Sodium-ion battery positive electrode material synthesis device and working method thereof

Through spray granulation and multiple sets of sintering disk devices, the problems of high protective gas consumption and material adhesion during the sintering process of sodium-ion battery cathode materials are solved, achieving uniformity of the sintering environment and improving production efficiency.

CN118729762APending Publication Date: 2024-10-01CHANGDE COSPOWERS NEW ENERGY TECH CO LTD
View PDF 0 Cites 0 Cited by

Patent Information

Application Number
CN202410921213.1
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Filing Date
2024-07-10
Publication Date
2024-10-01

AI Technical Summary

Technical Problem

The sintering process of existing sodium-ion battery cathode materials consumes a large amount of protective gas and the materials are easy to bond, resulting in high production costs and poor sintering quality.

Method used

Using a device with spray granulation and multiple sets of sintering disks, the raw material solution is atomized through the spray granulation mechanism and sintered evenly on multiple sets of sintering disks to ensure a consistent sintering environment and avoid material accumulation and adhesion.

Benefits of technology

The uniformity of the sintering environment is achieved, the production cycle is shortened, the production cost is reduced, and the material utilization rate and sintering quality are improved.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN118729762A_ABST
    Figure CN118729762A_ABST
Patent Text Reader

Abstract

The invention discloses a sodium-ion battery positive electrode material synthesis device and a synthesis method thereof, and belongs to the technical field of battery production. The air outlet end of the air blower communicates with the air inlet end of the heater, and the air outlet end of the heater communicates with the drying chamber. A high-speed centrifugal atomizer is arranged at the upper end of the drying chamber, the lower end of the drying chamber is communicated with the air inlet end of a cyclone separator through a conveying pipeline, the air outlet end of the cyclone separator is communicated with the air inlet end of a centrifugal fan, and the air outlet end of the centrifugal fan is communicated with a discharging pipeline. And a discharge hole in the lower end of the cyclone separator is communicated with the sintering mechanism. According to the method, atomization is conducted firstly, then sintering is conducted, the multiple sintering discs arranged in sequence are used in the sintering process, it is ensured that the sintering environment is more uniform, and the problem that in the traditional sintering process, due to material accumulation, the difference between the internal atmosphere and the external atmosphere is large, and then the consistency of sintered products is poor is solved.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The invention relates to a sodium ion battery positive electrode material synthesis device and a working method thereof, belonging to the technical field of battery production. Background Art

[0002] In the prior art, orbital vacuum furnaces and rotary kilns are widely used in the preparation of positive electrode materials for sodium ion batteries. Due to its design characteristics, the orbital vacuum furnace has a large furnace length and space, which results in the need to consume a large amount of protective gas during the sintering process to maintain the purity of the furnace environment. This high consumption not only increases production costs, but also poses a challenge to the effective use of resources. In contrast, although the rotary kiln can reduce the consumption of protective gas to a certain extent, its internal drum structure easily causes material agglomeration during the sintering process, especially when dealing with polyanion materials, the bonding phenomenon is particularly serious. This not only affects the sintering quality of the material, but also increases the difficulty and cost of subsequent cleaning work.

[0003] Specifically, when polyanion materials are sintered in an orbital vacuum furnace, due to the uneven temperature distribution in the furnace and the influence of gas flow characteristics, the materials are easy to stick to the bottom of the sagger, forming hard agglomerates that are difficult to remove. In a rotary kiln, due to the rotation of the drum and the change of temperature in the furnace, the materials are more likely to stick to the inside of the drum, forming a continuous agglomeration layer. These agglomeration phenomena not only reduce the utilization rate of materials, but also may cause damage to sintering equipment and increase maintenance costs. Summary of the invention

[0004] In order to solve the problems existing in the background technology, the present invention provides a sodium ion battery positive electrode material synthesis device and a working method thereof.

