Waterproof and oil-proof environment-friendly coating as well as preparation and application thereof

The Pickering emulsion-type structure of the Janus-type nanocellulose waterproof, oil-proof and environmentally friendly coating solves the problem of insufficient waterproof and oil-proof performance of cellulose-based materials, achieves efficient and environmentally friendly hydrophobic, waterproof and oil-proof effects, and simplifies the preparation process, which is suitable for Large-scale application of cellulose-based materials.

CN118727503AInactive Publication Date: 2024-10-01QUZHOU RES INST OF ZHEJIANG UNIV

Patent Information

Application Number
CN202410995259.8
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Filing Date
2024-07-24
Publication Date
2024-10-01
Estimated Expiration
Not applicable · inactive patent

AI Technical Summary

Technical Problem

Existing cellulose-based sheet materials have deficiencies in waterproof and oil-proof properties, and non-degradable polymers and organic solvents are often used in traditional methods, which leads to environmental and economic problems and makes it difficult to achieve large-scale application.

Method used

Janus type nanocellulose waterproof and oil-proof environmentally friendly coating is used. Its structure is Pickering emulsion type, including oil phase components and water phase components. The nanocellulose modified by a silane coupling agent is combined with natural polysaccharide substances to form a hydrophobic, waterproof and oil-proof layer. The use of organic solvents is avoided, and the preparation process is simplified through a one-step emulsification process.

Benefits of technology

It achieves efficient hydrophobic, waterproof, and oil-proof properties, improves the mechanical properties and air permeability of the paper, and reduces the water vapor transmission rate. The process is simple, environmentally friendly, and suitable for industrial applications.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN118727503A_ABST
    Figure CN118727503A_ABST
Patent Text Reader

Abstract

The invention discloses a waterproof oil-proof environment-friendly coating as well as a preparation method and application thereof. The environment-friendly coating is a Janus type nanocellulose coating prepared by a Pickering emulsion template method, a part of active hydroxyl groups on the surface of nanocellulose are connected with a waterproof component, and the other part of hydroxyl groups are connected with an oil-proof component through hydrogen bonds (three free hydroxyl groups are arranged on each ring in the middle of a cellulose macromolecular chain, two free hydroxyl groups are secondary hydroxyl groups (C2 and C3), one free hydroxyl group is primary hydroxyl group (C6), and the other free hydroxyl group is secondary hydroxyl groups (C2 and C3). Due to the fact that the affinity of the emulsion and components at the two ends of the Janus type nanocellulose is different, the waterproof end is exposed on the outer layer and the oil-proof end is combined with the substrate on the bottom layer through emulsion breaking, and the structure can well solve the problems that water and oil repel each other and cannot be achieved at the same time. The coating does not contain any organic solvent, is an environment-friendly and safe coating with good hydrophobicity, water resistance and oil resistance, can solve the problems that a current cellulose-based sheet material is not water-resistant and oil-resistant and is poor in barrier property, and has a large-scale application prospect.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The present invention relates to the technical field of waterproof and oil-proof environmentally friendly coatings, and more specifically, to a Janus-type nanocellulose environmentally friendly coating with hydrophobic, waterproof and oil-proof functions, a preparation method thereof, and an application thereof in waterproof and oil-proof paper. Background Art

[0002] Cellulose-based sheet materials are widely used due to their wide sources, low cost, renewable and biodegradable properties, and are expected to replace plastic packaging in the packaging field. However, due to the porosity and hydrophilicity of cellulose-based sheet materials, they have no barrier effect on gas, water and oil, and their strength is seriously reduced in high humidity environments or when exposed to water, which greatly limits their further application. Therefore, many methods are used to improve the waterproof and oil-proof properties of cellulose-based sheet materials to further expand their application range. For example, sizing agents are commonly used in the papermaking industry to improve the water resistance of paper; in the post-processing process, a polymer barrier layer (commonly used are polypropylene, low-density polyethylene, polyvinyl chloride and polyethylene terephthalate) is also formed on the surface of cellulose-based sheet materials through coating or lamination methods. Although the addition of sizing agents can improve the water resistance of paper, the amount of sizing agents used is large, the sizing agent loss is serious, and the economic efficiency is poor. The introduction of non-degradable polymers has indeed brought about significant improvements in water and oil resistance, but on the one hand, the polymer layer is difficult to separate from the cellulose-based sheet material, which makes it difficult to recycle and reuse the cellulose-based sheet material. On the other hand, the polymer layer cannot be degraded, which will aggravate the problem of microplastics. In the current situation where the intensity of "plastic restriction" and "plastic ban" is increasing, this method is not applicable to the preparation of disposable products.

[0003] In recent years, researchers have done a lot of work on the hydrophobicity, waterproofness and oil resistance of cellulose-based sheet materials. For example, CN 116084209 B introduces an inner oil-proof coating and an outer oil-proof coating by a double coating method to prepare a fluorine-free, degradable, waterproof and oil-proof packaging paper. However, this method is cumbersome, inefficient and difficult to apply industrially. CN 117265909 A uses a nanocellulose particle solution modified by long-chain alkyltrimethoxysilane and mixed with ethyl cellulose to prepare a waterproof and oil-proof barrier material, and coats it on the surface of paper to prepare waterproof and oil-proof paper. Although this method avoids the problems caused by multi-layer coating, an organic solvent is required in the preparation process of the waterproof and oil-proof barrier material, and the solvent is volatile, which has a negative impact on the environment and also endangers the health of operators. CN 116695483A mixes nano-modified cellulose with aqueous acrylic resin emulsion to prepare a waterproof and oil-proof coating, and compounds it on the surface of base paper to prepare waterproof and oil-proof paper. Although the coating avoids the use of organic solvents, the acrylic resin is non-degradable and still causes microplastic problems after the paper is discarded. CN111749046A prepares an alkyl ketene dimer sizing agent by a two-step emulsification method and uses it for paper surface sizing. The sizing degree of the paper is excellent, but its oil resistance is poor. Therefore, there is an urgent need for an environmentally friendly waterproof and oil-proof coating for improving the waterproof and oil-proof properties of cellulose-based sheet materials, and taking into account both operability and economy. Summary of the invention

[0004] Based on the above problems, the purpose of the present invention is to provide a Janus-type nanocellulose waterproof and oil-proof environmentally friendly coating and its preparation method and application, so as to solve the problem that at this stage it is impossible to provide a waterproof and oil-proof coating that is environmentally friendly and safe and can be used on a large scale and has good hydrophobicity, waterproofness and oil resistance.

