Preparation method of transmission electron microscope sample with internal defects

By filling the internal defects of the sample with ion beam deposition of metallic tungsten, it solves the problem of damage and misjudgment in the preparation and thinning process of layered or porous material samples in the existing technology, and achieves better transmission electron microscope observation effects.

CN118731067APending Publication Date: 2024-10-01TREND TECHNOLOGY(XIAMEN) INC
View PDF 0 Cites 2 Cited by

Patent Information

Application Number
CN202310339668.8
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Filing Date
2023-03-31
Publication Date
2024-10-01

AI Technical Summary

Technical Problem

It is difficult for the existing technology to effectively fill samples with irregular edge defects, such as samples with delaminated or porous materials, resulting in the sample not being completely removed during the model preparation process, and causing damage and misjudgment of analysis results during the thinning process.

Method used

Ion beam deposited metal tungsten is used as a protective layer. By adjusting the sample angle and ion beam current density, the internal defects of the sample are gradually filled, forming a dense block structure to protect the delamination interface and the surrounding area of ​​the hole, and reduce damage during the thinning process.

Benefits of technology

The complete removal of the sample during the preparation process and the reduction of damage during the thinning process are achieved, and the accuracy and effect of transmission electron microscopy observation are improved.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN118731067A_ABST
    Figure CN118731067A_ABST
Patent Text Reader

Abstract

The invention provides a preparation method of a transmission electron microscope sample with internal defects, which comprises the following steps: positioning the sample to enable the surface of the sample to be vertical to an ion beam; etching the periphery of the target area of the sample by using an ion beam with a beam current of 60 pA to 9.3 nA so as to form an observation main surface and an observation back surface of the sample; inspecting the sample, and confirming the internal defect condition of the sample; adjusting the sample, enabling the sample to tilt from the positioning position by 0-10 degrees, and then performing deposition with tungsten for the first time by using an ion beam with the beam current of 10-200pA so as to cover and observe the main surface; thinning the observation main surface of the sample, viewing the observation main surface, and if the internal defect of the target area of the sample is not substantially filled with tungsten, depositing with tungsten again until the internal defect of the target area of the sample is substantially filled with tungsten to form a compact blocky structure; and thinning the sample in a direction from the observation back surface to the observation main surface. The internal defect structure of the sample is filled with tungsten, so that the sample is fixed, and a layered or hole area is protected in the thinning process.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The invention relates to the technical field of a method for preparing a transmission electron microscope sample, in particular to a method for preparing a transmission electron microscope sample with layered or porous materials. Background Art

[0002] Before observing the sample structure with a transmission electron microscope (TEM), the target sample cross section may be delaminated or have holes. During the sample model preparation and sample thinning process, the sample may be unable to be removed or damaged during thinning, resulting in problems in observing the delaminated area or the area near the hole.

[0003] CN105200394A provides a method for forming a TEM sample lamella with uniform deposition using a focused ion beam, comprising: directing a focused ion beam toward a workpiece surface at an angle greater than 30 degrees from the surface normal, with charged particles having a landing energy of 10 kiloelectronvolts (keV) or less; providing a carbon precursor gas at the impact point of the charged particle beam, the carbon precursor gas decomposing in the presence of the ion beam to deposit carbon on the workpiece; and directing the focused ion beam toward the deposited material on the workpiece to remove material from both sides of the region of interest, thereby retaining a thin lamella containing the region of interest, the deposited carbon protecting the thin lamella during formation. The case discloses using carbon as a material for a TEM sample protective layer.

[0004] CN103808540A discloses a method for making a transmission electron microscope sample, which includes: providing an initial transmission electron microscope sample by cutting a wafer; depositing a protective layer on the surface of the initial TEM sample according to the different material contrasts of the TEM sample observation area, and the specific method is: depositing a carbon or silicon oxide protective layer on the surface of the sample material with deep contrast, and depositing a platinum or tungsten protective layer on the surface of the sample material with shallow contrast. This case is mainly a sample of a gold oxide semi-field effect transistor (MOSFET), which has a uniform and dense texture, and the protective layer is deposited and filled from the top of the through hole to the bottom. In addition, the purpose of selecting carbon, silicon oxide, or platinum, tungsten as a protective layer in this case is to solve the problem that in the prior art, only a unified protective layer is deposited on the surface of the sample. If the contrast of the protective layer is similar to the material contrast of the structure to be observed, a ghosting phenomenon will occur, and it will not be possible to distinguish the judgment of the structure morphology and the measurement of the size.

