then covering the activated impregnated film paper on the surface of the artificial board, and finally hot pressing to obtain the veneer artificial board;

[0048] The artificial board is a fiberboard; the water activation treatment is specifically carried out in the following steps: at room temperature, the coating amount is 0.5g / cm 2 Water is applied to the surface of the high-performance and high-flexibility formaldehyde-free impregnated adhesive film paper to be pasted, and the paper is allowed to stand for 1 to 3 minutes; the hot pressing is specifically performed at a temperature of 200° C. and a pressure of 2 MPa for 1 minute.

[0049] Embodiment 2:

[0050] A method for preparing high-performance and high-flexibility formaldehyde-free impregnated film paper is carried out according to the following steps:

[0051] 1. Under the condition of a rotation speed of 800 rpm, a NaOH solution with a concentration of 2 mol / L was added dropwise to the polyamide epichlorohydrin resin until the pH value reached 9, thereby obtaining a polyamide epichlorohydrin resin after pH adjustment;

[0052] The solid content of the polyamide epichlorohydrin resin is 12.5%;

[0053] 2. Dissolve polyvinyl alcohol in distilled water, then add melamine, react for 6 hours at a temperature of 95°C and a stirring speed of 500 rpm, and finally cool to room temperature to obtain a polyvinyl alcohol / melamine adhesive;

[0054] The mass percentage of polyvinyl alcohol in the polyvinyl alcohol / melamine adhesive is 8%; the mass percentage of melamine in the polyvinyl alcohol / melamine adhesive is 0.75%;

[0055] 3. At room temperature, the decorative base paper is first immersed in the polyamide epichlorohydrin resin after pH adjustment for 5 minutes, and then dried to obtain a primary impregnated paper. At room temperature, the primary impregnated paper is then immersed in the polyvinyl alcohol / melamine adhesive for 2 minutes, and then dried to obtain a high-performance and high-flexibility formaldehyde-free impregnated adhesive film paper;

[0056] The decorative base paper is made of fiber, the manufacturer is Qifeng New Materials Co., Ltd., the model is 9027-83g, the thickness is 0.09mm, and the area is 30×30cm 2 ; The drying is specifically carried out at a temperature of 60°C for 12 minutes; the thickness of the high-performance and high-flexibility formaldehyde-free impregnated film paper is 0.25mm;

[0057] Fourth, subjecting the high-performance and high-flexibility formaldehyde-free impregnated film paper to water activation treatment to obtain activated impregnated film paper, and then covering the activated impregnated film paper on the surface of the artificial board, and finally hot pressing to obtain the veneer artificial board;

[0058] The artificial board is a fiberboard; the water activation treatment is specifically carried out in the following steps: at room temperature, the coating amount is 0.5g / cm 2 Water is applied to the surface of the high-performance and high-flexibility formaldehyde-free impregnated adhesive film paper to be pasted, and the paper is allowed to stand for 1 to 3 minutes; the hot pressing is specifically performed at a temperature of 200° C. and a pressure of 2 MPa for 1 minute.

[0059] Embodiment 3:

[0060] A method for preparing high-performance and high-flexibility formaldehyde-free impregnated film paper is carried out according to the following steps:

[0061] 1. Under the condition of a rotation speed of 800 rpm, a NaOH solution with a concentration of 2 mol / L was added dropwise to the polyamide epichlorohydrin resin until the pH value reached 11, thereby obtaining a polyamide epichlorohydrin resin after pH adjustment;

[0062] The solid content of the polyamide epichlorohydrin resin is 12.5%;

[0063] 2. Dissolve polyvinyl alcohol in distilled water, then add melamine, react for 6 hours at a temperature of 95°C and a stirring speed of 500 rpm, and finally cool to room temperature to obtain a polyvinyl alcohol / melamine adhesive;

[0064] The mass percentage of polyvinyl alcohol in the polyvinyl alcohol / melamine adhesive is 9%; the mass percentage of melamine in the polyvinyl alcohol / melamine adhesive is 0.75%;