[0005] In one aspect, the present invention provides a Janus-type (Janus-type generally refers to an object or structure with two-sidedness or asymmetry) nanocellulose waterproof and oil-proof environmentally friendly coating, characterized in that its structure is a Pickering emulsion type, comprising the following components:

[0006] The oil phase component is one or more of wax, alkyl ketene dimer AKD, alkenyl succinic anhydride ASA, and rosin; the wax is one or more of plant wax, animal wax, and food-grade paraffin wax.

[0007] The aqueous phase component is Janus-type nanocellulose, one end of which is connected to an oil-proof component and the other end is a waterproof component. The waterproof component is mainly a silane coupling agent (including but not limited to hexadecyltrimethoxysilane, methyltrimethoxysilane, γ-methacryloxypropyltrimethoxysilane (KH570), 3-aminopropyltriethoxysilane (KH550), diaminopropyltriethoxysilane (KH560), vinyltriethoxysilane, vinyltrimethoxysilane), and the oil-proof component is a natural polysaccharide substance and its derivatives or polyvinyl alcohol (degree of polymerization is 1700±50, degree of alcoholysis is 88-99), etc.

[0008] In the above technical solution, the Pickering emulsion structure will demulsify under heating conditions. The hydrophobic end of the Janus nanocellulose will migrate to the coating surface due to its poor compatibility with the oil phase and low surface energy. The oil-proof component end can enter the interior of the paper, fill the fiber pores, reduce the porosity of the paper, and form a dense barrier layer to prevent oily substances from entering the interior of the paper. In addition, natural polysaccharides contain a large number of polar groups that repel the non-polar groups of the oil, which further improves the oil-proof performance. In addition, these polar groups can form hydrogen bonds with the hydroxyl groups on the surface of the paper fiber, thereby improving the mechanical properties of the paper.

[0009] Furthermore, the natural polysaccharide substance is selected from one or more of cellulose and its derivatives, chitosan, sodium alginate, starch, guar gum, and polyvinyl alcohol.

[0010] Furthermore, the oil-in-water Pickering emulsion is an oil phase component emulsified by Janus nanocellulose.

[0011] Further, the nanocellulose is selected from one or more of nanocellulose (diameter of 2-10 nm, length of 1-5 μm), cellulose nanocrystals (most of the amorphous regions of nanocellulose are removed, and the crystalline regions are retained, with a diameter of 2-6 nm and a length of 100-500 nm), and wood nanocellulose (containing 2-25% lignin and 2-20% hemicellulose, by mass);

[0012] Furthermore, the Janus type nanocellulose is surface-modified at one end by a silane coupling agent and connected to a natural polysaccharide substance at one end by a hydrogen bond. The degree of substitution of the silane coupling agent is 0.2-1 (preferably 0.4-0.9, more preferably 0.5-0.8) (the degree of substitution of cellulose refers to the amount of substances substituted on each D-glucose unit of cellulose, with a maximum value of 3); the amount of natural polysaccharide substance added relative to the mass fraction of the modified nanocellulose is 10%-200% (preferably 50%-150%, more preferably 75%-125%).

[0013] The oil phase component is selected from one or more of wax, AKD, ASA and rosin.

[0014] Furthermore, the wax is selected from one or more of plant waxes (palm wax, candelilla wax, rice bran wax, sugarcane wax, laurel wax, castor bean wax, etc.), animal wax (beeswax, insect wax, spermaceti, wool wax, etc.), and food-grade paraffin.

[0015] Furthermore, in the Pickering emulsion structure, the mass ratio of the Janus type nanocellulose component, the oil phase component and water is 0.5-5:0.5-10:99-85 (preferably 2-5:2-8:96-87, more preferably 2-5:3-7.5:95-87.5).

[0016] Furthermore, the degree of substitution DS of the hydrophobic end of the Janus type nanocellulose is 0.2-1, preferably 0.5-0.8, under which condition good hydrophobicity can be obtained; the amount of the oil-proof component added is 10%-200% relative to the mass fraction of the modified nanocellulose, preferably 50%-150%, under which condition good oil-proofness can be obtained. When the oil-proof component is too little, the oil-proof property will be poor; when the hydrophobic component is too little, its water-proof and oil-proof performance will deteriorate. When the silane coupling agent substitution degree is too high or there are too many oil-proof components, it cannot be guaranteed that the hydrophobic component is in the outer layer and the oil-proof component is in the inner layer when the Pickering emulsion is demulsified, so the water-proof and oil-proof effect will deteriorate.

[0017] In another aspect, the present invention provides a method for preparing the waterproof and oil-proof environmentally friendly coating as described in the first object above, the preparation method comprising the following steps:

[0018] The oil phase component and the Janus nanocellulose are mixed evenly, emulsified together, and cooled to obtain the waterproof and oil-proof environmentally friendly coating.

[0019] Furthermore, the mixing method is: slowly adding the oil phase component into the Janus nanocellulose dispersion under stirring conditions.

[0020] Furthermore, the emulsification process: the emulsification process is accelerated under heating conditions.

[0021] In yet another aspect, the present invention provides the use of the waterproof and oil-proof environmentally friendly coating as described in the first aspect above in the preparation of a hydrophobic, waterproof and oil-proof cellulose-based sheet material.

[0022] Furthermore, the waterproof and oil-proof environmentally friendly coating is applied to the surface of a cellulose-based sheet material and dried to obtain a hydrophobic, waterproof and oil-proof cellulose-based sheet material.

[0023] Furthermore, the application amount of the waterproof and oil-proof environmentally friendly coating is 2-10 g / m2 , through comprehensive consideration of economy and coating performance, 3-6g / m 2 .

[0024] Furthermore, the applying method is one of dip coating, spin coating, scraping coating and coating.

[0025] Furthermore, the waterproof and oil-proof environmentally friendly coating can be applied to one surface or both surfaces of the cellulose-based sheet material, and the specific surface can be selected according to the actual environment where the hydrophobic treatment is required.

[0026] Furthermore, the cellulose-based sheet material suitable for the present invention can be a sheet material with a porous network structure produced from natural plant fibers as raw materials or substrates. Preferably, the cellulose-based sheet material includes, but is not limited to, conventionally used paper selected from kraft paper, corrugated paper, parchment paper, newsprint, white cardboard, printing paper, etc.

[0027] Furthermore, the hydrophobic, waterproof and oil-proof cellulose-based sheet material is a hydrophobic and oil-proof paper packaging, paper straws, paper lunch boxes, paper cups, etc.