[0005] To achieve the above-mentioned purpose, the present invention adopts the following technical scheme: a sodium ion battery positive electrode material synthesis device, comprising a spray granulation mechanism and a sintering mechanism; the spray granulation mechanism comprises a blower, a heater, a high-speed centrifugal atomizer, a drying chamber, a cyclone separator and a centrifugal fan; the air outlet end of the blower is connected to the air inlet end of the heater, and the air outlet end of the heater is connected to the drying chamber; the upper end of the drying chamber is provided with a high-speed centrifugal atomizer, the lower end of the drying chamber is connected to the air inlet end of the cyclone separator through a conveying pipeline, the air outlet end of the cyclone separator is connected to the air inlet end of the centrifugal fan, and the air outlet end of the centrifugal fan is connected to the discharge pipeline; the discharge port at the lower end of the cyclone separator is connected to the sintering mechanism.

[0006] The air inlet end of the blower is provided with a dust filter.

[0007] A circulating cooling pipeline is arranged on the outer side of the high-speed centrifugal atomizer.

[0008] The side wall of the drying chamber is provided with an observation window.

[0009] The discharge port of the cyclone separator is provided with a bottom screen.

[0010] The discharge port of the cyclone separator is provided with a check valve.

[0011] An exhaust dust collecting bag is arranged between the cyclone separator and the centrifugal fan.

[0012] The sintering mechanism includes a central transmission shaft, a heat-insulating shell, a collecting bucket and a sintering unit; a feed port is provided at the upper end of the heat-insulating shell, and the feed port is connected with the discharge port; the lower end of the heat-insulating shell is connected with the collecting bucket, and the side wall of the heat-insulating shell is provided with an air inlet and an air outlet; a vertically arranged central transmission shaft is rotatably arranged in the heat-insulating shell, and a plurality of groups of sintering units are arranged from top to bottom on the outer side of the central transmission shaft, the feed end of the sintering unit located at the uppermost end is arranged in cooperation with the feed port, and the discharge end of the sintering unit located at the lowermost end is arranged in cooperation with the collecting bucket.

[0013] Each group of the sintering units includes an upper sintering disk, a lower sintering disk, an upper roller brush and a lower roller brush. The upper sintering disk and the lower sintering disk are coaxially and parallelly rotated and are mounted on the outside of the central transmission shaft. The upper sintering disk and the lower sintering disk are fixedly connected to the insulation shell. The diameter of the upper sintering disk is smaller than the diameter of the lower sintering disk. The upper sintering disk is a convex disk structure in the middle. The upper end of the upper sintering disk is rollingly fitted and connected to multiple upper roller brushes, and each of the upper roller brushes is a spiral structure with a decreasing diameter from the inside to the outside; the lower sintering disk is a concave disk structure in the middle. The lower sintering disk is rollingly fitted and connected to multiple lower roller brushes, and each of the lower roller brushes is a spiral structure with a decreasing diameter from the outside to the inside; a plurality of feeding holes are provided in the middle of the lower sintering disk; the inner end of each upper roller brush and each lower roller brush is rotationally connected to the central transmission shaft.

[0014] A working method of a sodium ion battery positive electrode material synthesis device of the present invention is characterized in that the method comprises the following steps:

[0015] S1: Air is sucked into the heater through the blower, the raw material solution is prepared, and the protective gas is introduced into the insulation shell;

[0016] S2: air enters the drying chamber through the heater;

[0017] S3: The raw material solution enters the high-speed centrifugal atomizer for atomization;

[0018] S4: The atomized raw material is dried into powder by hot air in the drying chamber;

[0019] S5: The dried powder is sucked into the cyclone separator through the conveying pipeline under the action of the centrifugal fan;

[0020] S6: The dried powder falls to the middle of the upper sintering plate of the uppermost sintering unit;

[0021] S7: The central transmission shaft rotates to drive the upper roller brush and the lower roller brush to revolve. At the same time, since the upper roller brush is in contact with the upper sintering plate, the upper roller brush revolves on the upper sintering plate while rotating, driving the powder to move out of the upper sintering plate until the powder falls onto the lower sintering plate.

[0022] S8: As the lower roller brush is in contact with the lower sintering plate, the lower roller brush rotates while revolving on the lower sintering plate, driving the powder to move inward to the discharge hole and then fall to the middle of the upper sintering plate of the next sintering unit;

[0023] S9: After the powder is sintered by multiple groups of sintering units, it falls into a collecting bucket;

[0024] S10: The collecting hopper transfers out the powder.