[0065] 3. At room temperature, the decorative base paper is first immersed in the polyamide epichlorohydrin resin after pH adjustment for 5 minutes, and then dried to obtain a primary impregnated paper. At room temperature, the primary impregnated paper is then immersed in the polyvinyl alcohol / melamine adhesive for 2 minutes, and then dried to obtain a high-performance and high-flexibility formaldehyde-free impregnated adhesive film paper;

[0066] The decorative base paper is made of fiber, the manufacturer is Qifeng New Materials Co., Ltd., the model is 9027-83g, the thickness is 0.09mm, and the area is 30×30cm 2 ; The drying is specifically carried out at a temperature of 60°C for 12 minutes; the thickness of the high-performance and high-flexibility formaldehyde-free impregnated film paper is 0.25mm;

[0067] Fourth, subjecting the high-performance and high-flexibility formaldehyde-free impregnated film paper to water activation treatment to obtain activated impregnated film paper, and then covering the activated impregnated film paper on the surface of the artificial board, and finally hot pressing to obtain the veneer artificial board;

[0068] The artificial board is a fiberboard; the water activation treatment is specifically carried out in the following steps: at room temperature, the coating amount is 0.5g / cm 2 Water is applied to the surface of the high-performance and high-flexibility formaldehyde-free impregnated adhesive film paper to be pasted, and the paper is allowed to stand for 1 to 3 minutes; the hot pressing is specifically performed at a temperature of 200° C. and a pressure of 2 MPa for 1 minute.

[0069] Embodiment 4:

[0070] A method for preparing high-performance and high-flexibility formaldehyde-free impregnated film paper is carried out according to the following steps:

[0071] 1. Under the condition of a rotation speed of 800 rpm, a NaOH solution with a concentration of 2 mol / L was added dropwise to the polyamide epichlorohydrin resin until the pH value reached 7, thereby obtaining a polyamide epichlorohydrin resin after pH adjustment;

[0072] The solid content of the polyamide epichlorohydrin resin is 12.5%;

[0073] 2. Dissolve polyvinyl alcohol in distilled water, then add melamine, react for 6 hours at a temperature of 95°C and a stirring speed of 500 rpm, and finally cool to room temperature to obtain a polyvinyl alcohol / melamine adhesive;

[0074] The mass percentage of polyvinyl alcohol in the polyvinyl alcohol / melamine adhesive is 8%; the mass percentage of melamine in the polyvinyl alcohol / melamine adhesive is 0.75%;

[0075] 3. At room temperature, the decorative base paper is first immersed in the polyamide epichlorohydrin resin after pH adjustment for 5 minutes, and then dried to obtain a primary impregnated paper. At room temperature, the primary impregnated paper is then immersed in the polyvinyl alcohol / melamine adhesive for 2 minutes, and then dried to obtain a high-performance and high-flexibility formaldehyde-free impregnated adhesive film paper;

[0076] The decorative base paper is made of fiber, the manufacturer is Qifeng New Materials Co., Ltd., the model is 9027-83g, the thickness is 0.09mm, and the area is 30×30cm 2 ; The drying is specifically carried out at a temperature of 60°C for 12 minutes; the thickness of the high-performance and high-flexibility formaldehyde-free impregnated film paper is 0.25mm;

[0077] Fourth, subjecting the high-performance and high-flexibility formaldehyde-free impregnated film paper to water activation treatment to obtain activated impregnated film paper, and then covering the activated impregnated film paper on the surface of the artificial board, and finally hot pressing to obtain the veneer artificial board;

[0078] The artificial board is a fiberboard; the water activation treatment is specifically carried out in the following steps: at room temperature, the coating amount is 0.5g / cm 2 Water is applied to the surface of the high-performance and high-flexibility formaldehyde-free impregnated adhesive film paper to be pasted, and the paper is allowed to stand for 1 to 3 minutes; the hot pressing is specifically performed at a temperature of 200° C. and a pressure of 2 MPa for 1 minute.