[0028] The preparation method is a Pickering emulsion template method, and the water-in-oil type Pickering emulsion structure is formed by emulsifying the Janus type nanocellulose water phase and the oil phase components; it includes the following steps:

[0029] 1) adjusting the pH of a 0.1-5wt.% nanocellulose aqueous suspension (preferably 1-5wt.%) to 8-10 (according to the selected silane coupling agent) with a NaOH solution, transferring it into a three-necked flask with stirring and reflux, adding a silane coupling agent dropwise to the three-necked flask and reacting for 4-6 hours (according to the selected silane coupling agent, adjusting the reaction time), so that the degree of substitution of the silane coupling agent is 0.2-1, and calculating the degree of substitution by weighing method (the weight gain before and after the reaction); washing with distilled water by centrifugation until neutral, and reconfiguring the mass fraction of the silane-modified nanocellulose aqueous suspension to be 0.1-1wt.% (preferably 1-5wt.%);

[0030] 2) adding a certain amount of natural polysaccharide to the silane-modified nanocellulose aqueous suspension (controlling the mass ratio of natural polysaccharide to modified nanocellulose to be 10%-200% (preferably 50%-150%)), heating and stirring at 25-90° C. (preferably 60-90° C.) for 1-3 h (preferably 1.5-3 h) until the mixture is uniformly mixed to obtain a Janus-type nanocellulose aqueous suspension;

[0031] 3) Adding 0.5-5 parts of Janus nanocellulose, 99-85 parts of water, and 0.5-10 parts of oil phase substance to the above suspension under heating and stirring conditions at 25-90° C. (preferably 60-90° C.), emulsifying for 5-180 min (preferably 5-60 min), and cooling to room temperature to obtain the waterproof and oil-proof environmentally friendly coating.

[0032] The environmentally friendly coating of the present invention is a Janus type nanocellulose coating prepared by a Pickering emulsion template method, a part of the more active hydroxyl groups on the surface of the nanocellulose are connected to the waterproof component, and the remaining hydroxyl groups are connected to the oil-proof component through hydrogen bonds (there are three free hydroxyl groups on each ring in the middle of the cellulose macromolecular chain, two of which are secondary hydroxyl groups (C2, C3), and one is a primary hydroxyl group (C6), and the activity is stronger in the primary hydroxyl group). Due to the different affinity between the components at both ends of the emulsion and the Janus type nanocellulose, the emulsion is demulsified, so that the waterproof end is exposed to the outer layer, and the oil-proof end is combined with the substrate at the bottom layer. This structure can well solve the problem that waterproof and oil-proof repel each other and cannot be achieved at the same time. The coating does not contain any organic solvent, is an environmentally friendly and safe coating with good hydrophobicity, waterproofness, and oil resistance, can solve the problems of the current cellulose-based sheet materials being not water-resistant, not oil-resistant, and having poor barrier properties, and has a prospect for large-scale application.

[0033] The beneficial effects of the present invention are as follows:

[0034] The waterproof and oil-proof environmentally friendly coating provided in the present invention has a Pickering emulsion structure, a spherical microstructure, high stability, does not use any organic solvents, is green and environmentally friendly, can be prepared by emulsification in one step, is simple to operate, and has high industrial feasibility. The waterproof and oil-proof environmentally friendly coating is applied to cellulose-based sheet materials to give the material good hydrophobic, waterproof, oil-proof and barrier properties. Among them, the water contact angle can reach up to 138°, and the Cobb60 value can reach as low as 5.5g / m 2 , the hydrophobic, waterproof and oil-proof properties are greatly improved, the air permeability is greatly reduced, the oil-proof performance Kit value is as high as 12, the water vapor permeability is greatly reduced, and the tensile strength of the paper is improved. BRIEF DESCRIPTION OF THE DRAWINGS

[0035] The specific implementation modes of the present invention are further described in detail below in conjunction with the accompanying drawings.

[0036] Figure 1 The SEM image of the water- and oil-proof coating of Example 1 is shown.

[0037] Figure 2 A physical picture showing the waterproof and oil-proof coating of Example 1

[0038] Figure 3The photograph (a) shows the state of water droplets on the surface of the water-proof and oil-proof paper of Example 1 and the photograph (b) shows the state of water droplets on the surface of the paper after wiping the paper for 5 minutes.

[0039] Figure 4 The photo shows the state of castor oil on the surface of water-proof and oil-proof paper in Example 1 (a) and the photo after castor oil was wiped on the paper surface for 5 minutes (b). DETAILED DESCRIPTION

[0040] In order to more clearly illustrate the present invention, the present invention is further described below in conjunction with preferred embodiments and accompanying drawings. Similar components in the accompanying drawings are represented by the same reference numerals. It should be understood by those skilled in the art that the content specifically described below is illustrative rather than restrictive, and should not be used to limit the scope of protection of the present invention.

[0041] Test the oil resistance of paper samples according to TAPPI T 559cm-12 standard. Drop solutions 1 to 12 of different ratios of castor oil / heptane / toluene from 2.54cm above the sample, and wipe after 15 seconds to see if the contact between the sample and the oil drop becomes darker. It is expressed by the kit value, where the maximum kit value is 12, and the larger the kit value, the better the oil resistance.

[0042] The air permeability of the paper samples was tested according to ISO 5636-2 standard using the Schhopper method (ZB-TQ1000) at 10.0 ± 0.2 cm 2 The samples were tested at 20±5℃. Each sample was tested at least three different locations to get the average value.

[0043] The hydrophobic properties of the samples were characterized by the water contact angle. The water contact angle of the paper samples was measured by using a contact angle tester DataPhysics OCA-20 at room temperature using 3 μL of deionized water. The larger the water contact angle, the more hydrophobic the prepared material is.

[0044] The water absorption Cobb60 value of the paper sample was tested according to ISO 535-2014. The paper sample (size) was placed in contact with 100 mL of deionized water at 20±1°C for 60 seconds using a Cobb water absorption meter (ZB-Cobb25) (the coated surface was the test surface), and each sample was tested three times to obtain the average value.

[0045] Tensile strength test: Cut the paper sample into strips with a length of 60mm and a width of 5mm, and use a universal mechanical testing machine for testing. The thickness of the strip is measured using a micrometer before testing, and the gauge length is set to 30mm, and the tensile speed is 5mm / min. Before testing, the sample needs to be balanced at room temperature with a humidity of 55% for 24 hours. At least five strips are tested for each sample, and the average value is taken as the final result.

