Calculation method for safe service time of 110H sleeve in chloride ion corrosion environment

By constructing a corrosion rate calculation model for 110H casing in a chloride ion corrosion environment, combined with thick-walled cylinders and thermal stress theory, the problem of the lack of safe service time evaluation in the existing technology is solved, and a fast and accurate safe service time of casing is achieved Calculations and life predictions to ensure wellbore integrity and safe injection and production well operations.

CN118734508APending Publication Date: 2024-10-01PETROCHINA CO LTD
View PDF 0 Cites 0 Cited by

Patent Information

Application Number
CN202310322794.2
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Filing Date
2023-03-30
Publication Date
2024-10-01

AI Technical Summary

Technical Problem

The existing technology lacks a method to calculate the safe use time of 110H casing in a chloride ion corrosion environment, and cannot effectively evaluate the integrity of the casing, which threatens the integrity of the wellbore and the operational safety of injection and production wells.

Method used

By fitting and regressing the corrosion rate of 110H casing at different chloride ion concentrations and temperatures, combined with thick-walled cylinder and thermal stress theory, a corrosion rate calculation model was constructed to calculate the equivalent stress and yield strength of the casing, and quantitatively judge the casing's Safe service time.

Benefits of technology

It can quickly and accurately calculate the safe service time of 110H casing in a chloride ion corrosion environment, determine whether the casing has failed and predict future life, providing a basis for wellbore integrity and injection and production well operation and maintenance.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN118734508A_ABST
    Figure CN118734508A_ABST
Patent Text Reader

Abstract

The invention belongs to the field of oil and gas production, and discloses a method for calculating the safe service time of a 110H casing in a chloride ion corrosion environment, aiming at an injection and production well adopting 110H casing well completion, a corrosion rate calculation model of the 110H casing in the chloride ion corrosion environment is constructed, and a thick-wall cylinder and a thermal stress theory are combined to calculate the safe service time of the 110H casing in the chloride ion corrosion environment. The influence of pressure and temperature of different injection-production working conditions on radial stress, circumferential stress and axial stress of the 110H casing pipe is considered, equivalent stress borne by the 110H casing pipe is further calculated and compared with the yield strength of the equivalent stress, and therefore the safe service time of the 110H casing pipe is calculated. According to the method, the integrity of the 110H casing pipe in the chloride ion corrosion environment and under different injection and production working conditions can be quantitatively judged, the safe service life of the 110H casing pipe can be predicted, and a basis can be provided for shaft integrity and injection and production well operation maintenance.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The invention belongs to the field of oil and gas production, and relates to a method for calculating the safe service time of a 110H casing in a chloride ion corrosion environment. Background Art

[0002] Wellbore integrity is a prerequisite for ensuring safe and smooth oil and gas production. If the wellbore of an injection and production well suffers casing damage and deformation due to factors such as the external formation environment or internal injection and production conditions, the wellbore integrity will inevitably be destroyed, affecting the operation of the injection and production well and even causing major safety accidents.

[0003] In some oil fields, the chloride ion content in shallow formation water is relatively high. For example, in Liaohe Oilfield, the shallow formation water is in the plain group, with a depth of 150-200m and a chloride ion content of about 17400mg / L. When the cement ring of the injection-production well has micro-gaps in the shallow area due to poor cementing quality or formation creep, the casing comes into contact with the shallow formation water. In the chloride ion corrosion environment of the shallow formation water, the casing wall thickness gradually decreases. In addition, under the influence of the pressure and temperature of the injection-production working conditions, the casing is perforated and ruptured, and its safe use time is greatly shortened.

[0004] Currently, there is no method to calculate the safe service life of 110H bushing in a chloride ion corrosion environment, and it is impossible to make a quantitative evaluation of the integrity of the in-service bushing. Summary of the invention

[0005] In order to overcome the shortcomings of the prior art, the present invention forms a calculation method that can calculate the safe service time of 110H casing by fitting and regressing the corrosion rate of 110H casing under different chloride ion concentrations and temperatures through actual indoor experimental fitting, combined with thick-walled tube and thermal stress theory, to provide a basis for wellbore integrity and injection and production well operation and maintenance.