[0079] Embodiment 5:

[0080] A method for preparing high-performance and high-flexibility formaldehyde-free impregnated film paper is carried out according to the following steps:

[0081] 1. Under the condition of a rotation speed of 800 rpm, a NaOH solution with a concentration of 2 mol / L was added dropwise to the polyamide epichlorohydrin resin until the pH value reached 9, thereby obtaining a polyamide epichlorohydrin resin after pH adjustment;

[0082] The solid content of the polyamide epichlorohydrin resin is 12.5%;

[0083] 2. Dissolve polyvinyl alcohol in distilled water, then add melamine, react for 6 hours at a temperature of 95°C and a stirring speed of 500 rpm, and finally cool to room temperature to obtain a polyvinyl alcohol / melamine adhesive;

[0084] The mass percentage of polyvinyl alcohol in the polyvinyl alcohol / melamine adhesive is 9%; the mass percentage of melamine in the polyvinyl alcohol / melamine adhesive is 0.75%;

[0085] 3. At room temperature, the decorative base paper is first immersed in the polyamide epichlorohydrin resin after pH adjustment for 5 minutes, and then dried to obtain a primary impregnated paper. At room temperature, the primary impregnated paper is then immersed in the polyvinyl alcohol / melamine adhesive for 2 minutes, and then dried to obtain a high-performance and high-flexibility formaldehyde-free impregnated adhesive film paper;

[0086] The decorative base paper is made of fiber, the manufacturer is Qifeng New Materials Co., Ltd., the model is 9027-83g, the thickness is 0.09mm, and the area is 30×30cm 2 ; The drying is specifically carried out at a temperature of 60°C for 12 minutes; the thickness of the high-performance and high-flexibility formaldehyde-free impregnated film paper is 0.25mm;

[0087] Fourth, subjecting the high-performance and high-flexibility formaldehyde-free impregnated film paper to water activation treatment to obtain activated impregnated film paper, and then covering the activated impregnated film paper on the surface of the artificial board, and finally hot pressing to obtain the veneer artificial board;

[0088] The artificial board is a fiberboard; the water activation treatment is specifically carried out in the following steps: at room temperature, the coating amount is 0.5g / cm 2 Water is applied to the surface of the high-performance and high-flexibility formaldehyde-free impregnated adhesive film paper to be pasted, and the paper is allowed to stand for 1 to 3 minutes; the hot pressing is specifically performed at a temperature of 200° C. and a pressure of 2 MPa for 1 minute.

[0089] Comparative experiment 1:

[0090] A method for preparing high-performance and high-flexibility formaldehyde-free impregnated film paper is carried out according to the following steps:

[0091] 1. Under the condition of a rotation speed of 800 rpm, a NaOH solution with a concentration of 2 mol / L was added dropwise to the polyamide epichlorohydrin resin until the pH value reached 13, thereby obtaining a polyamide epichlorohydrin resin after pH adjustment;

[0092] The solid content of the polyamide epichlorohydrin resin is 12.5%;

[0093] 2. Dissolve polyvinyl alcohol in distilled water, then add melamine, react for 6 hours at a temperature of 95°C and a stirring speed of 500 rpm, and finally cool to room temperature to obtain a polyvinyl alcohol / melamine adhesive;

[0094] The mass percentage of polyvinyl alcohol in the polyvinyl alcohol / melamine adhesive is 7%; the mass percentage of melamine in the polyvinyl alcohol / melamine adhesive is 0.75%;

[0095] 3. At room temperature, the decorative base paper is first immersed in the polyamide epichlorohydrin resin after pH adjustment for 5 minutes, and then dried to obtain a primary impregnated paper. At room temperature, the primary impregnated paper is then immersed in the polyvinyl alcohol / melamine adhesive for 2 minutes, and then dried to obtain a high-performance and high-flexibility formaldehyde-free impregnated adhesive film paper;

[0096] The decorative base paper is made of fiber, the manufacturer is Qifeng New Materials Co., Ltd., the model is 9027-83g, the thickness is 0.09mm, and the area is 30×30cm 2 ; The drying is specifically carried out at a temperature of 60°C for 12 minutes; the thickness of the high-performance and high-flexibility formaldehyde-free impregnated film paper is 0.25mm;

[0097] Fourth, subjecting the high-performance and high-flexibility formaldehyde-free impregnated film paper to water activation treatment to obtain activated impregnated film paper, and then covering the activated impregnated film paper on the surface of the artificial board, and finally hot pressing to obtain the veneer artificial board;

[0098] The artificial board is a fiberboard; the water activation treatment is specifically carried out in the following steps: at room temperature, the coating amount is 0.5g / cm 2 Water is applied to the surface of the high-performance and high-flexibility formaldehyde-free impregnated adhesive film paper to be pasted, and the paper is allowed to stand for 1 to 3 minutes; the hot pressing is specifically performed at a temperature of 200° C. and a pressure of 2 MPa for 1 minute.