[0046] Example 1

[0047] Here we take nanocellulose, methyltrimethoxysilane, polyvinyl alcohol 1799 and palm wax as examples

[0048] Nanocellulose (diameter 2-5 nm, length 1-3 μm) was prepared into 100 g dispersion (water as solvent) with a concentration of 3 wt%, dispersed evenly under ultrasound, adjusted to pH 10 with 0.1 M NaOH solution, added with 1 g methyltrimethoxysilane (136.22 g / mol), reacted for 4 h, and then washed to remove the unreacted silane coupling agent, to obtain nanocellulose with a degree of substitution of 0.5 (the degree of substitution was calculated by the weight gain), and a grafted mass of methyltrimethoxysilane of 0.41 g, to obtain silane-modified nanocellulose;

[0049] Reconfigure the water suspension of silane-modified nanocellulose to have a mass fraction of 3 wt.%, and obtain 100 g of nanocellulose dispersion;

[0050] Then, 4 g of polyvinyl alcohol was weighed and slowly added into the above 100 g of nanocellulose dispersion under heating and stirring at 90° C. After the polyvinyl alcohol was completely dissolved, it was stirred for 60 minutes to obtain a Janus-type nanocellulose mixed dispersion.

[0051] 7 g of palm wax was weighed and added to the above 104 g of mixed dispersion, and then 29 g of deionized water was added so that the mass ratio of palm wax, Janus nanocellulose and water was 5:5:90, and the mixture was heated to 90°C and emulsified at 30000 rpm for 5 min. After the emulsification, the mixture was cooled and the waterproof and oil-proof coating (waterproof and oil-proof agent) was obtained when the emulsion temperature dropped to room temperature.

[0052] Preparation of waterproof and oil-proof paper:

[0053] The weight is 80g / m 2 Unsized kraft paper (untreated base paper, blank kraft paper) was dried in an oven at 60°C for 2 h, and then the waterproof and oil-proof agent was coated on the surface of the paper by coating (only one side was coated, and the coated side was the test side), with a coating amount of 5 g / m 2 The coated paper was placed in an oven at 70°C and dried completely. The waterproof and oil-proof properties of the paper were then characterized. The water contact angle of the obtained paper was 122° and the cobb60 value was 9g / m 2 , kit value is 8, air permeability is 0.17μm / Pa·s, tensile strength is 37MPa. The water contact angle of blank kraft paper is 60°, and the cobb60 value is 88g / m 2 , kit value is 0, air permeability is 9.67μm / Pa·s, and tensile strength is 28MPa. This shows that the addition of waterproof and oil-proof coating improves the waterproof and oil-proof properties of kraft paper.

[0054] Example 2

[0055] Take nanocellulose, 3-aminopropyltriethoxysilane, starch and ASA as examples:

[0056] Nanocellulose (diameter 2-5 nm, length 1-3 μm) was prepared into 100 g dispersion (water as solvent) with a concentration of 3 wt%, dispersed evenly under ultrasound, 0.1 M NaOH solution was used to adjust the pH to 9, 0.6 g of 3-aminopropyltriethoxysilane (221.37 g / mol) was added, reacted for 5 h, and then washed to remove the unreacted silane coupling agent, the degree of substitution of nanocellulose was 0.2, and the grafting mass of 3-aminopropyltriethoxysilane was 0.27 g, to obtain silane-modified nanocellulose;

[0057] Reconfigure the water suspension of silane-modified nanocellulose to have a mass fraction of 3 wt.%, and obtain 100 g of nanocellulose dispersion;

[0058] Then, 0.8 g of starch was weighed and slowly added into the above 100 g of nanocellulose dispersion under stirring, and the mixture was heated to 95° C. and stirred for 60 min to obtain a Janus-type nanocellulose mixed dispersion.

[0059] Then, 11.4 g of ASA and 14.47 g of water were weighed and added to the above-mentioned mixed 100.8 g dispersion, so that the ratio of Janus nanocellulose: ASA mass: water was 3:9:88, heated to 90°C, and emulsified at 30,000 rpm for 5 minutes. After the emulsification was completed, it was cooled, and the waterproof and oil-proof coating (waterproof and oil-proof agent) was obtained when the emulsion temperature dropped to room temperature.

[0060] Preparation of waterproof and oil-proof paper:

[0061] The unsized white cardboard was dried in an oven at 60°C for 2 hours, and then the waterproof and oil-proof agent was coated on the paper surface by knife coating (only one side was coated, and the test side was the coated side), with a coating amount of 3g / m 2 The coated paper was placed in an oven at 70°C and dried completely. The waterproof and oil-proof properties of the paper were then characterized. The water contact angle of the obtained paper was 125° and the cobb60 value was 7.8 g / m 2 ,kit value is 6, air permeability is 0.23μm / Pa·s, tensile strength is 57MPa. Blank white cardboard water contact angle is 65°, cobb60 value is 64g / m 2 , kit value is 0, air permeability is 7.84μm / Pa·s, and tensile strength is 48MPa. This shows that the addition of waterproof and oil-proof coating improves the waterproof and oil-proof performance of white cardboard.

[0062] Example 3

[0063] Take wood nanocellulose, hexadecyltrimethoxysilane, chitosan and AKD as examples:

[0064] The wood nanocellulose (lignin content of 15.7%, diameter of 2-10 nm, length of 1-3 μm) was prepared into 100 g dispersion (water as solvent) with a concentration of 3 wt%, and dispersed evenly under ultrasound. The pH was adjusted to 10 with 0.1 M NaOH solution, and 3 g of hexadecyltrimethoxysilane (346.62 g / mol) was added to react for 6 h, and then the unreacted silane coupling agent was removed by washing. The degree of substitution of the nanocellulose was controlled to be 0.8, and the grafting mass of hexadecyltrimethoxysilane was 1.71 g, thereby obtaining silane-modified wood nanocellulose.

[0065] Reconfigure the water suspension of silane-modified nanocellulose to have a mass fraction of 3 wt.%, and obtain 100 g of wood nanocellulose dispersion;

[0066] Then, 2 g of chitosan was weighed and slowly added into the 100 g mixed dispersion under stirring at room temperature, and stirred for 2 h until the chitosan was completely dissolved to obtain a Janus-type nanocellulose mixed dispersion.

[0067] Then, 10 g of AKD and 54.67 g of deionized water were weighed and added to the above 102 g of the mixed dispersion so that the ratio of Janus-type wood nanocellulose: AKD: water was 3:6:91, heated to 90°C, and emulsified at 30,000 rpm for 5 minutes. After the emulsification, it was cooled and the waterproof and oil-proof coating (waterproof and oil-proof agent) was obtained when the emulsion temperature dropped to room temperature.