[0006] The present invention aims at the injection-production well completed with 110H casing, constructs a corrosion rate calculation model for the 110H casing in a chloride ion corrosion environment, combines thick-walled tube and thermal stress theory, considers the influence of different injection-production working pressures and temperatures on the radial stress, circumferential stress and axial stress of the 110H casing, further calculates the equivalent stress on the 110H casing and compares it with its yield strength, and calculates the safe service time of the 110H casing. The method can quantitatively judge the integrity of the 110H casing in a chloride ion corrosion environment and different injection-production working conditions and predict its safe service life, and can provide a basis for wellbore integrity and injection-production well operation and maintenance.

[0007] The above object of the present invention is achieved through the following technical solutions:

[0008] 1. Basic assumptions

[0009] (1) The elastic model, Poisson's ratio and other thermophysical parameters in the model system are functions of temperature, and the corresponding functional relationship can be found in the literature;

[0010] 2. Corrosion rate calculation model of 110H casing in chloride ion corrosion environment

[0011]

[0012] Where: cor_sp—corrosion rate of 110H casing in chloride ion corrosion environment, mm / year;

[0013] C(cl - )—chloride ion concentration in the fluid at the position where the casing contacts the fluid, mg / L;

[0014] t—110H The temperature of the casing where it contacts the fluid, °C.

[0015] 3. Calculation ideas

[0016] (1) According to the geological conditions of the injection and production well, the formation position of the shallow formation water (i.e., chloride ion corrosion environment) in contact with the 110H casing is determined, and this position is set as the corrosion core position of the 110H casing.

[0017] (2) Set the unit time node interval ("day", "hour", etc.).

[0018] (3) Set the initial time node.

[0019] (4) According to the chloride ion concentration and temperature at the corrosion core position at this time node, the corrosion rate calculation model of 110H casing in chloride ion corrosion environment is used to calculate the wall thickness corrosion amount and outer radius of the corrosion core position of 110H casing at this time node.

[0020] (5) According to the injection-production conditions of the injection-production well at this time node and the temperature at the core position of the 110H casing corrosion, the elastic modulus, Poisson's ratio, yield strength and other property parameters of the casing and surrounding rock at this time node are calculated. The total radial stress, total circumferential stress and total axial stress at the core position of the 110H casing corrosion at this time node are calculated by applying the thick-walled tube and thermal stress theory.

[0021] (a) The total radial stress is calculated according to formula (2)

[0022] σ r =σ r ′+σ r ″ (2)

[0023] Where: r —Total radial stress at the corrosion core of 110H casing at this time point, MPa;

[0024] σ r ′—Radial stress generated by internal pressure and external extrusion force at the corrosion core position of 110H casing at this time node, MPa;

[0025] σ r ″—Radial stress generated by thermal action at the corrosion core of 110H casing at this time node, MPa;

[0026] Among them, σ r ' is calculated according to formula (3), σ r ” Calculate according to formula (4).

[0027]

[0028] Where: P i —External squeeze force at the corrosion core position of 110H casing at this time node, MPa;

[0029] P o —Internal pressure of the 110H casing corrosion core at this time point, MPa;

[0030] r ci —110H casing inner radius at the corrosion core position at this time point, mm;

[0031] r co —110H casing outer radius at the corrosion core position at this time node, mm;

[0032] r—The average value of the inner and outer radius of the 110H casing at the corrosion core position at this time node, mm.

[0033]

[0034] Where: α c —Linear thermal expansion coefficient of 110H casing at this time node, m / (m·℃);

[0035] E c —Elastic modulus of 110H casing at this time node, MPa;

[0036] u c —Poisson’s ratio of 110H casing at this time point;

[0037] ΔT—the change of the temperature at the core position of the 110H casing corrosion at this time node and the temperature at the initial time node, ℃;

[0038] C c1 —Calculation coefficient, refer to formula (5) for calculation.

[0039]

[0040] Where: E f —Elastic modulus of the surrounding rock at the core position of 110H casing corrosion at this time node, MPa;

[0041] u f —Poisson’s ratio of the surrounding rock at the core position of 110H casing corrosion at this time node;

[0042] (b) The total circumferential stress is calculated according to formula (6)

[0043] σ θ =σ θ ′+σ θ ″ (6)

[0044] Where: θ —Total circumferential stress of the corrosion core of 110H casing at this time point, MPa;

[0045] σ θ ′—circumferential stress generated by internal pressure and external squeeze force at the corrosion core position of 110H casing at this time node, MPa;

[0046] σ θ ″—Circumferential stress generated by heat at the corrosion core of 110H casing at this time node, MPa.