[0099] Comparative Experiment 2: This comparative experiment is different from Example 2 in that the water activation treatment in step 4 of Example 2 is eliminated. The rest is the same as Example 2.

[0100] In order to verify the performance characteristics of high-performance and high-flexibility formaldehyde-free impregnated film paper, decorative base paper and melamine impregnated film paper were used as comparative experiments (the decorative base paper is composed of fibers, the manufacturer is Qifeng New Materials Co., Ltd., the model is 9027-83g, the thickness is 0.09mm, the area is 30×30cm 2 The melamine impregnated film paper manufacturer is Shandong Kaide Wood Industry Co., Ltd., the model is warm white, the thickness is 0.2mm, the area is 30×30cm 2 ), and perform the following test:

[0101] The tensile strength test was carried out according to the national standard GB / T453-2002 "Determination of tensile strength of paper and paperboard", and the elongation at break was calculated. The formaldehyde emission was tested according to the national standard GB / T 28995-2022 "Artificial boards and veneers are special paper for veneers".

[0102] The surface physical and mechanical properties are tested in accordance with the national standard GB / T 17657-2022 "Test methods for physical and chemical properties of wood-based panels and veneered wood-based panels", mainly testing the surface bonding strength, surface wear resistance, surface scratch resistance and surface cracking performance of the veneered wood-based panels.

[0103] 1. Surface bonding strength test

[0104] According to the Chinese national standard GB / T 17657-2022, a universal testing machine (AGS-X, Shimadzu) was used to test the surface bonding strength. The sample size was 50mm×50mm×2mm (thickness). A 1000mm 2 The circular groove of the test area is bonded to the circular surface of the test piece with hot melt adhesive. The steel pad on the back of the specimen is bonded with hot melt adhesive to enhance its strength. The tensile speed is 1mm / min. Each sample is tested six times and the average value is taken.

[0105] 2. Surface wear resistance test

[0106] The wear resistance was tested using a wear tester (JM-IV, Pushen Testing Instrument Co., Ltd.) according to the national standard GB / T 17657-2022. Before the test, all specimens and emery cloth were placed at a temperature of 23°C and a relative humidity of 50% for more than 72 hours. A sample with a size of 100mm×100mm was fixed on the wear tester and loaded with two (4.9±0.2)N grinding wheels. The test was stopped when grinding for 350r, the surface condition of the specimen was observed, and the weight loss of the specimen was recorded. Three samples in each group were subjected to standard tests.

[0107] 3. Surface scratch resistance test

[0108] The scratch resistance was tested using a scratch tester (HY-V, Shanghai Tianchen Modern Environmental Technology Co., Ltd.) according to the national standard GB / T 17657-2022. Before the test, all specimens and emery cloth were placed at a temperature of 23°C and a relative humidity of 50% for at least 72 hours. A sample with a size of 100mm×100mm was fixed on the scratch tester, and the surface of the specimen was scratched with a diamond needle under a load pressure of 2N. After the scratching, the specimen was placed at a temperature of 23°C and a relative humidity of 50% for 24 hours. The scratched part of the surface of the specimen was observed.

[0109] 4. Surface crack resistance test

[0110] According to GB / T 17657-2022, the surface crack resistance test is carried out to evaluate the adaptability of the specimen under rapid changes in temperature, humidity and other environmental conditions. The sample with a size of 250mm×250mm is placed in a blast drying oven at 70℃ for 24 hours, and then the specimen is taken out and placed in an environment with a temperature of 23℃ and a relative humidity of 50% for 24 hours to observe its surface changes.

[0111] Table 1 Mechanical properties and formaldehyde emission of paper

[0112]

[0113] As shown in the table, it can be seen that the tensile strength of the impregnated film paper prepared in the example is higher than that of the decorative base paper (11.87 MPa), and is equivalent to that of the melamine impregnated film paper. The elongation at break of the impregnated film paper is more than 5 times that of the decorative base paper (0.81%), and more than 9 times that of the melamine impregnated film paper (0.47%), which shows that the impregnated film paper has better flexibility.