[0068] Preparation of waterproof and oil-proof paper:

[0069] The unsized corrugated paper was dried in an oven at 60°C for 2 h, and then the waterproof and oil-proof agent was applied to the paper surface by spin coating (double-sided coating), with a total coating amount of 10 g / m 2 The coated paper was placed in an oven at 70°C and dried for 2 hours. The waterproof and oil-proof properties of the paper were then characterized. The water contact angle of the obtained paper was 135° and the cobb60 value was 6.1 g / m 2 ,kit value is 10, air permeability is 0.19μm / Pa·s, tensile strength is 45MPa. The water contact angle of blank corrugated paper is 52°, and the cobb60 value is 91g / m 2 , kit value is 0, air permeability is 9.44μm / Pa·s, and tensile strength is 36MPa. This shows that the addition of waterproof and oil-proof coating greatly improves the waterproof and oil-proof performance of corrugated paper.

[0070] Example 4

[0071] Take nanocellulose, γ-methacryloxypropyltrimethoxysilane, sodium alginate and rosin as examples:

[0072] Nanocellulose (diameter 2-5 nm, length 1-3 μm) was prepared into 100 g dispersion (water as solvent) with a concentration of 3 wt%, dispersed evenly under ultrasound, 0.1 M NaOH solution was used to adjust the pH to 10, 2.5 g of γ-methacryloxypropyltrimethoxysilane (248.35 g / mol) was added, reacted for 5 h, and then washed to remove the unreacted silane coupling agent, the substitution degree of nanocellulose was controlled at 0.5, and the grafting mass of γ-methacryloxypropyltrimethoxysilane was 0.77 g, to obtain silane-modified nanocellulose;

[0073] Reconfigure the water suspension of silane-modified nanocellulose to have a mass fraction of 3 wt.%, and obtain 100 g of nanocellulose dispersion;

[0074] Then, 0.5 g of sodium alginate was weighed and slowly added into the 100 g of the nanocellulose dispersion under stirring at room temperature, and stirred for 1 h until the sodium alginate was completely dissolved to obtain a Janus-type nanocellulose mixed dispersion.

[0075] Then, 7 g of rosin and 9.17 g of deionized water were weighed and added to the above 100.5 g of the mixed dispersion, so that the ratio of Janus nanocellulose: rosin: water was 3:6:91, heated to 90 ° C, and emulsified at 30000 rpm for 5 minutes. After the emulsification, it was cooled and the emulsion temperature was cooled to room temperature to obtain a waterproof and oil-proof coating (waterproof and oil-proof agent).

[0076] Preparation of waterproof and oil-proof paper:

[0077] The unsized printed paper was dried in an oven at 60°C for 2 h, and then the waterproof and oil-proof agent was coated on the surface of the paper (one-sided coating was performed, and the coated side was the test side), with a coating amount of 5 g / m 2 The coated paper was placed in an oven at 70°C and dried for 2 hours. The waterproof and oil-proof properties of the paper were then characterized. The water contact angle of the obtained paper was 119° and the cobb60 value was 7.4 g / m 2 ,kit value is 5, air permeability is 0.21μm / Pa·s, tensile strength is 31MPa. The water contact angle of blank printed paper is 63°, and the cobb60 value is 69g / m 2 , kit value is 0, air permeability is 7.49μm / Pa·s, and tensile strength is 23MPa. This shows that the addition of waterproof and oil-proof coating improves the waterproof and oil-proof properties of printing paper.

[0078] Example 5

[0079] Take cellulose nanocrystals, vinyl triethoxysilane, carboxymethyl cellulose and beeswax as examples:

[0080] Cellulose nanocrystals (with a diameter of 2-6 nm and a length of 100-500 nm) were prepared into 100 g of a dispersion liquid (water as a solvent) with a concentration of 3 wt%, dispersed evenly under ultrasound, adjusted to pH 10 with a 0.1 M NaOH solution, added with 2 g of vinyl triethoxysilane (190.31 g / mol), reacted for 5 h, and then washed to remove the unreacted silane coupling agent, the degree of substitution was controlled to be 0.5, and the grafted mass of vinyl triethoxysilane was 0.59 g, to obtain silane-modified nanocellulose;

[0081] Reconfigure the water suspension of silane-modified nanocellulose to have a mass fraction of 3 wt.%, and obtain 100 g of nanocellulose dispersion;

[0082] Then, 3 g of carboxymethyl cellulose was weighed and slowly added into the above 100 g of cellulose nanocrystal dispersion under stirring at room temperature, and stirred for 2 h until the carboxymethyl cellulose was completely dissolved to obtain a Janus-type nanocellulose mixed dispersion.

[0083] Then, 4 g of beeswax and 93 g of deionized water were weighed and added to the above 103 g of the mixed dispersion, so that the ratio of Janus-type cellulose nanocrystals: beeswax: water was 3:2:95, and the mixture was heated to 90°C and emulsified at 30,000 rpm for 5 minutes. After the emulsification, the mixture was cooled and the waterproof and oil-proof coating (waterproof and oil-proof agent) was obtained when the emulsion temperature dropped to room temperature.

[0084] Preparation of waterproof and oil-proof paper:

[0085] The unsized parchment paper was dried in an oven at 60°C for 5 h, and then the waterproof and oil-proof agent was applied to the surface of the paper by spin coating (double-sided coating), with a total coating amount of 15 g / m 2 The coated paper was placed in an oven at 70°C and dried for 2 hours. The waterproof and oil-proof properties of the paper were then characterized. The water contact angle of the obtained paper was 133° and the cobb60 value was 5.5 g / m 2 ,kit value is 12, air permeability is 0.08μm / Pa·s, tensile strength is 51MPa. Blank parchment water contact angle is 41°, cobb60 value is 85g / m 2 , kit value is 0, air permeability is 8.42μm / Pa·s, and tensile strength is 42MPa. This shows that the addition of waterproof and oil-proof coating improves the waterproof and oil-proof properties of parchment paper.

[0086] Example 6

[0087] Take nanocellulose, diaminopropyltriethoxysilane, hydroxypropyl cellulose and food-grade paraffin as examples:

[0088] Nanocellulose (diameter 2-5 nm, length 1-3 μm) was prepared into 100 g dispersion (water as solvent) with a concentration of 3 wt%, dispersed evenly under ultrasound, 0.1 M NaOH solution was used to adjust the pH to 8, 2.5 g of diaminopropyltriethoxysilane (225.3 g / mol) was added, reacted for 4 hours, and then washed to remove the unreacted silane coupling agent, the degree of substitution was controlled to be 0.5, and the grafting mass of diaminopropyltriethoxysilane was 0.70 g, to obtain silane-modified nanocellulose;

[0089] Reconfigure the water suspension of silane-modified nanocellulose to have a mass fraction of 3 wt.%, and obtain 100 g of nanocellulose dispersion;

[0090] Subsequently, 0.3 g of hydroxypropyl cellulose was weighed and slowly added to the above 100 g of nanocellulose dispersion under stirring at room temperature, and stirred for 2 h until the hydroxypropyl cellulose was completely dissolved to obtain a Janus-type nanocellulose mixed dispersion.