[0005] However, the conventional technology cannot effectively fill samples with irregular edge defects, such as samples with layered or porous materials, which results in the sample being unable to be completely removed during the model preparation process, and the sample being damaged during the thinning process, leading to misjudgment of the analysis results. Therefore, the existing technology needs to be improved. Summary of the invention

[0006] In order to solve the above-mentioned problems in the sample preparation process with layered or porous materials, the purpose of the present invention is to provide a method of using ion beam deposition of metal tungsten as a protective layer. Due to its slow deposition rate, the protective layer formation process is dense, so that the sample with layered or porous materials can be fully filled with the protective layer. Finally, the sample can be completely taken out during the preparation of the target model, and the layered interface or the surrounding area of ​​the hole is protected during the thinning process, reducing the damage to the sample during the thinning process and the misjudgment of the analysis results, so as to achieve a better TEM observation effect.

[0007] The technical solution adopted by the present invention is:

[0008] One embodiment of the present invention provides a method for preparing a transmission electron microscope sample with internal defects, comprising: positioning the sample so that the surface of the sample is perpendicular to the ion beam and enters the positioning position; etching the periphery of the target area of ​​the sample with an ion beam having a beam current of 60 picoamperes (pA) to 9.3 nanoamperes (nA) to form an observation main surface and an observation back surface of the sample relative to the observation main surface; inspecting the sample to confirm the internal defect of the sample; performing a first deposition: adjusting the sample so that the sample is tilted 0° to 10° from the positioning position (that is, firstly making the surface of the sample enter a positioning position at an angle of 90° to the ion beam, and then tilting from the positioning position to the back surface of the sample); The sample is rotated by 0° to 10° so that the sample surface and the ion beam are finally at 90° to 100°. Then, the first deposition is performed with an ion beam having a beam current of 10 picoamperes (pA) to 200 pA, and tungsten is deposited to cover the main observation surface. Deposition is performed again: the main observation surface of the sample is thinned, and the main observation surface is inspected. If the internal defects in the target area of ​​the sample are still not substantially filled with tungsten, tungsten is deposited again until the internal defects in the target area of ​​the sample are substantially filled with tungsten to form a dense block structure. The sample is thinned to between 50 nanometers (nm) and 100 nm in a manner parallel to the main observation surface in the direction from the back side of the observation surface to the main observation surface.

[0009] In some embodiments, the internal defects include layered structures or hole structures, wherein the edges of the layered structures or hole structures are irregular.

[0010] In some embodiments, in the first deposition step, the sample is adjusted by tilting the sample from the positioning position by 0° to 6°; preferably, the sample may be tilted by 2° to 5°.

[0011] In some embodiments, in the first deposition step, the beam current is an ion beam of 10 pA to 120 pA, preferably, 10 pA to 90 pA, preferably, 10 pA to 40 pA.

[0012] In some embodiments, in the first deposition step, the voltage may be 15-30 keV.

[0013] In some embodiments, in the first deposition step, the voltage may be 8 keV.

[0014] In some embodiments, in the step of re-deposition, the ion beam generated by a focused ion beam system to thin the observation main surface of the sample is sequentially thinned with beam currents of 0.79nA, 0.43nA, 0.23nA, and 80pA, and tilted by ±0.7° to ±3° to symmetrically thin the sample front and back until the thickness is 200nm to 300nm.

[0015] In some embodiments, the ion beam is generated by a focused ion beam (FIB) system.

[0016] In some embodiments, the material of the sample comprises a nano coating, a ceramic or a metal. The nano coating may be a coating having optical properties. The material of the sample comprises an electronic component of an optical film.

[0017] In some embodiments, when the material of the sample is a nano-coating or a ceramic, the step of positioning the sample comprises plating the surface of the sample with gold.

[0018] In some embodiments, the material of the sample is an electronic component having an optical property surface through lamination, coating, or film plating. The optical property surface may be a surface coated with an optical film. The optical film may be a polymer film of a multilayer composite material. The polymer film of the multilayer composite material may be an anti-reflection film, an anti-glare film, a polarizing film, etc.