[0047] Among them, σ r ' is calculated according to formula (7), σ r ″ Calculate according to formula (8).

[0048]

[0049]

[0050] (c) The total axial stress is calculated according to formula (9)

[0051] σ z =σ zo +σ zb +σ z ′+σ z ″ (9)

[0052] Where: z —Total axial stress of the corrosion core of 110H casing at this time node, MPa;

[0053] σ zo —The initial axial stress generated by the deadweight and buoyancy of the 110H casing corrosion core at this time point, MPa;

[0054] σ zb —Axial stress generated by pipe bending at the corrosion core of 110H casing at this time point, MPa;

[0055] σ z ′—Axial stress generated by internal pressure and external squeeze force at the corrosion core position of 110H casing at this time node, MPa;

[0056] σ z ″—Axial stress generated by thermal action at the corrosion core of 110H casing at this time node, MPa.

[0057] Among them, σ zo Refer to formula (10) to calculate, σ zb According to formula (11), σ z ' is calculated according to formula (12), σ z ” Calculate according to formula (13).

[0058] σ zo =(ρ c l c -ρ l l l )g·10 -6 (10)

[0059] Where: c —Density of 110H casing, kg / m 3 ;

[0060] ρ l —Drilling mud density, kg / m 3 ;

[0061] l c —110H casing length from the core position of casing corrosion to the bottom of the well, m;

[0062] l l —Casing length from the top of the drilling mud to the bottom of the well when the well is completed, m

[0063] g—acceleration due to gravity, take 9.8N / kg.

[0064] σ zb =0.060156D leg d is (11)

[0065] Where: D leg —110H casing curvature at the corrosion core, ° / 30m;

[0066] d is—Nominal inner diameter of 110H casing body, mm.

[0067] σ z ′=u c (σ r ′+σ θ ′) (12)

[0068]

[0069] (6) Calculate the equivalent stress on the corrosion core of the 110H casing at this time point. The equivalent stress is calculated according to formula (14).

[0070]

[0071] Where: equ —Equivalent stress on the corrosion core of 110H casing at this time point, MPa.

[0072] (7) Determine the equivalent stress and yield strength of the 110H bushing at this time node. If the equivalent stress is less than the yield strength, the bushing has not failed and the calculation proceeds to the next time node. If the equivalent stress is greater than the yield strength, the bushing is considered to have failed and the calculation ends.

[0073] (8) The product of the cumulative number of nodes from the initial time node to the end of the calculation and the unit time node interval is the safe service time of the 110H bushing.

[0074] The beneficial effects of the present invention compared with the prior art are:

[0075] The calculation method involved in the present invention has high field applicability. Through this method, the safe service time of 110H casing in a chloride ion corrosion environment and under different injection and production conditions can be quickly and accurately calculated, and it can determine whether the 110H casing is currently invalid and predict the future service life, providing a basis for wellbore integrity and injection and production well operation and maintenance. BRIEF DESCRIPTION OF THE DRAWINGS

[0076] In order to more clearly illustrate the technical solutions of the embodiments of the present invention, the following is a brief introduction to the drawings used in the embodiments. Obviously, the drawings listed below are only some embodiments of the present invention. For ordinary technicians in this field, other drawings can be obtained based on these drawings without creative work.

[0077] Figure 1 This is a flow chart for calculating the safe service time of 110H casing in a chloride ion corrosion environment. DETAILED DESCRIPTION

[0078] In order to make the objectives, technical solutions and advantages of the present invention more clear, the following will further describe the implementation methods of the present invention in detail with reference to the accompanying drawings.

[0079] Example 1

[0080] Combination Figure 1 The specific implementation methods of this patent are described in detail.

[0081] 1. Data preparation:

[0082] Initial outer radius, inner radius, and wall thickness of 110H casing; linear thermal expansion coefficient, elastic modulus, Poisson's ratio, and yield strength (as a function of temperature) of 110H casing; elastic modulus and Poisson's ratio (as a function of temperature) of the surrounding rock of 110H casing, etc.

