High-sensitivity rare earth doped tin oxide film gas sensor

Through rare earth La doping and multi-layer packaging technology, the selectivity and sensitivity of SnO2 thin film gas sensors are improved, solving the problems of low-concentration gas detection and stability of traditional sensors, and achieving efficient gas monitoring and real-time response.

CN118731114APending Publication Date: 2024-10-01YANGTZE DELTA REGION INST (QUZHOU) UNIV OF ELECTRONIC SCI & TECH OF CHINA
View PDF 0 Cites 0 Cited by

Patent Information

Application Number
CN202410752946.7
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Filing Date
2024-06-11
Publication Date
2024-10-01

AI Technical Summary

Technical Problem

Traditional SnO2 thin film gas sensors have limitations in low-concentration gas detection and gas selectivity, and their stability and response speed are insufficient, making it difficult to meet high-precision and real-time monitoring requirements.

Method used

The rare earth element La doped SnO2 is used as the gas sensing layer material, and through ultrasonic spray pyrolysis and multi-layer encapsulation technology, the crystallinity and electrical properties of the film are improved, the selectivity and sensitivity to specific gases are enhanced, and the temperature dependence and sensitivity are reduced. Recovery time.

Benefits of technology

It significantly improves the selectivity, stability and sensitivity of the gas sensor, weakens the temperature dependence, enhances the anti-interference ability and real-time monitoring capability, and is suitable for multiple application fields.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN118731114A_ABST
    Figure CN118731114A_ABST
Patent Text Reader

Abstract

The invention relates to the field of semiconductor materials, in particular to a high-sensitivity rare earth doped tin oxide thin film gas sensor, and aims to improve the gas detection sensitivity and selectivity of a tin oxide thin film, enhance the stability of the sensor and simplify the preparation process to adapt to large-scale production. The key technical innovation comprises the steps of using rare earth element doping and optimizing process conditions to improve the optical and electrical properties of the SnO2 film, so that the SnO2 film is suitable for multiple fields of solar cells, optoelectronic devices, gas sensors and the like. According to the technical scheme, the method mainly comprises the following steps: selecting a flexible material PI as an electrode substrate and cleaning; preparing a platinum electrode on the substrate; preparing a SnO2 precursor solution; generating a SnO2: La film by adopting an ultrasonic spray pyrolysis method; carrying out post-annealing treatment on the thin film; preparing a platinum electrode on the thin film; and performing multi-layer packaging processing on the sensor.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The present invention relates to the field of semiconductor materials, in particular to a high-sensitivity rare earth-doped tin oxide thin film gas sensor. Background Art

[0002] Semiconductor gas sensors detect gases by exploiting changes in physical properties such as conductivity that occur when the gas under test comes into contact with the surface of a semiconductor (primarily metal oxides). Depending on whether the changes caused by the interaction between the semiconductor and the gas are limited to the semiconductor surface or extend deep into the semiconductor, they can be categorized as surface-controlled or bulk-controlled. In the first type, electron transfer occurs between the gas adsorbed on the semiconductor surface and the semiconductor, resulting in changes in physical properties such as conductivity, while maintaining the internal chemical composition. In the second type, the reaction between the semiconductor and the gas causes changes in the semiconductor's internal composition (lattice defect concentration), which in turn alters the conductivity.

[0003] According to the physical properties of semiconductor changes, they can be divided into two categories: resistive and non-resistive. Resistive semiconductor gas sensors use the change in resistance of the sensitive material when it comes into contact with the gas to detect the composition or concentration of the gas; non-resistive semiconductor gas sensors use other parameters, such as the diode volt-ampere characteristics and the threshold voltage change of the field effect transistor to detect the gas being measured. SnO2 (tin oxide) is currently the most widely used gas sensor. SnO2 thin film, as an important semiconductor material, is widely used in gas sensors. Traditional SnO2 thin film gas sensors have certain limitations in terms of gas type detection and sensitivity, especially in low-concentration gas detection, which is not ideal. Therefore, there is an urgent need to develop a highly sensitive and selective SnO2 thin film gas sensor.

[0004] SnO2 is an important transparent conductive oxide widely used in optoelectronic devices, solar cells, and gas sensors. However, undoped tin oxide thin films still have deficiencies in conductivity and light transmittance, limiting their application. While existing technologies have improved their performance through doping, more efficient doping methods and materials are still needed to further enhance their performance. SnO2 thin films are widely used in gas sensors due to their excellent semiconductor properties and good chemical stability. However, conventional SnO2 thin-film gas sensors have limitations in low-concentration gas detection and gas selectivity. Therefore, there is an urgent need to develop SnO2 thin-film gas sensors with high sensitivity and excellent selectivity. La-doped SnO2 exhibits excellent performance in gas sensors: La doping can significantly improve the gas-sensing properties of tin oxide, enhancing its selectivity and sensitivity for certain gases while also improving sensor stability and response speed. La atoms incorporate into the SnO2 lattice, creating more oxygen vacancies and adsorption sites. This increases the adsorption of gas molecules on the sensor surface, strengthens the resistance change signal, and thus enhances its selectivity and sensitivity for target gases. La doping can also lower the optimal operating temperature of SnO2 sensors. Traditional SnO2 gas sensors usually operate at high temperatures of 200-400°C, but La doping allows the sensor to maintain high sensitivity and fast response at lower temperatures, reducing energy consumption and improving the practicality of the sensor; La doping increases the rate of redox reactions on the sensor surface, accelerates the adsorption and desorption process of gas molecules, thereby improving the response speed and recovery time of the sensor. Summary of the Invention