[0019] In some embodiments, during the re-deposition step, if the internal defects in the target area of ​​the sample are still not substantially filled with tungsten, tungsten is deposited again, including depositing tungsten with the ion beam at a voltage of 8 keV and a beam current of 15 pA to 1.2 nA.

[0020] In some embodiments, if the internal defects of the target region of the sample are still not substantially filled with tungsten during the step of performing the deposition again, the step comprises depositing tungsten with the ion beam having a voltage of 5 keV and a beam current of 15 pA to 1.2 nA.

[0021] In some embodiments, the first deposition step includes tilting the sample from the positioning position by 0° to 10°, and then depositing tungsten using an ion beam with a beam current of 10 to 200 pA and a voltage of 15 to 30 keV.

[0022] In some embodiments, the first deposition step includes tilting the sample from the positioning position by 0° to 5°, and then depositing tungsten with an ion beam having a beam current of 10 to 200 pA and a voltage of 8 keV.

[0023] In some embodiments, if the internal defects of the target region of the sample are still not substantially filled with tungsten, the step of performing deposition again includes depositing tungsten with an ion beam having a voltage of 8 keV and a beam current of 15 pA to 1.2 nA.

[0024] In some embodiments, in the step of re-depositing, if the internal defects of the target area of ​​the sample are still not substantially filled with tungsten, deposition is performed again, including depositing tungsten with an ion beam having a beam current of 66 pA, and the thickness of the sample is not less than 200 nm. Preferably, the thickness of the sample is between 200 nm and 550 nm. Preferably, the thickness of the sample is between 200 nm and 300 nm.

[0025] In some embodiments, during the step of re-deposition, if the internal defects in the target area of ​​the sample are still not substantially filled with tungsten, deposition is performed again until the internal defects in the target area of ​​the sample are substantially filled with tungsten, which means that at least 80% of the internal defects are filled with tungsten; preferably, at least 85% of the internal defects are filled with tungsten; more preferably, at least 90% of the internal defects are filled with tungsten.

[0026] In some embodiments, if the internal defects of the target region of the sample are still not substantially filled with tungsten, the step of performing deposition again includes depositing tungsten with an ion beam having a voltage of 5 keV and a beam current of 15 pA to 1.2 nA. BRIEF DESCRIPTION OF THE DRAWINGS

[0027] Figure 1 is a flow chart of a method for preparing a transmission electron microscope sample with internal defects according to some embodiments of the present invention;

[0028] Figure 2 is a top view of a sample of some embodiments of the present invention after front and rear ion machining to form a groove;

[0029] Figure 3A and Figure 3B is a side view of a sample with a layered structure according to some embodiments of the present invention;

[0030] Figure 4A and Figure 4Bis a side view of a sample with a hole structure according to some embodiments of the present invention;

[0031] Figure 5A and Figure 5B is a side view of a sample having a layered structure filled with metal according to some embodiments of the present invention;

[0032] Fig. 6A and Figure 6B is a side view of a sample having a hole structure filled with metal according to some embodiments of the present invention;

[0033] Figure 7 is a top view of a process of truncating a bottom and a side of a target area according to some embodiments of the present invention;

[0034] Figure 8 is a top view of a process of truncating the other side of a target area according to some embodiments of the present invention;

[0035] Fig. 9 is a side view of fixing a target model on a supporting copper sheet according to some embodiments of the present invention;

[0036] Fig. 10A and Fig. 10B is a side view of a thinned target model (a non-observation target area at a layered position) according to some embodiments of the present invention;

[0037] Fig.11 is a side view of a thinned target model (the layered position is the observation target area) according to some embodiments of the present invention;

[0038] Fig. 12A and Fig. 12B is a side view of a target model after thinning (hole structures are all filled with metal) according to some embodiments of the present invention;

[0039] Fig.13A and Fig. 13B is a side view of a thinned target model (part of the holes are not filled with metal) according to some embodiments of the present invention. DETAILED DESCRIPTION

[0040] In order to make the description of the present invention more detailed and complete, the following is an illustrative description of the implementation and specific embodiments of the present invention, but this is not the only form of implementing or using the specific embodiments of the present invention. The various embodiments of the invention described below can be combined or replaced with each other in a beneficial situation, and other embodiments can be added to one embodiment without further recording or explanation. In the following description, many specific details will be described in detail so that the reader can fully understand the following embodiments. However, the embodiments of the present invention can also be practiced without these specific details.