[0114] Figure 1 Actual pictures of the flexibility of the high-performance and high-flexibility formaldehyde-free impregnated film paper, decorative base paper and melamine impregnated film paper prepared in Example 4, a is the decorative base paper, b is the melamine impregnated film paper, and c is the high-performance and high-flexibility formaldehyde-free impregnated film paper; it can be seen from the figure that the formaldehyde-free flexible impregnated film paper has better flexibility.

[0115] Table 2 Physical and chemical properties of veneer panels

[0116]

[0117]

[0118] As other performances of comparative experiments 1 and 2 were unqualified, no subsequent performance tests were conducted; “ / ” in the table indicates that no relevant tests were conducted.

[0119] As can be seen from the table, the surface bonding strength test of the veneer wood-based panels in comparative experiment 1 did not reach the national standard (≥0.6MPa). The surface bonding strength and surface wear resistance of the veneer wood-based panels in Examples 1, 2, 3, 4 and 5 reached the national standard (<80mg / 100r), the surface scratch resistance reached the national standard (>1.5N surface without more than 90% continuous scratches), and the surface crack resistance reached the national standard (no cracks, bubbling, discoloration, wrinkles).

[0120] According to the requirements of GB / T15102-2017 "Impregnated Film Paper Veneer Fiberboard and Particleboard" on surface bonding strength, surface wear resistance and surface scratch resistance, the surface bonding strength of the prepared veneer artificial board is ≥0.60MPa, surface wear resistance is <80mg / 100r, surface scratch resistance is >1.5N, the surface has no continuous scratches greater than 90%, and the surface crack resistance has no cracks, bubbling, discoloration, and wrinkles, which is qualified. It can be seen that the embodiment improves the performance of environmentally friendly formaldehyde-free flexible impregnated film paper by effectively controlling the pH of the impregnated polyamidochloropropane resin and the content of polyvinyl alcohol / melamine adhesive.

[0121] Figure 2 is an infrared spectrum; a is the decorative base paper, b is the once impregnated paper prepared in step 3 of Example 4, and c is the high-performance and high-flexibility formaldehyde-free impregnated film paper prepared in step 3 of Example 4; the structural changes of the impregnated decorative paper were analyzed by infrared. Compared with the decorative base paper (a), the impregnated paper (b) impregnated with PAE resin for the first time has a peak value of 1639cm -1 The C=O absorption peak becomes stronger, 1550cm -1 The absorption peak of amide II (NH) becomes stronger at 1727 cm -1 The peaks at 3000cm are the characteristic peaks of the ester bond formed between the azetidinyl group of PAE resin and the carboxyl group of cellulose, and the stretching vibration of the ester bond formed between the carboxyl group at the end of the polyamide chain and the azetidinyl group in PAE, proving that the PAE resin was successfully impregnated into the base paper to form the first network structure. -1 ~3650cm -1 The broadening of the OH peak is due to the hydrogen bonding between the impregnated PAE decorative paper and PVA / MA. -1 The NH bond peak at 800 cm -1 ~847cm -1 The absorption peak of the triazine ring of MA is generated at the bottom. This indicates that the PVA / MA adhesive is successfully coated on the decorative paper impregnated with PAE resin to form a chemically and physically combined double cross-linked network structure through hydrogen bond supramolecular cross-linking to form an impregnated adhesive film paper (c).

[0122] Figure 3This is a physical picture of the polyvinyl alcohol / melamine adhesive prepared in Example 2; as can be seen from the figure, the adhesive is highly transparent.

[0123] Figure 4 The following are actual pictures of decorative base paper and impregnated adhesive film paper, where a is decorative base paper and b is high-performance and high-flexibility formaldehyde-free impregnated adhesive film paper prepared in Example 2. As can be seen from the figure, the adhesive prepared in the example has high transparency and does not affect the texture of the paper.