[0005] The key technical challenges addressed by this invention include improving the gas detection sensitivity and selectivity of tin oxide thin films, enhancing sensor stability, and simplifying the preparation process to facilitate large-scale production. By doping with rare earth elements and optimizing process conditions, the optical and electrical properties of SnO2 thin films are enhanced, making them suitable for a variety of applications, including solar cells, optoelectronic devices, and gas sensors.

[0006] In order to achieve the above object, the present invention adopts the following technical means:

[0007] The present invention provides a method for preparing a highly sensitive rare earth-doped tin oxide thin film, comprising the following steps:

[0008] Step 1: Select flexible material PI as the electrode substrate and clean it to remove organic matter, particles and other contaminants on the surface;

[0009] Step 2: Electrodes are prepared on the upper surface of the substrate. Platinum is selected as the electrode material and printed using a micro-nano 3D printer to form an electrode pattern with a thickness of 100 nanometers on the surface.

[0010] Step 3: Prepare a SnO2 precursor solution by dissolving SnCl2·2H2O in anhydrous ethanol water to prepare a 0.8 mol / l solution. At the same time, add 0.2 ml of concentrated hydrochloric acid and ethylene glycol as a surfactant to improve the quality of the film. Finally, stir evenly on a magnetic stirrer to obtain a SnO2 precursor solution.

[0011] Step 4: using ultrasonic spray pyrolysis, the precursor solution is atomized into tiny droplets using an ultrasonic oscillator, and the atomized droplets are transported to the surface of the heated substrate obtained in step 2 by airflow to form a SnO2:La thin film;

[0012] Step 5: Post-annealing the prepared SnO2:La film to improve the crystallinity and electrical properties of the film;

[0013] Step 6: Prepare an electrode on the surface of the SnO2:La film. The electrode material is platinum Pt. Print it with a micro-nano 3D printer to form an electrode pattern with a thickness of 100 nanometers on the surface.

[0014] Step 7: Perform multi-layer packaging processing on the SnO2 thin film gas sensor to obtain a well-packaged sensor.

[0015] In the above method, step 1 includes:

[0016] Step 1.1: Place the substrate in a mixture of acetone, ethanol, and deionized water and clean it using an ultrasonic cleaner for about 10-15 minutes each time.

[0017] Step 1.2: Rinse the substrate several times with deionized water to remove solvent residues.

[0018] Step 1.3, immersing the substrate in a diluted 0.5 mol / 1 hydrochloric acid solution and ultrasonically cleaning for 5-10 minutes to remove metal ions and inorganic pollutants on the surface;

[0019] Step 1.4: Rinse with deionized water to prevent residual acid and alkali from affecting subsequent steps;

[0020] Step 1.5: Place the substrate in a drying oven, dry it at 60-100° C., and anneal it at 500° C. for 1 hour to remove moisture and organic residues on the surface and improve the cleanliness of the substrate.

[0021] In the above method, step 2 includes:

[0022] Step 2.1, design the desired electrode pattern using computer-aided design software;

[0023] Step 2.2, fix the prepared substrate on the platform of the 3D printer;

[0024] Step 2.3: Set parameters such as print head speed, nozzle diameter, and ink flow rate to ensure uniform deposition.

[0025] Step 2.4: Thermally cure at 150-200° C. for 30-60 minutes to form an electrode.

[0026] In the above method, step 3 includes:

[0027] Step 3.1, dissolve SnCl2·2H2O in anhydrous ethanol water to form a homogeneous solution;

[0028] Step 3.2: Add 0.2 ml of concentrated hydrochloric acid and 10 ml of ethylene glycol as a surfactant to improve the quality of the film;

[0029] Step 3.3: Stir the solution evenly on a magnetic stirrer to obtain a SnO2 precursor solution.

[0030] In the above method, step 4 includes:

[0031] Step 4.1, using an ultrasonic oscillator to atomize the precursor solution into tiny droplets;

[0032] Step 4.2, transporting the atomized droplets to the surface of the heated substrate obtained in step 2 by air flow;

[0033] Step 4.3: Control the substrate temperature between 300°C and 600°C, and spray for 15 minutes. After the atomized droplets reach the heated substrate surface, they evaporate and decompose rapidly due to the high temperature of the substrate, and a pyrolysis reaction occurs to generate a SnO2:La film.

[0034] In the above method, step 5 includes:

[0035] Step 5.1, placing the prepared SnO2:La film into an annealing furnace;

[0036] Step 5.2: Anneal at 900°C in a nitrogen atmosphere for 1 hour to control the crystallization quality and microstructure of the film.