[0041] In the accompanying drawings, for the sake of clarity, the thickness of layers, films, panels, regions, etc. is magnified. Throughout the specification, the same reference numerals represent the same elements. It should be understood that when an element such as a layer, film, region or substrate is referred to as being "on" or "connected to" another element, it can be directly on or connected to another element, or an intermediate element can also exist. On the contrary, when an element is referred to as being "directly on" or "directly connected to" another element, there is no intermediate element. As used herein, "connection" can refer to physical and / or electrical connection. "About", "approximately", or "substantially" used herein include the average value within the acceptable deviation range of the value and the specific value determined by ordinary technicians in the field, taking into account the measurement discussed and the specific number of errors associated with the measurement (i.e., the limitations of the measurement system). For example, "about" can be expressed within one or more standard deviations of the value, or within ± 30%, ± 20%, ± 10%, ± 5%. Furthermore, the terms “about”, “approximately” or “substantially” used herein may select a more acceptable deviation range or standard deviation depending on the optical property, etching property or other property, and may not apply to all properties with one standard deviation.

[0042] See also Figure 1 , Figure 1 1 is a flow chart of a method for preparing a transmission electron microscope sample with internal defects according to some embodiments of the present invention. Preparation method 10 begins with step S11, which positions a sample so that the sample is perpendicular to the ion beam. In some embodiments, the sample is a sample with internal defects, such as a sample with a layered structure or a hole structure, and for example, in a FIB field of view of about 10 micrometers (μm) long and about 2 μm wide (that is, in a field of view magnified 1000 times), the layered and hole structures can be observed. In some embodiments, the material of the sample includes a nano coating, a ceramic or a metal. In some embodiments, the nano coating includes, but is not limited to, an indium tin oxide coating, a silicon oxide coating, an optical coating, a reflective coating, a glare coating, or a combination thereof. In some embodiments, the sample is made into a small piece and fixed on a sample stage. When the material of the sample is a nano coating or a ceramic, the surface of the sample is gold-plated to increase the conductivity of the sample, and then the sample is placed in the sample chamber of the device. In some embodiments, the gold plating time is 40 seconds, and the conductive sample may not be gold-plated. In some embodiments, the ion beam is generated by a focused ion beam system.

[0043] Next, step S12 is performed to etch the periphery of the target area of ​​the sample with an ion beam having a beam current of about 60 pA to about 9.3 nA to form an observation main surface and an observation back surface (such as Figure 2As shown). In some embodiments, the back side of the sample is opposite to the main side. In some embodiments, the target area is the area to be sampled for inspection. In some embodiments, the target area of ​​the sample is located, and the target area is first rough-processed, that is, an ion beam with a larger beam current is used to ion-etch (sputter) the front and rear areas of the target area into a groove shape to expose the main side and back side of the sample. In some embodiments, the sample is processed to a size of about length x width x height = 10x2x5 micrometers (μm), and the beam current can be selected to be 9.3nA.

[0044] Next, the sample is inspected in step S13 to confirm the internal defects of the sample. In some embodiments, the layering condition of the target area (e.g. Figure 3A , 3B The layered structure 114' shown in FIG. 114') or the hole distribution (eg Figure 4A , 4B The hole structure 114 is shown, the hole is located in the film layer, between the film layer and the substrate, in the substrate, or in both the film layer and the substrate.