Claims

1. A method for preparing high-performance and high-flexibility formaldehyde-free impregnated film paper, characterized in that It is carried out in the following steps:

1. adjusting the pH value of the polyamide epichlorohydrin resin to 7-11 to obtain the pH-adjusted polyamide epichlorohydrin resin; 2. Dissolve polyvinyl alcohol in distilled water, then add melamine, react for 1h to 7h at a temperature of 90°C to 100°C and a stirring speed of 300rpm to 600rpm, and finally cool to room temperature to obtain a polyvinyl alcohol / melamine adhesive; 3. At room temperature, the decorative base paper is first impregnated in the polyamide epichlorohydrin resin after pH adjustment, and then dried to obtain a primary impregnated paper. At room temperature, the primary impregnated paper is then impregnated in a polyvinyl alcohol / melamine adhesive, and then dried to obtain a high-performance and high-flexibility formaldehyde-free impregnated film paper.

2. The method for preparing a high-performance and high-flexibility formaldehyde-free impregnated film paper according to claim 1, characterized in that In step 1, at a rotation speed of 500 rpm to 1000 rpm, a NaOH solution with a concentration of 1 mol / L to 3 mol / L is added dropwise to the polyamide epichlorohydrin resin until the pH value is 7 to 11.

3. The method for preparing a high-performance and high-flexibility formaldehyde-free impregnated film paper according to claim 1, characterized in that The solid content of the polyamide epichlorohydrin resin described in step 1 is 5% to 20%.

4. The method for preparing a high-performance and high-flexibility formaldehyde-free impregnated film paper according to claim 1, characterized in that The mass percentage of polyvinyl alcohol in the polyvinyl alcohol / melamine adhesive described in step 2 is 5% to 20%; the mass percentage of melamine in the polyvinyl alcohol / melamine adhesive described in step 2 is 0.1% to 2%.

5. The method for preparing a high-performance and high-flexibility formaldehyde-free impregnated film paper according to claim 1, characterized in that In step 3, the decorative base paper is first immersed in the polyamide epichlorohydrin resin after pH adjustment at room temperature for 2 minutes to 10 minutes.

6. The method for preparing a high-performance and high-flexibility formaldehyde-free impregnated film paper according to claim 1, characterized in that In step 3, the primary impregnated paper is again immersed in the polyvinyl alcohol / melamine adhesive at room temperature for 2 to 5 minutes.

7. The method for preparing a high-performance and high-flexibility formaldehyde-free impregnated film paper according to claim 1, characterized in that The drying described in step 3 is specifically carried out at a temperature of 50° C. to 90° C. for 10 min to 15 min.

8. The use of a high-performance and high-flexibility formaldehyde-free impregnated film paper prepared as claimed in claim 1, characterized in that It is used as a facing material for artificial boards.

9. The use of a high-performance and high-flexibility formaldehyde-free impregnated film paper according to claim 8, characterized in that When it is used as a facing material for artificial boards, it is specifically carried out in the following steps: The high-performance and high-flexibility formaldehyde-free impregnated film paper is subjected to water activation treatment to obtain activated impregnated film paper, and then the activated impregnated film paper is covered on the surface of the artificial board, and finally hot-pressed to obtain the veneered artificial board.

10. The use of a high-performance and high-flexibility formaldehyde-free impregnated film paper according to claim 9, characterized in that The water activation treatment is specifically carried out in the following steps: at room temperature, the coating amount is 0.1 g / cm 2 ~1g / cm 2 Water is applied to the surface of the high-performance and high-flexibility formaldehyde-free impregnated adhesive film paper to be pasted, and the paper is allowed to stand for 1 to 3 minutes; the hot pressing is specifically performed at a temperature of 170°C to 230°C and a pressure of 1MPa to 3MPa for 10s to 3min.

Citation Information

Patent Citations

  • Cracking-resistant ecological board and production process thereof

    CN110666904A

  • Formaldehyde-free hot-pressed impregnated decorative paper and preparation method thereof

    CN114293402A

  • Preparation method of flexible decorative film and product thereof

    CN116791406A

  • Wear-resistant decorative paper and preparation method thereof

    CN117604817A

  • Preparation method and bonding method of polyvinyl alcohol solvent-free adhesive

    CN118256173A

Cited By

  • High-strength waterproof formaldehyde-free impregnated paper adhesive and preparation method thereof

    CN119529707A