Light-transmitting conductive sheet
By designing the thickness ratio of the crystalline and amorphous regions in the translucent conductive layer, and arranging and crystallizing it through sputtering, the problems of reduced resistivity and reduced bending caused by the increase in thickness of the translucent conductive layer are solved. , achieving both low resistivity and excellent bending properties.
Patent Information
- Application Number
- CN202410371856.3
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Priority Date
- 2023-03-30
- Filing Date
- 2024-03-29
- Publication Date
- 2024-10-01
- Estimated Expiration
- Not applicable · inactive patent
AI Technical Summary
When the existing light-transmitting conductive layer is thickened, the resistivity decreases but the flexibility decreases, leading to undesirable conditions.
Design a light-transmitting conductive sheet. The light-transmitting conductive layer includes a first region that is mainly crystalline and a second region that is mainly amorphous in order toward the thickness direction. The thickness of the second region is smaller than that of the first region. The regions are thicker, configured by sputtering and crystallized to achieve low resistivity and excellent bendability.
It is possible to optimize the bendability while maintaining low resistivity, and avoid the problem of reduced bendability caused by the increase in the thickness of the light-transmissive conductive layer.
Smart Images

Figure CN118737528A_ABST
Abstract
Description
Technical Field
[0001] The present invention relates to a light-transmitting conductive sheet. Background Art
[0002] Conventionally, a light-transmitting conductive sheet including a substrate and a light-transmitting conductive layer in this order has been known. Such a light-transmitting conductive sheet is suitable for use in various devices (for example, a touch sensor).
[0003] As such a light-transmitting conductive sheet, for example, a light-transmitting conductive sheet has been proposed which includes a resin layer and a light-transmitting conductive layer in sequence toward one side in the thickness direction, and the light-transmitting conductive layer includes an amorphous first region and a crystalline second region in sequence toward one side in the thickness direction (for example, refer to Patent Document 1).
[0004] Existing patent literature
[0005] Patent Literature
[0006] Patent Document 1: Handbook of International Publication No. 2021 / 241118 Summary of the invention
[0007] Problem that the invention aims to solve
[0008] On the other hand, the light-transmitting conductive layer is required to have a lower resistivity. From the viewpoint of reducing the resistivity, increasing the thickness of the light-transmitting conductive layer has been studied. However, increasing the thickness of the light-transmitting conductive layer has the disadvantage of reduced bendability.
[0009] The present invention provides a light-transmitting conductive sheet having low resistivity and excellent bendability.
[0010] Solutions for solving problems
[0011] The present invention [1] is a translucent conductive sheet, which comprises a substrate layer and a translucent conductive layer in sequence on one side in the thickness direction, wherein the translucent conductive layer comprises a first region and a second region in sequence on one side in the thickness direction, wherein a main region of the first region is crystalline, and a main region of the second region is amorphous.
[0012] The present invention [2] comprises the light-transmitting conductive sheet according to the above [1], wherein the thickness of the second region is thicker than the thickness of the first region.
[0013] Effects of the Invention
[0014] The light-transmitting conductive sheet of the present invention has a base material layer and a light-transmitting conductive layer in sequence toward one side in the thickness direction. In addition, in the light-transmitting conductive sheet, the light-transmitting conductive layer has a first region whose main region is crystalline and a second region whose main region is amorphous in sequence toward one side in the thickness direction. Therefore, it has a low resistivity and excellent bendability. BRIEF DESCRIPTION OF THE DRAWINGS
[0015] Figure 1 One embodiment of the light-transmitting conductive sheet of the present invention is shown.
[0016] Figure 2 middle, Figure 2 A~ Figure 2 D represents one embodiment of the method for producing a light-transmitting conductive sheet. Figure 2 A in the figure represents a step of preparing a substrate in the first step. Figure 2 B represents a step of disposing a cured resin layer on one surface in the thickness direction of the substrate in the first step. Figure 2 C represents a third step of disposing the first region on one surface in the thickness direction of the base material layer in the second step. Figure 2 D represents a fourth step of configuring the second region on one surface in the thickness direction of the first region in the second step.
