Calculation method for safe use time of 130TT casing pipe
By constructing a corrosion rate calculation model and thermal stress theory for 130TT casing in a chloride ion corrosion environment, and calculating its equivalent stress and yield strength, it solves the problem of difficulty in evaluating the safe use time of casing in the existing technology and achieves rapid and accurate The safe use time judgment and service life prediction provide a basis for the integrity of the wellbore and the operation of injection and production wells.
Patent Information
- Application Number
- CN202310324218.1
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Filing Date
- 2023-03-30
- Publication Date
- 2024-10-01
AI Technical Summary
The existing technology lacks a method to calculate the safe use time of 130TT casing in a chloride ion corrosion environment, and cannot effectively evaluate the integrity of the casing, which threatens the integrity of the wellbore and the operational safety of injection and production wells.
Construct a corrosion rate calculation model for 130TT casing in a chloride ion corrosion environment. Combined with thick-walled cylinders and thermal stress theory, the equivalent stress and yield strength of the casing are calculated to determine its safe use time.
It can quickly and accurately calculate the safe use time of 130TT casing in a chloride ion corrosion environment, judge the integrity of the casing and predict its service life, providing a basis for the integrity of the wellbore and the operation and maintenance of injection and production wells.
Smart Images

Figure CN118734510A_ABST
Abstract
Description
Technical Field
[0001] The invention belongs to the field of oil and gas production and relates to a method for calculating the safe service life of a 130TT casing. Background Art
[0002] Wellbore integrity is a prerequisite for ensuring safe and smooth oil and gas production. If the wellbore of an injection and production well suffers casing damage and deformation due to factors such as the external formation environment or internal injection and production conditions, it will inevitably destroy the wellbore integrity, affect the operation of the injection and production well, and even cause major safety accidents.
[0003] In some oilfields, shallow formation water contains high levels of chloride ions. For example, in the Liaohe Oilfield, the shallow formation water is located in the Plain Formation at a depth of 150-200 meters, with a chloride ion content of approximately 17,400 mg / L. When micro-gaps develop in the cement sheath of an injection-production well due to poor cementing quality or formation creep, the casing comes into contact with the shallow formation water. In the chloride-corrosive environment of the shallow formation water, the casing wall thickness gradually decreases. Combined with the pressure and temperature of the injection-production conditions, the casing can be perforated and ruptured, significantly shortening its safe service life.
[0004] Currently, there is no method to calculate the safe service life of 130TT casing in a chloride ion corrosion environment, making it impossible to make a quantitative evaluation of the integrity of the in-service casing. Summary of the Invention
[0005] In order to solve the problems existing in the prior art, the present invention aims at injection-production wells completed with 130TT casing, constructs a corrosion rate calculation model for 130TT casing in a chloride ion corrosion environment, combines thick-walled tube and thermal stress theory, considers the influence of different injection-production working pressures and temperatures on the radial stress, circumferential stress and axial stress of the 130TT casing, further calculates the equivalent stress on the 130TT casing and compares it with its yield strength, and calculates the safe service life of the 130TT casing. This method can quantitatively judge the integrity of the 130TT casing in a chloride ion corrosion environment and different injection-production working conditions and predict its safe service life, which can provide a basis for wellbore integrity and injection-production well operation and maintenance.
[0006] The above-mentioned object of the present invention is achieved through the following technical solutions:
[0007] 1. Basic Assumptions
[0008] (1) The elastic model, Poisson's ratio and other thermophysical parameters in the model system are functions of temperature, and the corresponding functional relationships can be found in the literature;
[0009] 2. Corrosion rate calculation model of 130TT casing in chloride ion corrosion environment
[0010]
[0011] Where: cor_sp—corrosion rate of 130TT casing in chloride ion corrosion environment, mm / year;
[0012] C(cl - )—chloride ion concentration in the fluid at the position where the casing contacts the fluid, mg / L;
[0013] t—Temperature of the 130TT casing where it contacts the fluid, °C.