[0083] 2. Calculation steps:

[0084] (1) According to the geological conditions of the injection and production well, the formation position of the shallow formation water (i.e., chloride ion corrosion environment) in contact with the 110H casing is determined, and this position is set as the corrosion core position of the 110H casing.

[0085] (2) Set the unit time node interval ("day", "hour", etc.).

[0086] (3) Set the initial time node i.

[0087] (4) According to the chloride ion concentration and temperature at the corrosion core position of the 110H casing at this time node, the wall thickness corrosion amount and outer radius at the corrosion core position of the 110H casing at this time node are calculated using formula (1).

[0088] (5) According to the temperature of the core position of the 110H casing corrosion at this time node, the elastic modulus, Poisson's ratio, yield strength and other attribute parameters of the casing and surrounding rock at this time node are calculated.

[0089] (6) Use formulas (2), (3), (4), and (5) to calculate the total radial stress at the corrosion core position of the 110H casing at this time node.

[0090] (7) The total circumferential stress at the corrosion core position of the 110H casing at this time node is calculated using formulas (6), (7), (8), and (5).

[0091] (8) The total axial stress at the corrosion core position of the 110H casing at this time node is calculated using formulas (9), (10), (11), (12), (13), and (5).

[0092] (9) Formula (14) is used to calculate the equivalent stress of the corrosion core position of the 110H casing at this time node.

[0093] (10) Determine whether the equivalent stress of the 110H casing corrosion core position at this time node is greater than the yield strength. If not, proceed to the calculation of the next time node and return to step (4); if yes, execute step (11).

[0094] (11) After the calculation is completed, the product of the cumulative number of nodes and the node interval per unit time is the safe service time of the 110H bushing.

[0095] The above-described embodiments are only preferred embodiments of the present invention, but not all feasible embodiments of the present invention. For those skilled in the art, any obvious changes made thereto without departing from the principles and spirit of the present invention should be considered to be included in the scope of protection of the claims of the present invention.

Claims

1. A method for calculating the safe service time of a 110H casing in a chloride ion corrosion environment, characterized in that: The following steps are involved: ① According to the geological conditions of the injection and production wells, determine the shallow formation water in contact with the 110H casing, that is, the formation position of the chloride ion corrosion environment, and set this position as the corrosion core position of the 110H casing; ②Set the unit time node interval; ③Set the initial time node; ④ According to the chloride ion concentration and temperature at the corrosion core position at this time node, the corrosion rate calculation model of 110H casing in chloride ion corrosion environment is used to calculate the wall thickness corrosion amount and outer radius of the corrosion core position of 110H casing at this time node; ⑤ According to the injection and production conditions of the injection and production well at this time node and the temperature at the core position of the 110H casing corrosion, the elastic modulus, Poisson's ratio and yield strength of the casing and surrounding rock at this time node are calculated. The total radial stress, total circumferential stress and total axial stress of the core position of the 110H casing corrosion at this time node are calculated by using the thick-walled tube and thermal stress theory; ⑥ Calculate the equivalent stress on the corrosion core position of the 110H casing at this time node; ⑦ Determine the equivalent stress and yield strength of 110H casing at this time point; ⑧The product of the cumulative number of nodes from the initial time node to the end of the calculation and the unit time node interval is the safe service time of the 110H bushing.

2. A method for calculating the safe service time of a 110H casing in a chloride ion corrosion environment, characterized in that: The unit time node interval in step ② is "day" or "hour".

3. A method for calculating the safe service time of a 110H casing in a chloride ion corrosion environment, characterized in that: The corrosion rate calculation model in step ④ is: Where: cor_sp—corrosion rate of 110H casing in chloride ion corrosion environment, mm / year; C(cl - )—chloride ion concentration in the fluid at the position where the casing contacts the fluid, mg / L; t—110H The temperature of the casing where it contacts the fluid, °C.

4. A method for calculating the safe service time of a 110H casing in a chloride ion corrosion environment, characterized in that: The elastic modulus, Poisson's ratio and yield strength at the time node described in step ⑤ can be calculated by searching the corresponding functional relationship in the literature.