[0017] Description of Reference Numerals
[0018] 1 Translucent conductive sheet
[0019] 2. Substrate layer
[0020] 31 Area 1
[0021] 32 Area 2 DETAILED DESCRIPTION
[0022] refer to Figure 1 , an embodiment of the light-transmitting conductive sheet of the present invention is described.
[0023] Figure 1 In the figure, the up-down direction of the paper is the up-down direction (thickness direction). In addition, the upper side of the paper is the upper side (one side in the thickness direction). In addition, the lower side of the paper is the lower side (the other side in the thickness direction). In addition, the left-right direction of the paper and the depth direction are the surface directions orthogonal to the up-down direction. Specifically, the directions of each figure are based on the arrows.
[0024] The light-transmitting conductive sheet 1 has a film shape (including a sheet shape) having a predetermined thickness. The light-transmitting conductive sheet 1 extends in a plane direction perpendicular to the thickness direction. The light-transmitting conductive sheet 1 has a flat upper surface and a flat lower surface. The light-transmitting conductive sheet 1 is preferably flexible.
[0025] like Figure 1As shown in , the light-transmitting conductive sheet 1 includes a substrate layer 2 and a light-transmitting conductive layer 3 disposed on one side in the thickness direction of the substrate layer 2. Specifically, the light-transmitting conductive sheet 1 includes a substrate layer 2 and a light-transmitting conductive layer 3 disposed directly on the upper surface (one side in the thickness direction) of the substrate layer 2. The light-transmitting conductive sheet 1 preferably includes a substrate layer 2 and a light-transmitting conductive layer 3.
[0026] The thickness of the light-transmitting conductive sheet 1 is, for example, 400 μm or less, or preferably 200 μm or less, and, for example, 1 μm or more, or preferably 5 μm or more.
[0027] <Base material layer>
[0028] The base layer 2 has a film shape. The base layer 2 is preferably flexible. The base layer 2 is disposed on the entire lower surface of the light-transmitting conductive layer 3 so as to contact the lower surface of the light-transmitting conductive layer 3. The base layer 2 is the lowermost layer of the light-transmitting conductive sheet 1.
[0029] The base material layer 2 includes a base material 11 and a cured resin layer 12 disposed on one side in the thickness direction of the base material 11 .
[0030] [Base material]
[0031] The substrate 11 is disposed on the entire lower surface of the cured resin layer 12 so as to contact the lower surface of the cured resin layer 12. The substrate 11 is the lowermost layer of the light-transmitting conductive sheet 1.
[0032] Examples of the substrate 11 include polymer films and glass. From the viewpoint of flexibility, preferably, the substrate 11 is a polymer film.
[0033] As materials for polymer films, for example, polyester resins, (meth) acrylic resins, olefin resins, polycarbonate resins, polyethersulfone resins, polyarylate resins, melamine resins, polyamide resins, polyimide resins, cellulose resins, and polystyrene resins can be cited. As polyester resins, for example, polyethylene terephthalate, polybutylene terephthalate, and polyethylene naphthalate can be cited. As (meth) acrylic resins, for example, polymethyl methacrylate can be cited. As olefin resins, for example, polyethylene, polypropylene, and cycloolefin polymers can be cited. As cellulose resins, for example, cellulose triacetate can be cited.
[0034] As a material for the polymer film, preferably, polyester resin can be used, and as a material for the polymer film, more preferably, polyethylene terephthalate can be used.
[0035] The thickness of the substrate 11 is, for example, 1 μm or more, preferably 5 μm or more, more preferably 10 μm or more, and, for example, 200 μm or less, preferably 150 μm or less, more preferably 100 μm or less.
[0036] The thickness of the substrate 11 can be measured using a direct-reading thickness gauge (“DG-205” manufactured by PEACOCK).