[0014] 3. Calculation ideas
[0015] (1) According to the geological conditions of the injection and production well, the formation position of the shallow formation water (i.e., chloride ion corrosion environment) in contact with the 130TT casing is determined, and this position is set as the corrosion core position of the 130TT casing.
[0016] (2) Set the unit time node interval ("day", "hour", etc.).
[0017] (3) Set the initial time node.
[0018] (4) According to the chloride ion concentration and temperature at the corrosion core position at this time node, the corrosion rate calculation model of 130TT casing in chloride ion corrosion environment is used to calculate the wall thickness corrosion amount and outer radius of the corrosion core position of 130TT casing at this time node.
[0019] (5) According to the injection and production conditions of the injection and production well at this time node and the temperature at the core position of the 130TT casing corrosion, the elastic modulus, Poisson's ratio, yield strength and other attribute parameters of the casing and surrounding rock at this time node are calculated. The thick-walled tube and thermal stress theory are applied to calculate the total radial stress, total circumferential stress and total axial stress at the core position of the 130TT casing corrosion at this time node.
[0020] (a) The total radial stress is calculated according to formula (2)
[0021] σ r =σ r ′+σ r ″ (2)
[0022] Where: σ r —Total radial stress at the corrosion core of 130TT casing at this time point, MPa;
[0023] σ r ′—Radial stress generated by internal pressure and external extrusion force at the corrosion core of 130TT casing at this time point, MPa;
[0024] σ r″—Radial stress generated by thermal action at the corrosion core of 130TT casing at this time point, MPa;
[0025] Among them, σ r ′ is calculated according to formula (3), σ r Calculate according to formula (4).
[0026]
[0027] Where: P i —External squeeze force at the corrosion core of 130TT casing at this time point, MPa;
[0028] P o —Internal pressure of the 130TT casing corrosion core at this time point, MPa;
[0029] r ci —Inner radius of the 130TT casing at the corrosion core position at this time point, mm;
[0030] r co —The outer radius of the 130TT casing at the corrosion core position at this time point, mm;
[0031] r—The average value of the inner and outer radius of the 130TT casing at the corrosion core position at this time point, mm.
[0032]
[0033] Where: α c —Linear thermal expansion coefficient of 130TT casing at this time point, m / (m·℃);
[0034] E c —Elastic modulus of 130TT casing at this time point, MPa;
[0035] u c —Poisson’s ratio of 130TT casing at this time point;
[0036] ΔT—the change in temperature of the corrosion core position of the 130TT casing at this time node compared to the temperature at the initial time node, ℃;
[0037] C c1 —Calculation coefficient, refer to formula (5).
[0038]
[0039] Where: E f —Elastic modulus of the surrounding rock at the core location of 130TT casing corrosion at this time point, MPa;
[0040] u f —Poisson’s ratio of the surrounding rock at the core location of 130TT casing corrosion at this time point;
[0041] (b) The total circumferential stress is calculated according to formula (6)
[0042] σ θ =σ θ ′+σ θ ″ (6)
[0043] Where: σ θ —Total circumferential stress of the corrosion core of 130TT casing at this time point, MPa;
[0044] σ θ ′—Circumferential stress generated by internal pressure and external extrusion force at the corrosion core of 130TT casing at this time point, MPa;
[0045] σ θ ″—Circumferential stress generated by thermal action at the corrosion core of 130TT casing at this time point, MPa.
[0046] Among them, σ r ' is calculated according to formula (7), σ r Calculate according to formula (8).
[0047]
[0048]
[0049] (c) The total axial stress is calculated according to formula (9)
[0050] σ z =σ zo +σ zb +σ z ′+σ z ″ (9)
[0051] Where: σ z —Total axial stress at the corrosion core of 130TT casing at this time point, MPa;
[0052] σ zo —The initial axial stress generated by the deadweight and buoyancy of the 130TT casing corrosion core at this time point, MPa;
[0053] σ zb —Axial stress generated by tubing bending at the corrosion core of 130TT casing at this time point, MPa;
[0054] σz ′—Axial stress generated by internal pressure and external extrusion force at the corrosion core of 130TT casing at this time point, MPa;
[0055] σ z ″—Axial stress generated by thermal action at the corrosion core of 130TT casing at this time point, MPa.