[0025] Compared with the prior art, the present invention has the following beneficial effects:

[0026] 1. The present invention performs atomization before sintering, and uses a plurality of sintering disks arranged in sequence during the sintering process, thereby ensuring a more uniform sintering environment and solving the problem of large difference in internal and external atmospheres caused by material accumulation in the traditional sintering process, which in turn causes poor consistency of the sintered products.

[0027] 2. The present invention realizes that the precursor after spray granulation can be seamlessly connected to the sintering mechanism, realizes a continuous operation mode, eliminates the cumbersome transportation process, shortens the production cycle, improves production efficiency, and reduces production costs. BRIEF DESCRIPTION OF THE DRAWINGS

[0028] Figure 1 It is a schematic diagram of the structure of the synthesis device of the present invention;

[0029] Figure 2 It is a schematic structural diagram of a sintering mechanism of a synthesis device of the present invention;

[0030] Figure 3 is a charge-discharge curve diagram of sodium iron pyrophosphate prepared in Example 1;

[0031] Figure 4 is a circulation curve diagram of sodium ferric pyrophosphate prepared in Example 1;

[0032] Figure 5 This is the charge and discharge curve of sodium vanadium phosphate prepared in Example 2. DETAILED DESCRIPTION

[0033] The technical solution of the present invention will be clearly and completely described below in conjunction with the drawings in the embodiments of the present invention. Obviously, the described embodiments are only part of the embodiments of the invention, rather than all of the embodiments. Based on the embodiments of the present invention, all other embodiments obtained by ordinary technicians in this field without making creative work are within the scope of protection of the present invention.

[0034] A sodium ion battery positive electrode material synthesis device comprises a spray granulation mechanism 100 and a sintering mechanism 200; the spray granulation mechanism 100 comprises a blower 102, a heater 103, a high-speed centrifugal atomizer 108, a drying chamber 109, a cyclone separator 111 and a centrifugal fan 113; the air outlet end of the blower 102 is connected to the air inlet end of the heater 103 of the resistance wire, and the air outlet end of the heater 103 is connected to the drying chamber 109 through an air supply pipe 104; A high-speed centrifugal atomizer 108 is provided at the upper end of the drying chamber 109, and a feed port 107 is provided at the upper end of the high-speed centrifugal atomizer 108; the lower end of the drying chamber 109 is connected to the air inlet end of the cyclone separator 111 through a conveying pipe, the air outlet end of the cyclone separator 111 is connected to the air inlet end of the centrifugal fan 113, and the air outlet end of the centrifugal fan 113 is connected to the exhaust pipe 114; the discharge port 117 at the lower end of the cyclone separator 111 is connected to the sintering mechanism 200.

[0035] A dust filter 101 is provided at the air inlet end of the blower 102 .

[0036] A circulating cooling pipe is provided on the outside of the high-speed centrifugal atomizer 108. The circulating cooling pipe pumps cooling water into the cooling pipe through the cold water inlet 105, and the cooling pipe pumps cooling water out through the cold water outlet 106 to cool the high-speed centrifugal atomizer 108 and prevent the electrode from burning due to excessive temperature.

[0037] The side wall of the drying chamber 109 is provided with an observation window 110. The observation window 110 facilitates real-time monitoring of the drying process.

[0038] The discharge port 117 of the cyclone separator 111 is provided with a bottom screen 116 .

[0039] A check valve 115 is provided at the discharge port 117 of the cyclone separator 111 .

[0040] An exhaust dust bag 112 is provided between the cyclone separator 111 and the centrifugal fan 113 . The exhaust dust bag 112 can collect fine dust in the dried exhaust gas to prevent dust pollution. The exhaust gas after dust removal is discharged from the exhaust pipe 114 through the centrifugal fan 113 .