[0045] Next, step S14 is performed for the first deposition: the sample is adjusted to tilt the sample from the positioning position by 0° to 10°, and then tungsten is deposited with an ion beam having a beam current of 10 pA to 200 pA to cover the main observation surface. In some embodiments, the sample angle is tilted, a lower voltage and beam current are selected, and the metal is sputtered by the ion beam to fill the main observation surface to cover the layered structure (such as Figure 5A , 5B as shown) or hole structure (as Fig. 6A , 6B As shown), a complete block structure with a dense surface is formed. From the perspective of observing the main surface, the width of the filled metal tungsten should be larger than the target area, that is, it should be larger than the target area (sampling area). Through low beam current, metal tungsten is used to fill the layered structure or hole structure at a slow speed, so that the filled sample is denser to play a fixing role. Furthermore, the deposition of metal tungsten is mainly achieved through low voltage. If the voltage is too strong, it will cause radiation damage to the sample. As for the selection of the tilt angle of 0° to 10°, it is to enable the hole structure of the sample to be deposited and filled with metal tungsten. If the angle is greater than 10°, it may cause the deposited metal tungsten to penetrate directly without being deposited in the hole. In some embodiments, the sample tilt angle is 5°, the low voltage can be selected to be 8keV, and the beam current can be selected to be 120pA, so that the layered or hole structure can be denser when filled with metal tungsten deposition. In addition, only the main surface to be observed can be filled with metal tungsten to play a fixing role. In other embodiments, metal tungsten is filled on the main observation surface and the back observation surface. In some embodiments, the target area is completely removed using a sampling needle to obtain a target model, and the target model of the sample is transferred to a supporting copper sheet for fixation (eg, Figure 7 ,8 , 9). In some embodiments, since the deposition rate of tungsten is slower than that of other materials (such as carbon, platinum, etc.), it can effectively fill samples with layered structures or porous structures to provide the effect of fixing and supporting the sample structure.

[0046] Then, step S15 is performed to deposit again: thinning the main observation surface of the sample, and inspecting the main observation surface. If the internal defects in the target area of ​​the sample are still not substantially filled with metal tungsten (such as Fig. 10A , 10B As shown in the figure), metal tungsten is deposited again until the internal defects in the target area of ​​the sample are substantially filled with metal tungsten to form a dense block structure (as shown in the figure). Fig.11 As shown). In some embodiments, the sample is first tangent (i.e., cut from the main observation surface) to remove the contamination layer that is deposited back on the sample surface during the sampling process, so that the true surface morphology after the first deposition is exposed, and then metal tungsten is deposited twice or multiple times. When the target area of ​​the sample is thin to a certain extent, both the main observation surface and the back observation surface are filled. In some embodiments, during the secondary deposition or multiple depositions, the sample tilt angle can be 5°, the low voltage can be selected to be 8keV, and the beam current can be selected to be 66pA. At this time, the target area thickness of the sample is 500nm, and the target area thickness of the sample must not be less than 200nm during the last deposition.

[0047] Next, step S16 is performed to thin the sample to between 50 nm and 100 nm in a manner parallel to the main observation surface from the back observation surface to the main observation surface. In some embodiments, after determining that the filling effect of the main observation surface of the sample is sufficient to meet the preparation requirements, the sample is then thinned by back cutting (i.e. cutting from the back observation surface) as the main method and tangent cutting as the auxiliary method to reduce the formation of new voids.

[0048] Finally, the sample can be selectively cleaned symmetrically on the main surface and the back surface by low voltage, and then the target model is taken out and transferred to the carrier copper sheet and observed in the transmission electron microscope. In some embodiments, the low voltage cleaning voltage is selected as 2keV, the beam current is selected as 72pA, the tilt angle is 6°, and the processing time is 20 seconds for the main surface and the back surface.

[0049] Example

[0050] Preliminary preparation: The focused ion beam microscope system is turned on in advance and stabilized for 15 minutes to avoid current fluctuations during TEM sample preparation that may affect the sample preparation effect. The ceramic pore structure sample 100 is selected as the test sample 100. The sample 100 has a substrate 102 and a film layer 104 disposed on the substrate 102.

[0051] Sample preparation: The test sample 100 is made into a size of 2 cm x 2 cm, placed on a non-magnetic metal sample table, fixed on the sample table with double-sided carbon conductive adhesive, and then placed in a gold plating machine for sputtering for 40 seconds, and then placed in a sample cabinet for use.

[0052] Injection: After the focused ion beam microscope system is stable, place the sample stage with the sample 100 on the turntable, deliver the sample 100 into the sample chamber through the injection rod, and tilt the sample stage to 52° so that the surface of the sample 100 is perpendicular to the ion beam (I-beam).