[0037] Furthermore, the substrate 11 preferably has transparency. Specifically, the total light transmittance (JIS K7375-2008) of the substrate layer 2 is, for example, 80% or more, or preferably 85% or more.
[0038] [Cured resin layer]
[0039] The cured resin layer 12 is arranged on the entire lower surface of the light-transmitting conductive layer 3 so as to be in contact with the lower surface of the light-transmitting conductive layer 3 .
[0040] A dielectric layer can be mentioned as the cured resin layer 12. In the following description, the case where the cured resin layer 12 is a dielectric layer will be described in detail.
[0041] The dielectric layer is a layer for insulating the base material 11 from the light-transmitting conductive layer 3 .
[0042] Examples of the dielectric layer include cured products of dielectric layer compositions (eg, melamine resins, alkyd resins, and organosilane condensates).
[0043] The thickness of the dielectric layer is, for example, greater than or equal to 10 nm, or preferably greater than or equal to 30 nm, and, for example, less than or equal to 100 nm, or preferably less than or equal to 50 nm.
[0044] The dielectric layer will be described in detail later, and is formed by applying a dielectric layer composition on one surface in the thickness direction of the substrate 11 and drying and curing the composition as necessary.
[0045] <Light-transmitting conductive layer>
[0046] The light-transmitting conductive layer 3 has a film shape and is disposed on the entire upper surface of the base layer 2 so as to be in contact with the upper surface of the base layer 2. The light-transmitting conductive layer 3 is the uppermost layer of the light-transmitting conductive sheet 1.
[0047] As a material of the light-transmitting conductive layer 3, for example, conductive oxides can be cited. As conductive oxides, for example, metal oxides containing at least one metal or semimetal selected from the group consisting of In, Sn, Zn, Ga, Sb, Ti, Si, Zr, Mg, Al, Au, Ag, Cu, Pd and W can be cited. If necessary, the metal oxides can also be doped with metal atoms or semimetal atoms shown in the above group.
[0048] Examples of the conductive oxide include metal oxides, such as indium zinc composite oxide (IZO), indium gallium zinc composite oxide (IGZO), indium gallium composite oxide (IGO), indium tin composite oxide (ITO), and antimony tin composite oxide (ATO).
[0049] As the conductive oxide, indium tin composite oxide (ITO) is preferably used from the viewpoint of improving transparency and conductivity. In the following description, the case where the material of the light-transmitting conductive layer 3 is indium tin composite oxide (ITO) is described in detail.
[0050] The concentration of tin oxide in the indium tin composite oxide (ITO) is, for example, 0.1 mass % or more, preferably 1 mass % or more, and for example, 30 mass % or less.
[0051] The light-transmitting conductive layer 3 includes a first region 21 and a second region 22 in this order toward one side in the thickness direction.
[0052] [Area 1]
[0053] The first region 21 is the other side portion in the thickness direction of the light-transmitting conductive layer 3. The first region 21 includes the other surface in the thickness direction of the light-transmitting conductive layer 3. The first region 21 is formed over the entire surface direction of the light-transmitting conductive layer 3.
[0054] The main region of the first region 21 is crystalline (crystallinity). Specifically, the first region 21 includes a crystalline region as the main region in cross-sectional observation. Specifically, as such a mode of the first region 21, for example, a mode in which all regions in the first region 21 are crystalline in cross-sectional observation, for example, a mode in which the main region in the first region 21 is crystalline in cross-sectional observation and the remaining small region is amorphous.
[0055] The crystallinity in the first region 21 is confirmed by observing the cross-sectional TEM image. In addition, by observing the presence or absence of the lattice pattern and the proportion of the region where the lattice pattern is confirmed using a high-magnification cross-sectional TEM, it can be determined that the first region 21 is crystalline and / or the crystalline is the main region. In addition, when the first region 21 is crystalline, for example, the first region 21 is immersed in a 5% by mass hydrochloric acid aqueous solution for 15 minutes, washed with water and dried, and the resistance between the two terminals between about 15 mm on the surface of the first region 21 is measured, and the resistance between the two terminals is 10 kΩ or less.