[0091] Then, 13.2 g of food-grade paraffin and 51.5 g of deionized water were weighed and added to the above 100.3 g of the mixed dispersion, so that the ratio of Janus nanocellulose: food-grade paraffin: water was 2:8:90, heated to 90°C, and emulsified at 30,000 rpm for 5 minutes. After the emulsification was completed, it was cooled, and the waterproof and oil-proof coating (waterproof and oil-proof agent) was obtained when the emulsion temperature dropped to room temperature.

[0092] Preparation of waterproof and oil-proof paper:

[0093] The unsized newsprint was dried in an oven at 60°C for 2 h, and then the waterproof and oil-proof agent was coated on the surface of the paper by knife coating (double-sided coating), with a total coating amount of 8 g / m 2 The coated paper was placed in an oven at 70°C and dried for 2 hours. The waterproof and oil-proof properties of the paper were then characterized. The water contact angle of the obtained paper was 119° and the cobb60 value was 8.9 g / m 2 , kit value is 6, air permeability is 0.18μm / Pa·s, tensile strength is 16MPa. Newsprint water contact angle is 26°, cobb60 value is 90g / m 2 , kit value is 0, air permeability is 12.4μm / Pa·s, and tensile strength is 9.8MPa. This shows that the addition of waterproof and oil-proof coating improves the waterproof and oil-proof properties of newsprint.

[0094] Comparative Example 1

[0095] Taking wood nanocellulose, palm wax and polyvinyl alcohol as examples, no oil phase substances are added.

[0096] Wood nanocellulose (lignin content of 15.7%, diameter of 2-10 nm, length of 1-3 μm) was prepared into 100 g dispersion (water as solvent) with a concentration of 3 wt %, and dispersed evenly under ultrasound.

[0097] Then, 3 g of polyvinyl alcohol was weighed and slowly added into the above 100 g of wood nanocellulose dispersion under stirring at 90° C., and stirred for 1 hour until the polyvinyl alcohol was completely dissolved; thus obtaining a nanocellulose / polyvinyl alcohol mixed dispersion.

[0098] Then, 12 g of palm wax and 14 g of deionized water were weighed and added to the above 103 g of mixed dispersion, so that the ratio of wood nanocellulose / polyvinyl alcohol mixed solution: palm wax: water was 5:10:85, heated to 90°C, and emulsified at 30,000 rpm for 5 minutes. After the emulsification was completed, it was cooled, and the waterproof and oil-proof coating (waterproof and oil-proof agent) was obtained when the emulsion temperature dropped to room temperature.

[0099] Preparation of waterproof and oil-proof paper:

[0100] The unsized kraft paper was dried in an oven at 60°C for 2 h, and then the waterproof and oil-proof agent was coated on the surface of the paper (only one side was coated, and the test side was the coated side), with a coating amount of 7 g / m 2 The coated paper was placed in an oven at 70°C and dried for 2 hours. The waterproof and oil-proof properties of the paper were then characterized. The water contact angle of the obtained paper was 100° and the cobb60 value was 19.4 g / m 2 , kit value is 10, air permeability is 0.11μm / Pa·s, tensile strength is 41MPa. The water contact angle of blank kraft paper is 60°, and the cobb60 value is 88g / m 2 , kit value is 0, air permeability is 9.67μm / Pa·s, and tensile strength is 28MPa. This indicates that the waterproof performance of kraft paper is deteriorated without adding silane coupling agent.

[0101] The oil-proof component is selected from one or more of natural polysaccharide substances and polyvinyl alcohol (polymerization degree is 1750±50, alcoholysis degree is 88-99).

[0102] Comparative Example 2

[0103] Taking nanocellulose, 3-aminopropyltriethoxysilane and ASA as examples, no natural polysaccharide substances were added.

[0104] Nanocellulose (diameter 2-5nm, length 1-3μm) was prepared into 100g dispersion (water as solvent) with a concentration of 3wt%, dispersed evenly under ultrasound, 0.1M NaOH solution was used to adjust the pH to 9, 3g of 3-aminopropyltriethoxysilane (221.37g / mol) was added, reacted for 5h, and then washed to remove the unreacted silane coupling agent, the substitution degree of nanocellulose was controlled to be 0.8, and the grafting mass of 3-aminopropyltriethoxysilane was 1.08g, to obtain silane-modified nanocellulose;

[0105] Reconfigure the water suspension of silane-modified nanocellulose to have a mass fraction of 3 wt.%, and obtain 100 g of nanocellulose dispersion;

[0106] Then, 9 g of ASA and 41 g of water were weighed and added to the above 100 g mixed dispersion so that the ratio of nanocellulose: ASA: water was 2:6:92, heated to 90°C, and emulsified at 30,000 rpm for 5 minutes. After the emulsification was completed, it was cooled and the waterproof and oil-proof coating (waterproof and oil-proof agent) was obtained when the emulsion temperature dropped to room temperature.

[0107] Preparation of waterproof and oil-proof paper:

[0108] The unsized kraft paper was dried in an oven at 60°C for 5 h, and then the waterproof and oil-proof agent was coated on the surface of the paper (only one side was coated, and the coated side was the test side), with a coating amount of 4 g / m 2 The coated paper was placed in an oven at 70°C and dried for 2 hours. The waterproof and oil-proof properties of the paper were then characterized. The water contact angle of the obtained paper was 132° and the cobb60 value was 8.3 g / m 2 , kit value is 3, air permeability is 0.27μm / Pa·s, tensile strength is 37MPa. The water contact angle of blank kraft paper is 60°, and the cobb60 value is 88g / m 2 , kit value is 0, air permeability is 9.67μm / Pa·s, and tensile strength is 28MPa. This indicates that the oil-proof performance of kraft paper becomes worse without adding natural polysaccharides.

[0109] Comparative Example 3

[0110] Example 3 was repeated (process and conditions were the same as Example 3), except that polyvinyl alcohol was added first, and then the silane coupling agent modification and oily substance were added. Specifically:

[0111] The wood nanocellulose was prepared into 100 g dispersion with a concentration of 3 wt%, and dispersed evenly under ultrasound. Subsequently, 2 g of polyvinyl alcohol was weighed and slowly added to the above 100 g nanocellulose dispersion under heating and stirring at 90°C. After the polyvinyl alcohol was completely dissolved, it was stirred for 60 minutes to obtain a wood nanocellulose / polyvinyl alcohol mixed solution.