[0053] TEM sample preparation: A certain thickness of tungsten (1.5 μm thick) was sputtered on the top surface 111 (about 10 μm long and 2 μm wide) of the target area 110 of the sample 100 as protection, and a 9.3 nA beam current stepping (Regular) processing model was used to dig front and back pits (front pit 106, back pit 108, such as Figure 2 ), so that the target area 110 of the sample 100 forms an observation main surface 112 and an observation back surface 113 (as shown in Figure 2 , 4A 4B). Then, the surface cutting (Cleanning) processing model is further processed to eliminate the back deposition pollution. Then, the sample 100 is tilted to 57°, and the metal tungsten W is filled with 8keV voltage and 120pA beam current to cover the hole structure 114 (as shown in FIG. Fig. 6A , 6B As shown); in addition, in the viewing angle of the main surface 112, the width D1 of the filled metal tungsten W should be greater than the width D2 of the target area 110 (i.e., the sampling area). In addition to having the effect of fixing the structure of the sample 100, the filling of the metal tungsten W also makes it easy to observe and distinguish the internal structure of the sample due to the strong contrast difference between the metal tungsten W and the ceramic pore structure sample 100 under TEM. Next, the sample stage is turned back to the 0° state, and the left side 115 and the bottom 116 of the target area 110 are processed and cut using the 2.5μA beam current other side cutting (Rectangle) processing model, leaving only the right side 117 connected to the main body of the target area 110 to fix it. The height of the sample 100 is retained at 5μm. Next, the sampling needle X is introduced, and the sampling needle X moves and contacts the left side of the top surface 111 of the target area 110, and the sampling needle X is welded and fixed to the sample 100 by the method of depositing tungsten (as shown in FIG. Figure 7 ); using the 0.79μA beam current Rectangle processing method to cut off the right side 117 of the target area 110 (as shown in Figure 8 As shown in FIG. 1 ), the sampling needle X is raised to take out the target area 110 of the sample 100 to obtain a target model 110A, and the sampling needle X is withdrawn and the gas injection system (GIS) is withdrawn.

[0054] Transfer the target model 110A to the copper plate Y (Holder) installed by the navigation map, and then rotate the sample stage 180° relative to the current position, confirm that the height between the surface of the target model 110A and the electron beam pole shoe is 4 millimeters (mm), and then tilt the sample stage 52°. Next, select the location where the target model 110A is to be placed and move it to the middle of the screen, insert the sampling needle X (carrying the target model 110A), place the target model 110A on the copper plate Y, and also use the method of depositing tungsten to weld the bottom edge of the target model 110A to the copper plate Y (such as Fig. 9 As shown). When the main observation surface 112 of the target model 110A is viewed directly, a width structure Z is retained on each side without being thinned to serve as a support for the target model 110A on the supporting copper sheet Y. Next, the sampling needle X is cut off to separate it from the target model 110A, and the sampling needle X and GIS are withdrawn. Next, the sample stage is rotated 180° relative to each other, and the sample stage is tilted to 0°. It is confirmed that the height between the surface of the target model 110A and the electron beam pole shoe is 4mm. A 30keV voltage and a 0.79pA beam current are used to first perform a tangent to the target model 110A to remove the contamination layer that is deposited back on the surface of the sample 100 during the sampling process, so that the true surface morphology after the first deposition is exposed. Next, after back-cutting the sample 100 to 500nm, the sample 100 is tilted 5°, and metal tungsten W is filled using an 8keV voltage and a 66pA beam current to cover the hole structure 114 (as shown in FIG. Fig. 12A and 12B Then, the target model 110A is thinned by back cutting as the main method and front cutting as the auxiliary method. When the target model 110A is thinned to 200nm, if it is found that some of the hole structures 114 are filled with metal tungsten W, but some of the hole structures 114 are not filled with metal tungsten W, the step of depositing metal tungsten W is no longer performed to avoid damage to the sample 100 due to too thin thickness during deposition (such as Fig.13A and 13B ). Then, the film is further thinned to a thickness of less than 100 nm.

[0055] Low voltage surface cleaning: select voltage 2keV, beam current 72pA, focus adjustment clear, front and back tilt angle 6°, use Rectangle processing method, and set the processing time to 20s each. Then the target model 110A is prepared. Exit the sample rod, remove the carrier copper sheet Y and enter the TEM for observation.