[0041] The sintering mechanism 200 includes a central transmission shaft 205, a heat-insulating shell 207, a collecting hopper 208 and a sintering unit; the upper end of the heat-insulating shell 207 is provided with a feed inlet 209, and the feed inlet 209 is connected to the discharge port 117; the lower end of the heat-insulating shell 207 is connected to the collecting hopper 208, and the side wall of the heat-insulating shell 207 is provided with an air inlet 201 and an air outlet 202; the air inlet 201 is a protective gas inlet channel, and the air outlet 202 is a sintering exhaust gas discharge channel. 7. Ensure the temperature stability in the sintering mechanism 200; a vertically arranged central transmission shaft 205 is rotatably arranged in the heat-insulating shell 207, and the central transmission shaft 205 is driven to rotate by a motor. This is the prior art and will not be described in detail. The motor is fixed on the heat-insulating shell 207; a plurality of groups of sintering units are evenly distributed on the outer side of the central transmission shaft 205 from top to bottom, and the feed end of the sintering unit at the uppermost end is coordinated with the feed port 209, and the discharge end of the sintering unit at the lowermost end is coordinated with the collecting bucket 208.

[0042] Each group of the sintering units includes an upper sintering disk 203, a lower sintering disk 210, an upper roller brush 206 and a lower roller brush 211. The upper sintering disk 203 and the lower sintering disk 210 are coaxially arranged and rotatably mounted on the outer side of the central transmission shaft 205 through bearings. The interval between the upper sintering disk 203 and the lower sintering disk 210 needs to be small enough to ensure that all the powder can fall into the lower sintering disk 210. The upper sintering disk 203 and the lower sintering disk 210 are both fixedly connected to the insulation shell 207. The diameter of the upper sintering disk 203 is smaller than the diameter of the lower sintering disk 210. The upper sintering disk 203 is a convex disk structure in the middle. The upper end of the upper sintering disk 203 is rollingly fitted and connected with multiple upper roller brushes 206 evenly arranged along its circumference. Each of the upper roller brushes 206 is a spiral structure with a decreasing diameter from the inside to the outside; the lower sintering disk 210 is a concave disk structure in the middle. The lower sintering disk 210 is rollingly fitted and connected with multiple lower roller brushes 211 evenly arranged along its circumference. Each of the lower roller brushes 211 is a spiral structure with a decreasing diameter from the outside to the inside; the middle part of the lower sintering disk 210 is evenly distributed along its circumference with multiple feeding holes 204 running through its thickness direction; the inner end of each upper roller brush 206 and each lower roller brush 211 is rotatably connected to the central transmission shaft 205 through a bearing.

[0043] The heating temperature range of the heater 103 is 50-400°C.

[0044] The high-speed centrifugal atomizer 108 has a rotation frequency ranging from 50 Hz to 450 Hz.

[0045] The sintering disk is made of graphite, alumina, ceramic or other high temperature resistant materials. Each sintering disk can independently control the heating temperature, and the heating range is 200-1200°C.

[0046] The protective gas entering the sintering mechanism through the gas inlet 201 may be nitrogen, argon, helium, a hydrogen-argon mixture, or other inert gases.

[0047] The bottom screen 116 can be replaced with screens of different mesh sizes to prevent foreign particles from entering the sintering mechanism.

[0048] A working method of a sodium ion battery positive electrode material synthesis device of the present invention is characterized in that the method comprises the following steps:

[0049] S1: air is sucked into the heater 103 through the blower 102 to heat the air; raw material solution is prepared and protective gas is introduced into the heat-insulating shell 207;

[0050] S2: air passes through the heater 103 and the air delivery duct 104 into the drying chamber 109;

[0051] S3: The raw material solution enters the high-speed centrifugal atomizer 108 from the feed inlet 107 for atomization;

[0052] The sodium source, phosphorus source, iron source or vanadium source, carbon source, dopant, etc. required for synthesizing the positive electrode material of the sodium ion battery are dispersed in a solvent, and the dispersed solution is pumped into the spray granulation mechanism 100 which has been heated to a preset temperature through the feed port 107 using a peristaltic pump;

[0053] The sodium source is an inorganic salt or organic sodium salt containing sodium, such as sodium carbonate, sodium hydroxide, sodium pyrophosphate, sodium dihydrogen phosphate, and disodium hydrogen phosphate.