[0112] Then, 0.1M NaOH solution was used to adjust the pH to 9, and 3g of 3-aminopropyltriethoxysilane (221.37g / mol) was added to react for 5h without washing (washing will remove polyvinyl alcohol) to obtain a wood nanocellulose mixture. Then, 16g of AKD and 79g of deionized water were weighed and added to the above 105g mixed dispersion so that the ratio of wood nanocellulose mixture: AKD: water was 4:8:88, heated to 90°C, and emulsified at 30000rpm for 5min. After the emulsification was completed, it was cooled, and the waterproof and oil-proof coating was obtained when the emulsion temperature dropped to room temperature.

[0113] Preparation of waterproof and oil-proof paper:

[0114] The unsized corrugated paper was dried in an oven at 60°C for 2 h, and then the waterproof and oil-proof agent was applied to the paper surface by spin coating (double-sided coating), with a total coating amount of 10 g / m 2 The coated paper was placed in an oven at 70°C and dried for 2 hours. The waterproof and oil-proof properties of the paper were then characterized. The water contact angle of the obtained paper was 121° and the cobb60 value was 8.6 g / m 2 ,kit value is 8, air permeability is 0.23μm / Pa·s, tensile strength is 43MPa. The water contact angle of blank corrugated paper is 52°, and the cobb60 value is 91g / m 2 , kit value is 0, air permeability is 9.44 μm / Pa·s, and tensile strength is 36 MPa. Compared with Example 3, the waterproof and oil-proof properties of the sample are deteriorated.

[0115] Comparative Example 4

[0116] Example 3 was repeated (process and conditions were the same as Example 3), except that 3 g of 3-aminopropyltriethoxysilane (221.37 g / mol) was added in the last step of forming the emulsion and then reacted without washing (washing would remove polyvinyl alcohol and AKD). Specifically:

[0117] The wood nanocellulose was prepared into 100 g dispersion with a concentration of 3 wt%, and dispersed evenly under ultrasound. Subsequently, 2 g of polyvinyl alcohol was weighed and slowly added to the above 100 g nanocellulose dispersion under heating and stirring at 90°C. After the polyvinyl alcohol was completely dissolved, it was stirred for 60 minutes to obtain a wood nanocellulose / polyvinyl alcohol mixed solution.

[0118] Then, 16 g of AKD and 79 g of deionized water were weighed and added to the above 102 g of mixed dispersion, and finally the pH was adjusted to 9 with 0.1 M NaOH solution, and 3 g of 3-aminopropyltriethoxysilane (221.37 g / mol) was added to react for 5 h without washing (washing would remove polyvinyl alcohol and AKD), so that the ratio of wood nanocellulose mixture: AKD: water was 4:8:88. The mixture was heated to 90 ° C and stirred at 30,000 rpm for 5 min. No emulsion coating was obtained.

[0119] Comparative Example 5:

[0120] Example 3 was repeated (process and conditions were the same as Example 3), except that the mass of polyvinyl alcohol was controlled to be 0.25 g, and the mass fraction relative to nanocellulose was 8.3%, and other conditions remained unchanged.

[0121] The water contact angle of the obtained paper is 123° and the cobb60 value is 8.2 g / m 2 ,kit value is 4, air permeability is 0.42μm / Pa·s, and tensile strength is 42MPa. Compared with Example 3, the waterproof and oil-proof properties of the sample are deteriorated, especially the oil-proof property.

[0122] Comparative Example 6:

[0123] Example 3 was repeated (process and conditions were the same as Example 3), except that 0.8 g of 3-aminopropyltriethoxysilane (221.37 g / mol) was added for reaction and then washed to remove unreacted silane coupling agent, the degree of substitution of nanocellulose was 0.16, and other conditions remained unchanged.

[0124] The water contact angle of the obtained paper is 108° and the cobb60 value is 12.5 g / m 2 ,kit value is 10, air permeability is 0.22μm / Pa·s, and tensile strength is 44MPa. Compared with Example 3, the waterproof and oil-proof properties of the sample are deteriorated.

[0125] Comparative Example 7:

[0126] Example 3 was repeated (process and conditions were the same as Example 3), except that wood nanocellulose (lignin content of 15.7%, diameter of 2-10 nm, length of 1-3 μm) was replaced with microcellulose (diameter of 200-500 nm, length of 3-10 μm), and other conditions remained unchanged.

[0127] The water contact angle of the obtained paper is 111° and the cobb60 value is 10.6 g / m 2 ,kit value is 7, air permeability is 0.96μm / Pa·s, and tensile strength is 41MPa. Compared with Example 3, the waterproof and oil-proof properties of the sample are slightly worse.

[0128] Comparative Example 8:

[0129] Example 3 was repeated (process and conditions were the same as Example 3), except that wood nanocellulose (lignin content of 15.7%, diameter of 2-10 nm, length of 1-3 μm) was replaced with wood microcellulose (lignin content of 15.7%, diameter of 200-1000 nm, length of 3-10 μm), and other conditions remained unchanged.

[0130] The water contact angle of the obtained paper is 118° and the cobb60 value is 11.4 g / m 2 ,kit value is 6, air permeability is 1.21μm / Pa·s, and tensile strength is 40MPa. Compared with Example 3, the waterproof and oil-proof properties of the sample are slightly worse.

[0131] Comparative Example 9:

[0132] Example 3 was repeated (the process and conditions were the same as those of Example 3), except that the water-proof and oil-proof agent was applied to the paper surface by spin coating (single-sided coating), and the coating amount was 1 g / m 2 , other conditions remain unchanged.

[0133] The water contact angle of the obtained paper is 91° and the cobb60 value is 35.3 g / m 2 ,kit value is 4, air permeability is 7.6μm / Pa·s, and tensile strength is 40MPa. Compared with Example 3, the waterproof and oil-proof properties of the sample are worse.

[0134] Table 1 Test results of water contact angle, cobb60 value, kit value, air permeability and tensile strength of waterproof and oil-proof paper of Examples 1-8

[0135]

[0136] Table 2 Test results of water contact angle, cobb60 value, kit value, air permeability and tensile strength of waterproof and oil-proof paper of comparative examples 1-7

[0137]

[0138] The results show that when Janus-type nanocellulose cannot be formed, or the added amount of silane coupling agent and natural polysaccharide material (including polyvinyl alcohol) is not within the scope of the claims, or the added amount of oil phase material and the coating amount of waterproof and oil-proof coating are not within the scope of the claims, it is impossible to obtain an environmentally friendly and economical paper material with good waterproof and oil-proof effect.