[0037] In the above method, step 6 includes:

[0038] Step 6.1, design the desired electrode pattern using computer-aided design software;

[0039] Step 6.2, fix the prepared SnO:La thin film substrate on the platform of the 3D printer;

[0040] Step 6.3: Set parameters such as print head speed, nozzle diameter, and ink flow rate to ensure uniform deposition;

[0041] Step 6.4: Thermally cure at 150-200° C. for 30-60 minutes to form an electrode.

[0042] In the above method, step 7 includes:

[0043] Step 7.1: Deposit a gas permeable membrane on the gas-sensitive film to allow specific gas molecules to pass through and prevent dust and other impurities from entering;

[0044] Step 7.2: Depositing a corrosion-resistant and high-temperature-resistant protective layer on the gas permeable layer to improve the environmental adaptability and durability of the sensor;

[0045] Step 7.3: Remove the sample from the reaction chamber, rinse with ethanol and deionized water, and then blow dry with nitrogen to remove any residual chemicals;

[0046] Step 7.4: High-temperature annealing is performed in an argon environment at 500° C. for 30 minutes to further improve the density and durability of the silicon nitride film.

[0047] The commonly used gas sensor materials currently have the following main problems:

[0048] Poor selectivity: Existing gas sensor materials are often interfered with by other gases when detecting specific gases, resulting in inaccurate detection results.

[0049] Insufficient stability: During long-term use, the sensitivity and response speed of the sensor material may decrease, affecting the reliability and life of the sensor.

[0050] Limited sensitivity: Some gas sensors have poor detection capabilities for low-concentration gases and cannot meet the needs of high-precision detection.

[0051] Strong temperature dependence: The performance of gas sensors is often greatly affected by the ambient temperature, resulting in inconsistent detection results under different temperature conditions.

[0052] Poor recovery: Existing gas-sensitive materials take a long time to recover after detection, affecting the real-time monitoring capability of the sensor.

[0053] The present invention uses rare earth La-doped SnO2 as the gas-sensing layer material to address the above-mentioned shortcomings of the prior art. Analyzing the technical characteristics of the present invention from the technical implementation level, it has the following beneficial effects:

[0054] High gas selectivity

[0055] The rare earth element La has a unique electronic structure and catalytic properties. Doping tin oxide with La can significantly improve the material's selectivity for specific gases. La doping can also modulate the adsorption and reaction properties of the tin oxide surface, making it more selective for target gases.

[0056] High stability

[0057] La doping improves the structural stability of the SnO2 material and reduces performance degradation over long-term use. Rare earth elements possess high chemical stability and oxidation resistance, effectively suppressing device performance degradation in high temperatures and harsh environments. Furthermore, the multi-layer packaging technology employed effectively isolates the sensor material from external environmental influences by adding multiple protective layers to the sensor surface. These layers prevent moisture, dust, and other contaminants from entering the sensor material, significantly improving the sensor's long-term stability and reliability.

[0058] Improve sensitivity

[0059] The addition of rare earth La creates a large number of oxygen vacancies and surface active sites in SnO2, increasing the adsorption capacity and reactivity of gas molecules, thereby improving the sensor's detection sensitivity to low-concentration gases. La doping also promotes electron transfer and gas reaction speed, further enhancing the sensor's sensitivity.

[0060] Reduce temperature dependence

[0061] La doping can modulate the electrical and surface chemical properties of tin oxide, resulting in a relatively consistent gas-sensing response across different temperatures. This can reduce the impact of temperature changes on sensor performance and improve the stability and accuracy of detection results. Multi-layer packaging materials can also effectively reduce the impact of ambient temperature and humidity on sensor performance to a certain extent, thereby improving the consistency and accuracy of detection results.

[0062] Improved recovery

[0063] Multi-layer packaging technology can optimize the sensor's thermodynamic and kinetic properties, promote the rapid adsorption and desorption of gas molecules on the sensor surface, accelerate response and recovery speeds, and enhance real-time monitoring capabilities. It can also quickly return to its initial state during continuous detection and maintain efficient working performance. It can also effectively shield and filter external interference signals, thereby improving the sensor's anti-interference ability and signal stability.

[0064] La doping can promote the rapid adsorption and desorption of gas molecules on the tin oxide surface, shortening the response and recovery time of the sensor. This modification improves the real-time monitoring capability of the sensor.

[0065] Through multi-layer packaging technology and rare earth La doping, this invention significantly improves the selectivity, stability, sensitivity, and resilience of SnO2 gas sensors, reduces temperature dependence, and enhances anti-interference capabilities. These improvements address technical issues with existing gas sensor materials, enabling them to perform better in a variety of applications, with broad application prospects and significant technical advantages. BRIEF DESCRIPTION OF THE DRAWINGS

[0066] Figure 1 The device preparation flow chart;

[0067] Figure 2 is the photolithographic shape of the Pt electrode;

[0068] Figure 3 This is a schematic diagram of the planed structure of the gas sensor. DETAILED DESCRIPTION

[0069] The following is a detailed description of the embodiments of the present invention. Although the present invention will be described and illustrated in conjunction with certain specific embodiments, it should be noted that the present invention is not limited to these embodiments. On the contrary, modifications or equivalent substitutions of the present invention are intended to fall within the scope of the claims of the present invention.

[0070] In addition, in order to better illustrate the present invention, numerous specific details are given in the following detailed description. It will be understood by those skilled in the art that the present invention can also be implemented without these specific details.