[0054] The phosphorus source is phosphate such as diammonium phosphate, diammonium hydrogen phosphate, ammonium phosphate, or phosphoric acid.

[0055] The iron source is iron phosphate, iron nitrate, iron powder, ferrous oxalate, rust and other iron-containing oxides or salts; the vanadium source is vanadium pentoxide, ammonium vanadate and other vanadium-containing oxides or salts.

[0056] The carbon source is one or more organic substances such as graphene oxide, carbon nanotubes, carbon quantum dots, citric acid, glucose, starch, oleic acid, ethylene glycol, and n-propanol.

[0057] The dopant includes one or more of manganese-containing oxides and salts thereof, aluminum-containing oxides and salts thereof, magnesium-containing oxides and salts thereof, sodium fluoride, and the like.

[0058] S4: The atomized raw material is dried into powder by hot air in the drying chamber 109;

[0059] S5: The dried powder is sucked into the cyclone separator 111 through the conveying pipeline under the action of the centrifugal fan 113, and the completely dried powder settles on the bottom screen 116. The powder collected on the bottom screen 116 is the precursor powder;

[0060] S6: After the check valve 115 is opened, the dried powder falls to the middle of the upper sintering disk 203 of the uppermost sintering unit through the discharge port 117 and the feed port 209, and the precursor powder is heated and sintered using the sintering disk under a protective atmosphere;

[0061] S7: The central transmission shaft 205 rotates to drive the upper roller brush 206 and the lower roller brush 211 to revolve. At the same time, since the upper roller brush 206 is in contact with the upper sintering disk 203, the upper roller brush 206 revolves on the upper sintering disk 203 and rotates on itself, driving the powder to move out of the upper sintering disk 203 until the powder falls onto the lower sintering disk 210.

[0062] S8: As the lower roller brush 211 is in contact with the lower sintering disk 210, the lower roller brush 211 rotates while revolving on the lower sintering disk 210, driving the powder to move inward to the discharge hole 204 and then fall to the middle of the upper sintering disk 203 of the next sintering unit; the rotation speed of the central transmission shaft 205 is controlled to make the precursor powder flow through the sintering disks of different temperatures in sequence at a certain rate;

[0063] The spray drying atomization frequency of the polyanion compound sodium positive electrode material is 50Hz-400Hz, the injection port temperature is 80-200°C; the sintering temperature is 200-950°C, the heating rate is 1-5°C / min, and the sintering time is 2h-20h, wherein the sintering time is controlled by the number of sintering disk layers and the rotation speed of the roller brush.

[0064] The amount of the dopant is 0wt%-10wt%.

[0065] S9: After the powder is sintered by multiple groups of sintering units, it falls into the collecting bucket 208 and is cooled to obtain a polyanion compound sodium positive electrode material;

[0066] S10: The collecting hopper 208 transfers out the powder.

[0067] Embodiment 1:

[0068] S1: Weigh ferrous oxalate, sodium pyrophosphate, ammonium dihydrogen phosphate, and citric acid according to the stoichiometric ratio, add them into water, stir, mix and disperse them, and prepare a raw material mixed solution;

[0069] S2: Turn on the blower 102, the heater 103 and the centrifugal fan 113,

[0070] S3: Introduce cooling water and adjust the speed of high-speed centrifugal atomizer 108 to 380Hz.

[0071] S4: pumping the raw material mixed solution into the spray granulation mechanism 100 through a peristaltic pump while stirring at an inlet air temperature of 150°C;

[0072] S5: a total of 11 sintering units are loaded into the sintering mechanism 200, the temperature of the first and second sintering disks is adjusted to 150°C, the temperature of the third to sixth sintering disks is adjusted to be 50°C higher than the previous sintering disk, that is, the temperature of the sixth sintering disk is 350°C, the temperature of the seventh to ninth sintering disks are all 350°C, the temperature of the tenth to twelfth sintering disks is 50°C higher than the previous sintering disk, that is, the temperature of the twelfth sintering disk is 500°C, the temperature of the thirteenth to eighteenth sintering disks are all 500°C, and the heating of the nineteenth to twenty-second sintering disks is turned off, that is, used for cooling;

[0073] S6: introducing nitrogen;

[0074] S7: adjusting the rotation speed of the central transmission shaft 205 so that the powder flows through a single sintering disk for 20 minutes, and the powder obtained from the collecting hopper 208 after 7 hours is carbon-coated sodium ferric pyrophosphate.