[0056] Among them, σ zo Refer to formula (10) to calculate, σ zb Calculate according to formula (11), σ z ' is calculated according to formula (12), σ z Calculate according to formula (13).
[0057] σ zo =(ρ c l c -ρ l l l )g·10 -6 (10)
[0058] Where: ρ c —Density of 130TT casing, kg / m 3 ;
[0059] ρ l —Drilling mud density, kg / m 3 ;
[0060] l c —130TT casing length from the corrosion core to the bottom of the well, m;
[0061] l l —Casing length from the top of the drilling mud to the bottom of the well when the well is completed, m
[0062] g—acceleration due to gravity, taken as 9.8N / kg.
[0063] σ zb =0.060156D leg d is (11)
[0064] Where: D leg —130TT casing curvature at the corrosion core, ° / 30m;
[0065] d is —Nominal inner diameter of 130TT casing body, mm.
[0066] σ z ′=u c (σ r ′+σ θ′) (12)
[0067]
[0068] (6) Calculate the equivalent stress on the corrosion core of the 130TT casing at this time point. The equivalent stress is calculated according to formula (14).
[0069]
[0070] Where: σ equ —Equivalent stress on the corrosion core of 130TT casing at this time point, MPa.
[0071] (7) Determine the equivalent stress and yield strength of the 130TT casing at this time node. If the equivalent stress is less than the yield strength, the casing has not failed and the calculation proceeds to the next time node; if the equivalent stress is greater than the yield strength, the casing is considered to have failed and the calculation ends.
[0072] (8) The product of the cumulative number of nodes from the initial time node to the end of the calculation and the unit time node interval is the safe use time of the 130TT casing.
[0073] The beneficial effects of the present invention compared with the prior art are:
[0074] The calculation method involved in the present invention has high field applicability. Through this method, the safe service life of 130TT casing in a chloride ion corrosion environment and different injection and production conditions can be quickly and accurately calculated. It can also determine whether the 130TT casing is currently invalid and predict its future service life, providing a basis for wellbore integrity and injection and production well operation and maintenance. BRIEF DESCRIPTION OF THE DRAWINGS
[0075] In order to more clearly illustrate the technical solutions of the embodiments of the present invention, the following is a brief introduction to the drawings used in the embodiments. Obviously, the drawings listed below are only some embodiments of the present invention. For ordinary technicians in this field, other drawings can be obtained based on these drawings without paying any creative work.
[0076] Figure 1 This is a flow chart for calculating the safe service life of 130TT casing in a chloride ion corrosion environment. DETAILED DESCRIPTION
[0078] To make the objectives, technical solutions and advantages of the present invention more clear, the embodiments of the present invention will be described in further detail below with reference to the accompanying drawings.
[0079] Example 1
[0080] Combine Figure 1 Specific embodiments of the present invention will be described in detail.
[0081] 1. Data preparation:
[0082] Initial outer radius, inner radius, and wall thickness of the 130TT casing; linear thermal expansion coefficient, elastic modulus, Poisson's ratio, and yield strength of the 130TT casing (as a function of temperature); elastic modulus and Poisson's ratio of the surrounding rock of the 130TT casing (as a function of temperature), etc.
[0083] 2. Calculation steps:
[0084] (1) According to the geological conditions of the injection and production well, the formation position of the shallow formation water (i.e., chloride ion corrosion environment) in contact with the 130TT casing is determined, and this position is set as the corrosion core position of the 130TT casing.
[0085] (2) Set the unit time node interval ("day", "hour", etc.).
[0086] (3) Set the initial time node i.
[0087] (4) According to the chloride ion concentration and temperature at the corrosion core position of the 130TT casing at the time node, the wall thickness corrosion amount and outer radius at the corrosion core position of the 130TT casing at the time node are calculated using formula (1).