[0071] The present invention aims to solve a series of problems in the practical application of the device, such as stability, sensitivity, durability and anti-interference ability.

[0072] 1. Environmental stability: Multi-layer packaging effectively prevents the influence of environmental humidity and pollutants on the SnO2 gas-sensitive film, improving the long-term stability and durability of the device.

[0073] 2. Sensitivity and selectivity: By introducing catalysts and porous structures, the sensitivity and selectivity of gas sensors to specific gases are significantly improved, and the response to non-target gases is reduced.

[0074] 3. Anti-interference capability: Multi-layer packaging effectively reduces the impact of external interference gases and electromagnetic waves on sensor performance, ensuring the accuracy and stability of sensor signals. It can work stably under different temperature conditions, improving the response speed and consistency of the sensor.

[0075] The present invention provides a method for preparing a highly sensitive rare earth-doped tin oxide thin film, comprising the following steps:

[0076] Step 1: Select flexible material PI as the electrode substrate and clean it to remove organic matter, particles and other contaminants on the surface;

[0077] Step 2: Electrodes are prepared on the upper surface of the substrate. Platinum is selected as the electrode material and printed using a micro-nano 3D printer to form an electrode pattern with a thickness of 100 nanometers on the surface.

[0078] Step 3, preparing a SnO2 precursor solution, dissolving SnCl2·2H2O in anhydrous ethanol water to prepare a 0.8 mol / l solution, adding 0.2 ml of concentrated hydrochloric acid and ethylene glycol as a surfactant to improve the quality of the film, and finally stirring evenly on a magnetic stirrer to obtain a SnO2 precursor solution;

[0079] Step 4: using ultrasonic spray pyrolysis, the precursor solution is atomized into tiny droplets using an ultrasonic oscillator, and the atomized droplets are transported to the surface of the heated substrate obtained in step 2 by airflow to form a SnO2:La thin film;

[0080] Step 5: Post-annealing the prepared SnO2:La film to improve the crystallinity and electrical properties of the film;

[0081] Step 6: Prepare an electrode on the surface of the SnO2:La film. The electrode material is platinum Pt. Print it with a micro-nano 3D printer to form an electrode pattern with a thickness of 100 nanometers on the surface.

[0082] Step 7: Perform multi-layer packaging processing on the SnO2 thin film gas sensor to obtain a well-packaged sensor.

[0083] In the above method, step 1 includes:

[0084] Step 1.1: Place the substrate in a mixture of acetone, ethanol, and deionized water and clean it using an ultrasonic cleaner for about 10-15 minutes each time.

[0085] Step 1.2: Rinse the substrate several times with deionized water to remove solvent residues.

[0086] Step 1.3, immersing the substrate in a diluted 0.5 mol / 1 hydrochloric acid solution and ultrasonically cleaning for 5-10 minutes to remove metal ions and inorganic pollutants on the surface;

[0087] Step 1.4: Rinse with deionized water to prevent residual acid and alkali from affecting subsequent steps;

[0088] Step 1.5: Place the substrate in a drying oven, dry it at 60-100° C., and anneal it at 500° C. for 1 hour to remove moisture and organic residues on the surface and improve the cleanliness of the substrate.

[0089] In the above method, step 2 includes:

[0090] Step 2.1, design the desired electrode pattern using computer-aided design software;

[0091] Step 2.2, fix the prepared substrate on the platform of the 3D printer;

[0092] Step 2.3: Set parameters such as print head speed, nozzle diameter, and ink flow rate to ensure uniform deposition.

[0093] Step 2.4: Thermally cure at 150-200° C. for 30-60 minutes to form an electrode.

[0094] In the above method, step 3 includes:

[0095] Step 3.1, dissolve SnCl2·2H2O in anhydrous ethanol water to form a homogeneous solution;

[0096] Step 3.2: Add 0.2 ml of concentrated hydrochloric acid and 10 ml of ethylene glycol as a surfactant to improve the quality of the film;

[0097] Step 3.3: Stir the solution evenly on a magnetic stirrer to obtain a SnO2 precursor solution.

[0098] In the above method, step 4 includes:

[0099] Step 4.1, using an ultrasonic oscillator to atomize the precursor solution into tiny droplets;

[0100] Step 4.2, transporting the atomized droplets to the surface of the heated substrate obtained in step 2 by air flow;

[0101] Step 4.3: Control the substrate temperature between 300°C and 600°C, and spray for 15 minutes. After the atomized droplets reach the heated substrate surface, they evaporate and decompose rapidly due to the high temperature of the substrate, and a pyrolysis reaction occurs to generate a SnO2:La film.

[0102] In the above method, step 5 includes:

[0103] Step 5.1, placing the prepared SnO2:La film into an annealing furnace;

[0104] Step 5.2: Anneal at 900°C in a nitrogen atmosphere for 1 hour to control the crystallization quality and microstructure of the film.

[0105] In the above method, step 6 includes:

[0106] Step 6.1, design the desired electrode pattern using computer-aided design software;

[0107] Step 6.2, fix the prepared SnO:La thin film substrate on the platform of the 3D printer;

[0108] Step 6.3: Set parameters such as print head speed, nozzle diameter, and ink flow rate to ensure uniform deposition;

[0109] Step 6.4: Thermally cure at 150-200° C. for 30-60 minutes to form an electrode.