[0075] Embodiment 2:

[0076] S1: Weigh vanadium pentoxide, sodium dihydrogen phosphate, ammonium dihydrogen phosphate, and citric acid according to the stoichiometric ratio, add 30% ethanol aqueous solution, stir and dissolve, and prepare a raw material mixed solution;

[0077] S2: Turn on the blower 102, the heater 103 and the centrifugal fan 113,

[0078] S3: Introduce cooling water and adjust the speed of high-speed centrifugal atomizer 108 to 300Hz.

[0079] S4: pumping the raw material mixed solution into the spray granulation mechanism 100 through a peristaltic pump while stirring at an inlet air temperature of 130°C;

[0080] S5: A total of 15 sintering units are loaded into the sintering mechanism 200, and the temperature of the first and second sintering disks is adjusted to 150°C. The temperature of the third to thirteenth sintering disks is increased by 50°C compared with the previous sintering disk, that is, the temperature of the thirteenth sintering disk is 700°C, the temperature of the fourteenth to twenty-fifth sintering disks is 700°C, and the heating of the twenty-sixth to thirtieth sintering disks is turned off, that is, used for cooling;

[0081] S6: introducing helium;

[0082] S7: adjusting the rotation speed of the central transmission shaft 205 so that the powder flows through a single sintering disk for 20 minutes. Then, the powder obtained from the collecting hopper 208 after 10 hours is carbon-coated sodium vanadium phosphate.

[0083] It will be apparent to those skilled in the art that the invention is not limited to the details of the exemplary embodiments described above and that the invention can be implemented in other forms without departing from the spirit or essential features of the invention. Therefore, the embodiments should be considered in all respects as exemplary and non-limiting, and the scope of the invention is defined by the appended claims rather than the foregoing description, and it is intended that all variations within the meaning and range of equivalents of the claims be included in the invention. Any reference numeral in a claim should not be considered as limiting the claim to which it relates.

[0084] In addition, it should be understood that although the present specification is described according to implementation modes, not every implementation mode contains only one independent technical solution. This description of the specification is only for the sake of clarity. Those skilled in the art should regard the specification as a whole. The technical solutions in each embodiment may also be appropriately combined to form other implementation modes that can be understood by those skilled in the art.

Claims

1. A sodium ion battery cathode material synthesis device, Features: The invention comprises a spray granulation mechanism (100) and a sintering mechanism (200); the spray granulation mechanism (100) comprises a blower (102), a heater (103), a high-speed centrifugal atomizer (108), a drying chamber (109), a cyclone separator (111) and a centrifugal fan (113); the air outlet end of the blower (102) is connected to the air inlet end of the heater (103), and the air outlet end of the heater (103) is connected to the drying chamber (109); A high-speed centrifugal atomizer (108) is provided at the upper end of the drying chamber (109); the lower end of the drying chamber (109) is connected to the air inlet end of a cyclone separator (111) through a conveying pipeline; the air outlet end of the cyclone separator (111) is connected to the air inlet end of a centrifugal fan (113); the air outlet end of the centrifugal fan (113) is connected to a discharge pipeline (114); and the discharge port (117) at the lower end of the cyclone separator (111) is connected to the sintering mechanism (200).

2. A sodium ion battery positive electrode material synthesis device according to claim 1, Features: The air inlet end of the blower (102) is provided with a dust filter (101).

3. A sodium ion battery positive electrode material synthesis device according to claim 1, Features: A circulating cooling pipeline is provided on the outer side of the high-speed centrifugal atomizer (108).

4. A sodium ion battery positive electrode material synthesis device according to claim 1, Features: The side wall of the drying chamber (109) is provided with an observation window (110).

5. A sodium ion battery positive electrode material synthesis device according to claim 1 or 4, Features: The discharge port (117) of the cyclone separator (111) is provided with a bottom screen (116).