[0088] (5) According to the temperature of the corrosion core position of the 130TT casing at the time node, the elastic modulus, Poisson's ratio, yield strength and other attribute parameters of the casing and surrounding rock at the time node are calculated.
[0089] (6) Use formulas (2), (3), (4), and (5) to calculate the total radial stress at the corrosion core position of the 130TT casing at this time node.
[0090] (7) Use formulas (6), (7), (8), and (5) to calculate the total circumferential stress at the corrosion core position of the 130TT casing at this time node.
[0091] (8) Use formulas (9), (10), (11), (12), (13), and (5) to calculate the total axial stress at the corrosion core position of the 130TT casing at this time node.
[0092] (9) Use formula (14) to calculate the equivalent stress of the corrosion core position of the 130TT casing at this time node.
[0093] (10) Determine whether the equivalent stress at the corrosion core of the 130TT casing at this time node is greater than the yield strength. If not, proceed to the calculation of the next time node and return to step (4); if so, proceed to step (11).
[0094] (11) After the calculation is completed, the product of the cumulative number of nodes and the node interval per unit time is the safe use time of the 130TT casing.
[0095] The above-described embodiments are only preferred embodiments of the present invention, and are not intended to be all feasible embodiments of the present invention. Any obvious modifications made by a person skilled in the art without departing from the principles and spirit of the present invention should be considered to be included within the scope of protection of the claims of the present invention.
Claims
1. A method for calculating the safe use time of a 130TT casing, characterized in that: Use in a chloride ion corrosive environment, including the following steps: ① According to the geological conditions of the injection and production wells, determine the shallow formation water in contact with the 130TT casing, that is, the formation position of the chloride ion corrosion environment, and set this position as the corrosion core position of the 130TT casing; ②Set the unit time node interval; ③Set the initial time node i; ④ According to the chloride ion concentration and temperature at the corrosion core position of the 130TT casing at the time node, the wall thickness corrosion amount and outer radius at the corrosion core position of the 130TT casing at the time node are calculated using formula (1); ⑤ According to the temperature of the 130TT casing corrosion core position at this time node, calculate the elastic modulus, Poisson's ratio, yield strength and other attribute parameters of the casing and surrounding rock at this time node; ⑥ Use formulas (2), (3), (4), and (5) to calculate the total radial stress at the corrosion core of the 130TT casing at this time node; ⑦ Use formulas (6), (7), (8), and (5) to calculate the total circumferential stress at the corrosion core position of the 130TT casing at this time node; ⑧Use formulas (9), (10), (11), (12), (13), and (5) to calculate the total axial stress at the corrosion core position of the 130TT casing at this time node; ⑨Use formula (14) to calculate the equivalent stress of the corrosion core position of 130TT casing at this time node; ⑩ Determine whether the equivalent stress at the corrosion core position of the 130TT casing at this time node is greater than the yield strength. If not, proceed to the calculation of the next time node and return to step ④; if yes, execute step At the end of the calculation, the product of the cumulative number of nodes and the node interval per unit time is the safe use time of the 130TT casing.
2. A method for calculating the safe use time of a 130TT casing as claimed in claim 1, characterized in that: The unit time node interval in step ② is "day" or "hour".
3. A method for calculating the safe use time of a 130TT casing as claimed in claim 1, characterized in that: The formula (1) in step ④ is Where: cor_sp—corrosion rate of 130TT casing in chloride ion corrosion environment, mm / year; C(cl - )—chloride ion concentration in the fluid at the position where the casing contacts the fluid, mg / L; t—Temperature of the 130TT casing where it contacts the fluid, °C.