[0110] In the above method, step 7 includes:

[0111] Step 7.1: Deposit a gas permeable membrane on the gas-sensitive film to allow specific gas molecules to pass through and prevent dust and other impurities from entering;

[0112] Step 7.2: Depositing a corrosion-resistant and high-temperature-resistant protective layer on the gas permeable layer to improve the environmental adaptability and durability of the sensor;

[0113] Step 7.3: Remove the sample from the reaction chamber, rinse with ethanol and deionized water, and then blow dry with nitrogen to remove any residual chemicals;

[0114] Step 7.4: High-temperature annealing is performed in an argon environment at 500° C. for 30 minutes to further improve the density and durability of the silicon nitride film.

[0115] Example 1

[0116] 1. Preparation method of SnO2 thin film:

[0117] Selection and cleaning of the substrate: The present invention selects flexible material PI as the electrode substrate and cleans it. The cleaning process of the substrate is intended to remove organic matter, particles and other contaminants on the surface to ensure the uniformity and adhesion of the material deposition. First, the PI substrate is placed in a mixture of acetone, ethanol and deionized water, and cleaned using an ultrasonic cleaner for about 10-15 minutes each time; after cleaning, the substrate is rinsed with deionized water several times to remove solvent residues; then the substrate is immersed in a diluted hydrochloric acid (HCl, 0.5 mol / l) solution and ultrasonically cleaned for 5-10 minutes to remove metal ions and inorganic pollutants on the surface; after acid and alkali cleaning, a large amount of deionized water is used for thorough rinsing to avoid residual acid and alkali affecting subsequent steps; finally, the substrate is placed in a drying oven, dried at a temperature of 60-100°C, and subjected to high-temperature annealing to remove surface moisture and organic residues to improve the cleanliness of the substrate (500°C, 1h). By cleaning the substrate in the above steps, the substrate surface can be ensured to be clean, providing a good foundation for subsequent material deposition and patterning.

[0118] Electrode preparation: Electrodes are prepared on the surface of the substrate. Platinum is selected as the electrode material and printed using a micro-nano 3D printer to form an electrode pattern with a thickness of 100 nanometers on the surface.

[0119] Preparation of precursor solution: Dissolve stannous chloride (SnCl2·2H2O) in anhydrous ethanol water to prepare a 0.8 mol / l solution. Add a small amount of concentrated hydrochloric acid (0.2 ml) and surfactant (ethylene glycol) to improve the quality of the film. Finally, stir evenly on a magnetic stirrer to prepare a SnO2 precursor solution. Then add LACl3·7H2O (La:Sn) with an atomic ratio of 1-3 at% to form a rare earth doping solution.

[0120] Thin film deposition: Ultrasonic Spray Pyrolysis (USP) is used, employing an ultrasonic oscillator to atomize the precursor solution into tiny droplets. The frequency and power of the ultrasonic oscillator can be adjusted to control the size and distribution of the atomized droplets. An airflow then transports the atomized droplets to a heated substrate surface. The airflow rate and nozzle design affect the efficiency and uniformity of the atomized droplet transport. Upon reaching the heated substrate surface, the atomized droplets rapidly evaporate and decompose due to the high temperature of the substrate, undergoing a pyrolysis reaction to form a SnO2:La thin film. The substrate temperature is controlled between 300°C and 600°C, the spray pressure is set at 2-3 bar, the atomizer frequency is set at 1.7 MHz, the spray rate is 2 ml / min, and the spray distance to the substrate is 15 cm. Once deposition begins, a tin oxide thin film grows layer by layer on the substrate surface, forming a uniform film (the spray time is controlled to be 15-30 minutes).

[0121] Post-treatment: The prepared SnO2:La film was subjected to post-annealing treatment to improve the crystallinity and electrical properties of the film (annealing at 900°C in a nitrogen atmosphere for 1 h) and to control the crystallization quality and microstructure of the film.

[0122] 2. Preparation of gas sensor:

[0123] 2.1 Photolithography

[0124] A photoresist is applied to the substrate, and photolithography is used to form patterned microstructures that will define the areas of the gas-sensing film and electrodes.

[0125] 2.2 Pt electrode preparation

[0126] Electrodes were prepared on the upper and lower surfaces of the SnO2:La film. Platinum (Pt) was selected as the electrode material. Electrode patterns with a thickness of 50-100 nm were formed on the surface by micro-nano 3D printer (see attached figure). Figure 2 high-resolution and high-precision electrode preparation is achieved.

[0127] First, use computer-aided design software to design the required electrode pattern, ensuring that the pattern meets the design and functional requirements of the sensor, and prepare the selected Pt nanoparticle ink. Then, fix the prepared SnO:La film substrate to the platform of the 3D printer to ensure the substrate surface is flat. The specific operating parameters are set as follows:

[0128] Print head speed: Typically in the range of 1-10 mm / s. Needs to be adjusted based on the ink viscosity and jetting characteristics to ensure uniform deposition.