[0139] Obviously, the above embodiments of the present invention are merely examples for clearly illustrating the present invention, and are not limitations on the implementation methods of the present invention. For ordinary technicians in the relevant field, other different forms of changes or modifications can be made based on the above description. It is impossible to list all the implementation methods here. All obvious changes or modifications derived from the technical solution of the present invention are still within the protection scope of the present invention.

Claims

1. A waterproof and oil-proof environmentally friendly coating, characterized in that: It is a Pickering emulsion structure, including the following components: Pickering emulsion contains oil phase and water phase, and is an oil-in-water Pickering emulsion structure; The oil phase substance is one or more of wax (one or more of plant wax, animal wax, food-grade paraffin), alkyl ketene dimer (AKD), alkenyl succinic anhydride (ASA), and rosin; The aqueous phase material other than water in the aqueous phase is Janus-type nanocellulose, on which both the oil-proof component and the water-proof component are connected; The oil-proof component is selected from one or more of natural polysaccharide substances and polyvinyl alcohol (polymerization degree of 1750±50, alcoholysis degree of 88-99); The waterproof component is selected from one or more silane coupling agents.

2. The waterproof and oil-proof environmentally friendly coating according to claim 1, characterized in that: The silane coupling agent includes but is not limited to one or more of hexadecyltrimethoxysilane, methyltrimethoxysilane, γ-methacryloxypropyltrimethoxysilane (KH570), 3-aminopropyltriethoxysilane (KH550), diaminopropyltriethoxysilane (KH560), vinyltriethoxysilane, vinyltrimethoxysilane, etc.

3. The waterproof and oil-proof environmentally friendly coating according to claim 1, characterized in that: The natural polysaccharide material is selected from one or more of cellulose and its derivatives, chitosan, sodium alginate, starch or polyvinyl alcohol.

4. The waterproof and oil-proof environmentally friendly coating according to claim 1, characterized in that: The nanocellulose fibers are selected from one or more of nanocellulose (with a diameter of 2-10 nm and a length of 1-5 μm), cellulose nanocrystals (most of the amorphous regions of the nanocellulose are removed, and the crystalline regions are retained, with a diameter of 2-6 nm and a length of 100-500 nm), and wood nanocellulose (containing 2-25% lignin and 2-20% hemicellulose, by mass).

5. The waterproof and oil-proof environmentally friendly coating according to claim 1, characterized in that: The Janus type nanocellulose is a cellulose hydroxyl group that is first surface-modified by a silane coupling agent, and the remaining unreacted hydroxyl groups are connected to natural polysaccharide substances through hydrogen bonds; the degree of substitution of the silane coupling agent is 0.2-1 (preferably 0.4-0.9, more preferably 0.5-0.8) (the degree of substitution of cellulose refers to the amount of substances that replace the active hydroxyl groups on each D-glucose unit of cellulose, and the maximum value is 3), and the amount of natural polysaccharide substances added relative to the mass fraction of the modified nanocellulose is 10%-200% (preferably 50%-150%, more preferably 75%-125%).

6. The waterproof and oil-proof environmentally friendly coating according to claim 1 or 5, characterized in that: In the Pickering emulsion structure, the mass ratio of the dry weight of Janus nanocellulose, the dry weight of the oil phase component and water is 0.5-5:0.5-10:99-85 (preferably 2-5:2-8:96-87, more preferably 2-5:3-7.5:95-87.5).

7. A method for preparing the waterproof and oil-proof environmentally friendly coating according to any one of claims 1 to 6, characterized in that: The preparation method is a Pickering emulsion template method, and the water-in-oil type Pickering emulsion structure is formed by emulsifying the Janus type nanocellulose water phase and the oil phase components; it includes the following steps: 1) adjusting the pH of a 0.1-5wt.% nanocellulose aqueous suspension (preferably 1-5wt.%) to 8-10 (according to the selected silane coupling agent) with a NaOH solution, transferring it into a three-necked flask with stirring and reflux, adding a silane coupling agent dropwise to the three-necked flask and reacting for 4-6 hours (according to the selected silane coupling agent, adjusting the reaction time), so that the degree of substitution of the silane coupling agent is 0.2-1, and calculating the degree of substitution by weighing method (the weight gain before and after the reaction); washing with distilled water by centrifugation until neutral, and reconfiguring the mass fraction of the silane-modified nanocellulose aqueous suspension to be 0.1-1wt.% (preferably 1-5wt.%); 2) adding a certain amount of natural polysaccharide to the silane-modified nanocellulose aqueous suspension (controlling the mass ratio of natural polysaccharide to modified nanocellulose to be 10%-200% (preferably 50%-150%)), heating and stirring at 25-90° C. (preferably 60-90° C.) for 1-3 h (preferably 1.5-3 h) until the mixture is uniformly mixed to obtain a Janus-type nanocellulose aqueous suspension; 3) Adding 0.5-5 parts of Janus nanocellulose, 99-85 parts of water, and 0.5-10 parts of oil phase substance to the above suspension under heating and stirring conditions at 25-90° C. (preferably 60-90° C.), emulsifying for 5-180 min (preferably 5-60 min), and cooling to room temperature to obtain the waterproof and oil-proof environmentally friendly coating.

8. An application of the waterproof and oil-proof environmentally friendly coating according to any one of claims 1 to 6, It is applied to the surface of cellulose-based sheet materials to prepare functional cellulose-based sheet materials with hydrophobic, waterproof and oil-proof properties.

9. The use according to claim 8, characterized in that: Applying the waterproof and oil-proof environmentally friendly coating on the surface of a cellulose-based sheet material and drying it to obtain a functional cellulose-based sheet material with hydrophobic, waterproof and oil-proof properties; Cellulose-based sheet materials refer to commonly used paper, including but not limited to one or more of white board paper, white cardboard, kraft paper, kraft paper, corrugated paper, boxboard, label paper, etc.; The application amount of the waterproof and oil-proof environmentally friendly coating is 2-10 g / m 2 (Preferably 3-6g / m 2 ).

10. The use according to claim 9, characterized in that: The application method is one of dip coating, spin coating, blade coating, and coating.

Citation Information

Patent Citations

  • Water-based coating with water-proof and oil-proof performance as well as preparation method and application thereof

    CN114059386A

  • Preparation method of waterproof and oilproof barrier material and application of waterproof and oilproof barrier material in waterproof and oilproof paper

    CN117265909A

Cited By

  • Bio-based fluoride-free oil-proofing agent and preparation process thereof

    CN119531177A

  • A bio-based fluorine-free oil repellent and a preparation process thereof

    CN119531177B

  • Wet-end papermaking process for improving surface smoothness of paper

    CN120193440A