6. A sodium ion battery positive electrode material synthesis device according to claim 5, Features: The discharge port (117) of the cyclone separator (111) is provided with a check valve (115).

7. A sodium ion battery positive electrode material synthesis device according to claim 6, Features: An exhaust dust collecting bag (112) is provided between the cyclone separator (111) and the centrifugal fan (113).

8. A sodium ion battery positive electrode material synthesis device according to claim 6 or 7, Features: The sintering mechanism (200) comprises a central transmission shaft (205), a heat-insulating shell (207), a collecting hopper (208) and a sintering unit; the upper end of the heat-insulating shell (207) is provided with a material inlet (209), and the material inlet (209) is connected to a material outlet (117); the lower end of the heat-insulating shell (207) is connected to a collecting hopper (208), and the side wall of the heat-insulating shell (207) is provided with an air inlet (201) and an air outlet (202); a vertically arranged central transmission shaft (205) is rotatably arranged inside the heat-insulating shell (207), and multiple groups of sintering units are arranged from top to bottom on the outer side of the central transmission shaft (205), the material inlet end of the sintering unit located at the uppermost end is arranged in cooperation with the material inlet (209), and the material outlet end of the sintering unit located at the lowermost end is arranged in cooperation with the collecting hopper (208).

9. A sodium ion battery positive electrode material synthesis device according to claim 8, Features: Each group of the sintering units comprises an upper sintering disk (203), a lower sintering disk (210), an upper roller brush (206) and a lower roller brush (211); the upper sintering disk (203) and the lower sintering disk (210) are coaxially rotated in parallel and are sleeved on the outside of the central transmission shaft (205); the upper sintering disk (203) and the lower sintering disk (210) are both fixedly connected to the heat-insulating shell (207); the diameter of the upper sintering disk (203) is smaller than the diameter of the lower sintering disk (210); the upper sintering disk (203) is a convex disc structure in the middle; the upper end of the upper sintering disk (203) is connected to a plurality of The upper roller brushes (206) are all connected by rolling fit, and each of the upper roller brushes (206) is a spiral structure with a diameter decreasing from the inside to the outside; the lower sintering disk (210) is a concave disc structure in the middle, and the lower sintering disk (210) and the plurality of lower roller brushes (211) are all connected by rolling fit, and each of the lower roller brushes (211) is a spiral structure with a diameter decreasing from the outside to the inside; a plurality of material discharge holes (204) are provided in the middle of the lower sintering disk (210); the inner ends of each upper roller brush (206) and each lower roller brush (211) are rotatably connected to the central transmission shaft (205).

10. A method for operating the sodium ion battery cathode material synthesis device according to any one of claims 1 to 9, Features: The method comprises the following steps: S1: air is sucked into the heater (103) through the blower (102), the raw material solution is prepared, and the protective gas is introduced into the heat-insulating shell (207); S2: air passes through the heater (103) and enters the drying chamber (109); S3: the raw material solution enters the high-speed centrifugal atomizer (108) for atomization; S4: the atomized raw material is dried into powder by hot air in the drying chamber (109); S5: The dried powder is sucked into the cyclone separator (111) through the conveying pipeline under the action of the centrifugal fan (113); S6: the dried powder falls to the middle of the upper sintering plate (203) of the uppermost sintering unit; S7: The central transmission shaft (205) rotates to drive the upper roller brush (206) and the lower roller brush (211) to revolve. At the same time, since the upper roller brush (206) is in contact with the upper sintering disk (203), the upper roller brush (206) revolves on the upper sintering disk (203) and rotates on its own, driving the powder to move outside the upper sintering disk (203) until the powder falls onto the lower sintering disk (210); S8: As the lower roller brush (211) is in contact with the lower sintering disk (210), the lower roller brush (211) revolves on the lower sintering disk (210) and rotates on its own, driving the powder to move inward to the discharge hole (204) and then fall to the middle of the upper sintering disk (203) of the next sintering unit; S9: After the powder is sintered by multiple groups of sintering units, it falls into a collecting bucket (208); S10: The collecting hopper (208) transfers out the powder.