[0129] Nozzle diameter: The nozzle diameter should be selected to an appropriate size, generally in the range of 10-50μm, depending on the resolution requirements of the electrode pattern.

[0130] Ink flow rate: The ink flow rate should be precisely controlled, generally within the range of 0.1-10μl / min. Excessive flow rate will result in blurred patterns, while too low flow rate will cause line breakage. The inkjet time should be controlled within 5-10 minutes, and the electrode thickness formed should be within the range of 300-400nm. Finally, heat curing should be carried out (it should be controlled within the curing temperature range of the ink) at 150-200℃ for 30-60 minutes.

[0131] 2.3 Multi-layer packaging

[0132] The prepared SnO2 thin film gas sensor is connected to the lead wire, and a multi-layer packaging design is adopted in combination with flexible packaging materials (polyimide). This not only provides good sealing, but also makes the sensor flexible, making it suitable for wearable devices and flexible electronic products. Nano-coating technology is applied to the surface of the packaging material to enhance the waterproof, oil-proof and dust-proof properties, thereby improving the reliability of the sensor in harsh environments.

[0133] 2.3.1 Preparation of gas permeable layer

[0134] A gas permeable membrane (porous alumina) is deposited on the gas-sensitive film. This membrane can selectively allow specific gas molecules to pass through while preventing dust and other impurities from entering, thus protecting the gas-sensitive film. The specific steps are as follows:

[0135] Aluminum sheet preparation:

[0136] Aluminum sheet cleaning: Use an organic solvent (such as ethanol or acetone) to clean the aluminum sheet surface to remove grease and other organic contaminants. Then rinse with deionized water.

[0137] Surface treatment: Use a weak acid (such as a 1-5% NaOH or KOH solution) to chemically etch the surface of the aluminum sheet to remove the oxide layer. Rinse with deionized water, then use a dilute acid (such as a 5% HNO3 solution) to neutralize the remaining alkali solution. Finally, rinse thoroughly with deionized water and dry.

[0138] Pre-oxidation:

[0139] A short anodization (in the same electrolyte and conditions) was performed to form an initial aluminum oxide layer, which was then peeled off to obtain a smooth and uniform surface, which helped to obtain a more uniform porous structure (anodization time was 50 s, voltage was set between 20 and 35 V, and scan speed was ).

[0140] Anodizing:

[0141] Electrolyte preparation: 0.1 mol / 1 sulfuric acid.

[0142] Electrolytic cell preparation: Place the aluminum sheet as the anode (positive electrode) and the platinum sheet as the cathode (negative electrode) into the electrolytic cell.

[0143] Apply voltage: A constant voltage (typically between 30-40V) is applied to the electrolyte to initiate the anodizing process. Current flows through the aluminum sheet, causing an oxidation reaction to occur on the surface, forming a porous aluminum oxide film. The oxidation time is set to 20-25 minutes at room temperature.

[0144] Washing and drying:

[0145] After anodization, the aluminum sheet was thoroughly rinsed with deionized water and ethanol to remove residual electrolyte and by-products, and then dried under a nitrogen atmosphere (300°C, 20 min).

[0146] Separation and cleaning of alumina membrane:

[0147] The porous alumina membrane prepared by electrochemically dissolving the underlying aluminum is separated from the aluminum substrate, and then the porous alumina membrane is thoroughly rinsed with deionized water to remove residual electrolyte; the cleaned porous alumina membrane is then immersed in anhydrous ethanol and then dried in a nitrogen atmosphere or in a low-temperature oven.

[0148] Spin coating of porous aluminum oxide film on gas sensitive film:

[0149] The porous alumina membrane is cut into thin slices of appropriate size and placed in anhydrous ethanol to form a suspension for later use; the prepared gas-sensitive film is fixed on the sample stage of the spin coating equipment, and an appropriate amount of suspension is dropped on the center of the gas-sensitive film using a dropper. The rotation speed (2000-3000 rpm) and time (30-60s) of the coater are set to make the suspension evenly distributed on the surface of the gas-sensitive film, and then placed in a low-temperature oven (60-80℃ drying for 15-30min) for slight heat treatment to promote the adhesion of the porous alumina membrane and the gas-sensitive film and promote interface bonding.

[0150] 2.3.2 Preparation of protective layer

[0151] A corrosion-resistant and high-temperature-resistant protective layer (silicon nitride) is deposited on top of the gas permeable layer to improve the environmental adaptability and durability of the sensor. The following are the detailed process steps:

[0152] Deposition Equipment Preparation: Silicon nitride is deposited using a plasma-enhanced chemical vapor deposition (PECVD) system. Process parameters are set using ammonia (NH3) and silane (SiH4) or dichlorosilane (SiCl2H2) as the reactant gases. The temperature is between 300-400°C and the pressure is relatively high (500-800 mTorr). Appropriate gas flow rates are set to ensure uniform film deposition. The SiH4:NH3 flow ratio is typically 1:5-1:10.

[0153] Deposition process:

[0154] The prepared sample (SnO2 thin film with a gas permeable layer of porous alumina) is placed in a CVD reaction chamber.

[0155] Gradually increase the temperature to the set temperature and keep it stable (300℃).