5. A method for calculating the safe service time of a 110H casing in a chloride ion corrosion environment, characterized in that: The total radial stress in step ⑤ is calculated according to formula (2): s r =s r ′+σ r ″ (2) Where: r —Total radial stress at the corrosion core of 110H casing at this time node, MPa; σ r ′—Radial stress generated by internal pressure and external extrusion force at the corrosion core position of 110H casing at this time node, MPa; σ r ″—Radial stress generated by thermal action at the corrosion core of 110H casing at this time node, MPa; Among them, σ r ' is calculated according to formula (3), σ r ″ Calculate according to formula (4); Where: P i —External squeeze force at the corrosion core position of 110H casing at this time node, MPa; P o —Internal pressure of the 110H casing corrosion core at this time point, MPa; r ci —110H casing inner radius at the corrosion core position at this time point, mm; r co —110H casing outer radius at the corrosion core position at this time node, mm; r—average value of the inner and outer radius of the 110H casing at the corrosion core position at this time node, mm; Where: α c —Linear thermal expansion coefficient of 110H casing at this time node, m / (m·℃); E c —Elastic modulus of 110H casing at this time node, MPa; u c —Poisson’s ratio of 110H casing at this time point; ΔT—the change of the temperature at the core position of the 110H casing corrosion at this time node and the temperature at the initial time node, ℃; C c1 —Calculation coefficient, calculated according to formula (5); Where: E f —Elastic modulus of the surrounding rock at the core position of 110H casing corrosion at this time node, MPa; u f —Poisson’s ratio of the surrounding rock at the core position of 110H casing corrosion at this time node.

6. A method for calculating the safe service time of a 110H casing in a chloride ion corrosion environment, characterized in that: The total circumferential stress in step ⑤ is calculated according to formula (6) s θ =s θ ′+σ θ ″ (6) Where: θ —Total circumferential stress of the corrosion core of 110H casing at this time point, MPa; σ θ ′—circumferential stress generated by internal pressure and external squeeze force at the corrosion core position of 110H casing at this time node, MPa; σ θ ″—circumferential stress generated by thermal action at the corrosion core of 110H casing at this time node, MPa; Among them, σ r ' is calculated according to formula (7), σ r ″ Calculate according to formula (8); (c) The total axial stress is calculated according to formula (9) s z =s zo +s zb +s z ′+σ z ″ (9) Where: z —Total axial stress of the corrosion core of 110H casing at this time node, MPa; σ zo —The initial axial stress generated by the deadweight and buoyancy of the 110H casing corrosion core at this time point, MPa; σ zb —Axial stress generated by pipe bending at the corrosion core of 110H casing at this time point, MPa; σ z ′—Axial stress generated by internal pressure and external squeeze force at the corrosion core position of 110H casing at this time node, MPa; σ z ″—Axial stress generated by thermal action at the corrosion core of 110H casing at this time node, MPa; Among them, σ zo Refer to formula (10) to calculate, σ zb According to formula (11), σ z ' is calculated according to formula (12), σ z ″ Calculate according to formula (13); s zo =(ρ c l c -r l l l )g·10 -6 (10) Where: c —Density of 110H casing, kg / m 3 ; ρ l —Drilling mud density, kg / m 3 ; l c —110H casing length from the core position of casing corrosion to the bottom of the well, m; l l —Casing length from the top of the drilling mud to the bottom of the well when the well is completed, m g—gravitational acceleration, taken as 9.8N / kg; s zb =0.060156D leg d is (11) Where: D leg —110H casing curvature at the corrosion core, ° / 30m; d is —Nominal inner diameter of 110H casing body, mm s z ′=u c (s r ′+σ θ ′) (12) 7. A method for calculating the safe service time of a 110H casing in a chloride ion corrosion environment, characterized in that: The equivalent stress in step ⑤ is calculated according to formula (14): Where: equ —Equivalent stress on the corrosion core of 110H casing at this time point, MPa.

8. A method for calculating the safe service time of a 110H casing in a chloride ion corrosion environment, characterized in that: The result of the judgment in step ⑦ is divided into two cases: if the equivalent stress is less than the yield strength, the casing has not failed and the calculation proceeds to the next time node; if the equivalent stress is greater than the yield strength, the casing is considered to have failed and the calculation ends.