4. A method for calculating the safe use time of a 130TT casing as claimed in claim 1, characterized in that: The formulas (2), (3), (4) and (5) in step ⑥ are respectively: The total radial stress is calculated according to formula (2) s r =s r ′+σ r ″ (2) Where: r —Total radial stress at the corrosion core of 130TT casing at this time node, MPa; σ r ′—Radial stress generated by internal pressure and external extrusion force at the corrosion core position of 130TT casing at this time node, MPa; σ r ″—Radial stress generated by thermal action at the corrosion core of 130TT casing at this time node, MPa; Among them, σ r ' is calculated according to formula (3), σ r ″ Calculate according to formula (4), Where: P i —External squeeze force at the corrosion core of 130TT casing at this time point, MPa; P o —Internal pressure of the 130TT casing corrosion core at this time point, MPa; r ci —Inner radius of the 130TT casing at the corrosion core position at this time point, mm; r co —130TT casing outer radius at the corrosion core position at this time node, mm; r—average value of the inner and outer radius of the 130TT casing at the corrosion core position at this time node, mm, Where: α c —Linear thermal expansion coefficient of 130TT casing at this time node, m / (m·℃); E c —Elastic modulus of 130TT casing at this time node, MPa; u c —Poisson’s ratio of 130TT casing at this time point; ΔT—the change of the temperature at the corrosion core position of 130TT casing at this time node and the temperature at the initial time node, ℃; C c1 —Calculation coefficient, refer to formula (5), Where: E f —Elastic modulus of the surrounding rock at the core position of 130TT casing corrosion at this time node, MPa; u f —Poisson’s ratio of the surrounding rock at the core position of 130TT casing corrosion at this time node.
5. A method for calculating the safe use time of a 130TT casing as claimed in claim 1, characterized in that: The formulas (6), (7) and (8) in step ⑦ are respectively: The total circumferential stress is calculated according to formula (6) s θ =s θ ′+σ θ ″ (6) Where: θ —Total circumferential stress of the corrosion core of 130TT casing at this time point, MPa; σ θ ′—circumferential stress generated by internal pressure and external squeeze force at the corrosion core position of 130TT casing at this time node, MPa; σ θ ″—Circumferential stress generated by heat at the corrosion core of 130TT casing at this time node, MPa, Among them, σ′ r According to formula (7), σ r ″ Calculate according to formula (8), 6. A method for calculating the safe use time of a 130TT casing as claimed in claim 1, characterized in that: The formulas (9), (10), (11), (12), and (13) in step ⑧ are respectively: The total axial stress is calculated according to formula (9) s z =s zo +s zb +s z ′+σ z ″ (9) Where: z —Total axial stress of the corrosion core of 130TT casing at this time point, MPa; σ zo —The initial axial stress generated by the deadweight and buoyancy of the 130TT casing corrosion core at this time point, MPa; σ zb —Axial stress generated by the bending of the pipe string at the corrosion core position of 130TT casing at this time node, MPa; σ z ′—Axial stress generated by internal pressure and external squeeze force at the corrosion core position of 130TT casing at this time node, MPa; σ z ″—Axial stress generated by heat at the corrosion core of 130TT casing at this time node, MPa, Among them, σ zo Refer to formula (10) to calculate, σ zb According to formula (11), σ z ′ According to formula (12), σ z ″ Calculate according to formula (13), s zo =(ρ c l c -r l l l )g·10 -6 (10) Where: c —Density of 130TT casing, kg / m 3 ; ρ l —Drilling mud density, kg / m 3 ; l c —130TT casing length from the corrosion core position to the bottom of the well, m; l l —Casing length from the top of the drilling mud to the bottom of the well when the well is completed, m g—gravitational acceleration, take 9.8N / kg, s zb =0.060156D leg d is (11) Where: D leg —130TT casing curvature at the corrosion core, ° / 30m; d is —Nominal inner diameter of 130TT casing body, mm, s z ′=u c (s r ′+σ θ ′) (12) 7. A method for calculating the safe use time of a 130TT casing as claimed in claim 1, characterized in that: The formula (14) in step ⑨ is: The equivalent stress is calculated according to formula (14): Where: equ —The equivalent stress on the corrosion core of 130TT casing at this time point, MPa.
Citation Information
Cited By
Method for predicting service life cycle of over-well inclined well cementation casing
CN120745265A