[0156] Turn on the flow of the reaction gases (SiH4 and NH3) and start depositing the silicon nitride film to form a dense silicon nitride layer. Control the deposition time to 5-10 minutes to obtain a silicon nitride protective layer of the desired thickness (usually 80-200 nm).

[0157] Drying and annealing process

[0158] After deposition, the sample was removed from the reaction chamber, rinsed with ethanol and deionized water, and then blown dry with nitrogen to remove any residual chemicals; followed by post-annealing treatment (high-temperature annealing in an argon environment, 500°C, 30 minutes) to further improve the density and durability of the silicon nitride film.

[0159] Through the above innovative packaging process, the performance, reliability and applicability of semiconductor thin-film gas sensors can be significantly improved to meet the needs of modern smart devices and Internet of Things applications.

[0160] The innovative points of the present invention are summarized as follows:

[0161] High sensitivity: By optimizing the preparation process and structural design of the tin oxide film, the present invention significantly increases the surface area and the number of active sites of the tin oxide film, thereby improving the sensitivity of the gas sensor, especially in the detection of low-concentration gases.

[0162] High selectivity: By regulating the microstructure of the film, special surfactants and heat treatment process and electrode design, the gas sensor of the present invention has high selectivity for gases and reduces cross interference.

[0163] Good stability: The optimized packaging process (multi-layer packaging) ensures the stability and reliability of the gas sensor in long-term use.

[0164] Simple preparation process: The preparation method of the tin oxide thin film gas sensor of the present invention is simple, can be produced on a large scale, and has good industrial application prospects.

[0165] Through this multi-layer packaging process, a selectively permeable gas membrane is deposited on the gas-sensitive film. This multi-layer structure not only protects the gas-sensitive film from contamination by dust and other impurities, but also selectively allows specific gas molecules to pass through, improving the selectivity and sensitivity of the sensor.

[0166] Application Areas

[0167] The innovative doped tin oxide film of the present invention can be widely used in the following fields:

[0168] Solar cells: As a transparent conductive electrode, it improves the photoelectric conversion efficiency of solar cells.

[0169] Optoelectronic devices: used in electronic devices such as displays and touch screens that require high transparency and conductivity.

[0170] Gas sensor: Improve the sensitivity and stability of gas sensors.

[0171] Smart windows: As the core material of smart windows, it provides high light transmittance and electrical conductivity.

[0172] This invention provides a method for improving the optical and electrical properties of SnO2 thin films by doping with novel rare earth elements and optimizing process conditions. This method has the advantages of simple process, low cost, and excellent performance, and has broad application prospects. A detailed analysis is as follows:

[0173] The honeycomb-shaped Pt electrode can improve the sensitivity, stability, selectivity and response speed of the sensor:

[0174] Pt as the upper and lower electrode material of gas sensors has the advantages of high chemical stability, high electrical conductivity, good oxidation resistance, and good compatibility with oxide materials. It can improve the performance and stability of the sensor, is suitable for a variety of gas detection scenarios, and can meet the application requirements of different sensors. The honeycomb structure of Pt electrode has the following advantages:

[0175] Increase surface area: The honeycomb structure can greatly increase the surface area of ​​the electrode, that is, it can provide more active sites, promote the adsorption and reaction of gas molecules, and thus improve the response and sensitivity of the sensor.

[0176] Improved stability: The honeycomb electrode structure increases the surface area of ​​the electrode, disperses the current density through the device, reduces local corrosion of the electrode, and thus increases stability.

[0177] Improve electrode reaction speed: The honeycomb structure has a larger reaction surface area, which can provide higher electron and ion transmission speed, improving the response speed and dynamic performance of the sensor.

[0178] Overall structural effect of the device

[0179] The gas sensor structure design using honeycomb-shaped Pt electrodes for the upper and lower electrodes, La-doped tin oxide as the gas sensitive material, and PI as the substrate has the following excellent performance:

[0180] High sensitivity and fast response: La-doped tin oxide is a commonly used gas-sensing material with excellent gas-sensing properties. Paired with a honeycomb-shaped Pt electrode, it increases the surface area of ​​the gas-sensing material in contact with the gas, improving the sensor's sensitivity to the target gas. Combined with the high electron transfer speed of the honeycomb Pt electrode, the sensor achieves a fast response and can rapidly detect changes in the target gas.

[0181] Stability: The honeycomb-like Pt electrode structure helps to disperse the current density and reduce local corrosion or changes in the electrode, thereby improving the stability and long-term reliability of the sensor.

[0182] Flexible substrate design: Sensors using PI as a substrate are flexible and can adapt to complex shapes or curved surfaces while maintaining stability and performance, which is very useful in some special scenarios.

[0183] In summary, the present invention provides a highly sensitive tin oxide thin film gas sensor and a preparation method thereof. By optimizing the thin film preparation process and device structure, the sensitivity and selectivity of gas detection are significantly improved, and the sensor has broad application prospects.