[0056] The present invention is a method for filling a layered structure and / or a porous structure by depositing metal tungsten. Due to its slow deposition rate, the protective layer formation process is dense, so that the sample with layered or porous materials can be fully filled with the protective layer. Finally, the sample can be completely taken out during the preparation of the target model, and the layered interface or the surrounding area of ​​the hole is protected during the thinning process, reducing the damage to the sample during the thinning process and the misjudgment of the analysis results, so as to achieve a better TEM observation effect.

[0057] The above description is only a preferred embodiment of the present invention and is not intended to limit the present invention. Any modifications, equivalent substitutions, improvements, etc. made within the spirit and principles of the present invention should be included in the scope of protection of the present invention.

Claims

1. A method for preparing a transmission electron microscope sample with internal defects, It is characterized in that include: Positioning a sample so that the surface of the sample is perpendicular to an ion beam and enters a positioning position; Etching a periphery of a target area of ​​the sample with the ion beam having a beam current of 60 pA to 9.3 nA to form an observation main surface and an observation back surface of the sample opposite to the observation main surface; Inspect the sample to confirm the internal defects of the sample; Deposition is performed for the first time: the sample is adjusted so that the sample is tilted from the positioning position by 0° to 10°, and then tungsten is deposited with the ion beam having a beam current of 10 pA to 200 pA to cover the observation main surface; Depositing again: thinning the observation main surface of the sample and inspecting the observation main surface. If the internal defects of the target area of ​​the sample are still not substantially filled with tungsten, depositing tungsten again until the internal defects of the target area of ​​the sample are substantially filled with tungsten to form a dense block structure; and The sample is thinned to a thickness between 50 nanometers and 100 nanometers in a direction from the observation back surface to the observation main surface in parallel with the observation main surface.

2. The method for preparing a transmission electron microscope sample with internal defects according to claim 1, It is characterized in that The internal defects include a layered structure or a hole structure.

3. The method for preparing a transmission electron microscope sample with internal defects according to claim 1, It is characterized in that In the step of performing deposition for the first time, the sample is adjusted to tilt 2° to 5° from the positioning position.

4. The method for preparing a transmission electron microscope sample with internal defects according to claim 1, It is characterized in that In the step of re-deposition, the main observation surface of the sample is thinned by sequentially using beam currents of 0.79nA, 0.43nA, 0.23nA, and 80pA, and tilting ±0.7° to ±3° to symmetrically thin the sample front and back until the thickness reaches 200nm to 300nm.

5. The method for preparing a transmission electron microscope sample with internal defects according to claim 1, It is characterized in that The material of the sample includes nano-coating, ceramic or metal.

6. The method for preparing a transmission electron microscope sample with internal defects according to claim 5, It is characterized in that The material of the sample is an electronic component including an optical film.

7. The method for preparing a transmission electron microscope sample with internal defects according to claim 1, It is characterized in that The first deposition step includes tilting the sample from the positioning position by 0° to 10°, and then depositing tungsten with the ion beam having a beam current of 10 to 200 pA and a voltage of 15 to 30 keV.

8. The method for preparing a transmission electron microscope sample with internal defects as claimed in claim 1, It is characterized in that The first deposition step includes tilting the sample from the positioning position by 0° to 5°, and then depositing tungsten with the ion beam having a beam current of 10 to 120 pA and a voltage of 8 keV.

9. The method for preparing a transmission electron microscope sample with internal defects according to claim 1, It is characterized in that If the internal defects of the target area of ​​the sample are still not substantially filled with tungsten, a deposition step is performed again, including depositing tungsten with the ion beam having a voltage of 8 keV and a beam current of 15 pA to 1.2 nA.

10. The method for preparing a transmission electron microscope sample with internal defects according to claim 9, It is characterized in that If the internal defects of the target area of ​​the sample are still not substantially filled with tungsten, a deposition step is performed again, including depositing tungsten with the ion beam having a voltage of 5 keV and a beam current of 15 pA to 1.2 nA.

Citation Information

Cited By

  • Preparation method of transmission electron microscope sample of cutting edge of single-point diamond cutter

    CN119985563A

  • Focused ion beam sample preparation method for reducing curtain effect of porous transmission sample

    CN121007748A