Claims

1. A method for preparing a highly sensitive rare earth-doped tin oxide thin film, characterized in that: The following steps are involved: Step 1: Select flexible material PI as the electrode substrate and clean it to remove organic matter, particles and other contaminants on the surface; Step 2: Electrodes are prepared on the upper surface of the substrate. Platinum is selected as the electrode material and printed using a micro-nano 3D printer to form an electrode pattern with a thickness of 100 nanometers on the surface. Step 3, preparing a SnO2 precursor solution, dissolving SnCl2·2H2O in anhydrous ethanol water to prepare a 0.8 mol / l solution, adding 0.2 ml of concentrated hydrochloric acid and ethylene glycol as a surfactant to improve the quality of the film, and finally stirring evenly on a magnetic stirrer to obtain a SnO2 precursor solution; Step 4: using ultrasonic spray pyrolysis, the precursor solution is atomized into tiny droplets using an ultrasonic oscillator, and the atomized droplets are transported to the surface of the heated substrate obtained in step 2 by airflow to form a SnO2:La thin film; Step 5: Post-annealing the prepared SnO2:La film to improve the crystallinity and electrical properties of the film; Step 6: Prepare an electrode on the surface of the SnO2:La film. The electrode material is platinum Pt. Print it with a micro-nano 3D printer to form an electrode pattern with a thickness of 100 nanometers on the surface. Step 7: Perform multi-layer packaging processing on the SnO2 thin film gas sensor to obtain a well-packaged sensor.

2. The method for preparing a highly sensitive rare earth-doped tin oxide thin film according to claim 1, characterized in that: Step 1 includes: Step 1.1: Place the substrate in a mixture of acetone, ethanol, and deionized water and clean it using an ultrasonic cleaner for about 10-15 minutes each time. Step 1.2: Rinse the substrate several times with deionized water to remove solvent residues. Step 1.3, immersing the substrate in a diluted 0.5 mol / 1 hydrochloric acid solution and ultrasonically cleaning for 5-10 minutes to remove metal ions and inorganic pollutants on the surface; Step 1.4: Rinse with deionized water to prevent residual acid and alkali from affecting subsequent steps; Step 1.5: Place the substrate in a drying oven, dry it at 60-100° C., and anneal it at 500° C. for 1 hour to remove moisture and organic residues on the surface and improve the cleanliness of the substrate.

3. The method for preparing a highly sensitive rare earth-doped tin oxide thin film according to claim 1, characterized in that: Step 2 includes: Step 2.1, design the desired electrode pattern using computer-aided design software; Step 2.2, fix the prepared substrate on the platform of the 3D printer; Step 2.3: Set parameters such as print head speed, nozzle diameter, and ink flow rate to ensure uniform deposition. Step 2.4: Thermally cure at 150-200° C. for 30-60 minutes to form an electrode.

4. The method for preparing a highly sensitive rare earth-doped tin oxide thin film according to claim 1, characterized in that: Step 3 includes: Step 3.1, dissolve SnCl2·2H2O in anhydrous ethanol water to form a homogeneous solution; Step 3.2: Add 0.2 ml of concentrated hydrochloric acid and 10 ml of ethylene glycol as a surfactant to improve the quality of the film; Step 3.3: Stir the solution evenly on a magnetic stirrer to obtain a SnO2 precursor solution.

5. The method for preparing a highly sensitive rare earth-doped tin oxide thin film according to claim 1, characterized in that: Step 4 includes: Step 4.1, using an ultrasonic oscillator to atomize the precursor solution into tiny droplets; Step 4.2, transporting the atomized droplets to the surface of the heated substrate obtained in step 2 by air flow; Step 4.3: Control the substrate temperature between 300°C and 600°C, and spray for 15 minutes. After the atomized droplets reach the heated substrate surface, they evaporate and decompose rapidly due to the high temperature of the substrate, and a pyrolysis reaction occurs to generate a SnO2:La film.

6. The method for preparing a highly sensitive rare earth-doped tin oxide thin film according to claim 1, characterized in that: Step 5 includes: Step 5.1, placing the prepared SnO2:La film into an annealing furnace; Step 5.2: Anneal at 900°C in a nitrogen atmosphere for 1 hour to control the crystallization quality and microstructure of the film.

7. The method for preparing a highly sensitive rare earth-doped tin oxide thin film according to claim 1, characterized in that: Step 6 includes: Step 6.1, design the desired electrode pattern using computer-aided design software; Step 6.2, fix the prepared SnO:La thin film substrate on the platform of the 3D printer; Step 6.3: Set parameters such as print head speed, nozzle diameter, and ink flow rate to ensure uniform deposition; Step 6.4: Thermally cure at 150-200° C. for 30-60 minutes to form an electrode.

8. The method for preparing a highly sensitive rare earth-doped tin oxide thin film according to claim 1, characterized in that: Step 7 includes: Step 7.1: Deposit a gas permeable membrane on the gas-sensitive film to allow specific gas molecules to pass through and prevent dust and other impurities from entering; Step 7.2: Depositing a corrosion-resistant and high-temperature-resistant protective layer on the gas permeable layer to improve the environmental adaptability and durability of the sensor; Step 7.3: Remove the sample from the reaction chamber, rinse with ethanol and deionized water, and then blow dry with nitrogen to remove any residual chemicals; Step 7.4: High-temperature annealing is performed in an argon environment at 500° C. for 30 minutes to further improve the density and durability of the silicon nitride film.