[0056] In cross-sectional observation, the area ratio of the main region (area ratio of crystalline matter) in the first region 21 is, for example, 0.7 or more, preferably 0.8 or more, more preferably 0.9 or more, and for example, 1 or less.
[0057] The thickness of the first region 21 is preferably thinner than the thickness of the second region 22 described later, and is, for example, 1 nm or more, preferably 10 nm or more, more preferably 20 nm or more, and, for example, 70 nm or less, preferably 50 nm or less, more preferably 30 nm or less.
[0058] The ratio of the thickness of the first region 21 to the thickness of the light-transmitting conductive layer 3 is, for example, 0.10 or more, preferably 0.15 or more, and, for example, 0.40 or less, preferably 0.20 or less, and more preferably 0.17 or less.
[0059] When the ratio is within the above range, the resistivity is low and the bendability can be improved.
[0060] In addition, the method of measuring the thickness of the first region 21 will be described in detail in the examples described later.
[0061] Furthermore, the first region 21 includes a third region 31 and a fourth region 32 in this order toward one side in the thickness direction. The third region 31 and the fourth region 32 are formed over the entire surface direction of the light-transmitting conductive layer 3 .
[0062] The ratio of the amount of tin oxide (tin oxide content ratio) to the total amount of indium oxide (In2O3) and tin oxide (SnO2) in ITO is different in the third region 31 and the fourth region 32. From the viewpoint of reducing resistance, the tin oxide content ratio of the third region 31 is preferably greater than the tin oxide content ratio of the fourth region 32.
[0063] The tin oxide content of the third region 31 is, for example, 5 mass % or more, preferably 7 mass % or more, more preferably 9 mass % or more, and, for example, 15 mass % or less, preferably 12 mass % or less. The tin oxide content of the fourth region 32 is, for example, 1 mass % or more, preferably 2 mass % or more, and, for example, less than 5 mass %, preferably 4 mass % or less.
[0064] The thickness of the third region 31 is, for example, not less than 0.5 nm, preferably not less than 5 nm, more preferably not less than 10 nm, and is, for example, not more than 35 nm, preferably not more than 25 nm, more preferably not more than 15 nm.
[0065] The ratio of the thickness of the third region 31 to the thickness of the first region 21 is, for example, 20% or more, preferably 40% or more, and, for example, 80% or less, preferably 60% or less.
[0066] The thickness of the fourth region 32 is, for example, not less than 0.5 nm, preferably not less than 5 nm, more preferably not less than 10 nm, and, for example, not more than 35 nm, preferably not more than 25 nm, more preferably not more than 15 nm.
[0067] The ratio of the thickness of the fourth region 32 to the thickness of the first region 21 is, for example, 20% or more, preferably 40% or more, and, for example, 80% or less, preferably 60% or less.
[0068] [Area 2]
[0069] The second region 22 is a portion on one side in the thickness direction of the light-transmitting conductive layer 3. The second region 22 includes one side in the thickness direction of the light-transmitting conductive layer 3. In addition, the second region 22 is continuous on one side in the thickness direction of the first region 21. In addition, the second region 22 is formed over the entire surface direction of the light-transmitting conductive layer 3.
[0070] The main area of the second region 22 is amorphous (non-crystalline). Specifically, in cross-sectional observation, the second region 22 includes an amorphous area as the main area. Specifically, as such a second region 22, for example, in cross-sectional observation, the entire area of the second region 22 is amorphous, for example, in cross-sectional observation, the main area of the second region 22 is amorphous and the remaining small area is crystalline.
[0071] The amorphous nature of the second region 22 is confirmed by observing the cross-sectional TEM image. In addition, by observing the presence or absence of the lattice pattern and the ratio of the region where the lattice pattern is confirmed using a high-magnification cross-sectional TEM, it can be determined that the second region 22 is amorphous and / or the amorphous is the main region. In addition, when the second region 22 is amorphous, for example, the second region 22 is immersed in a 5% by mass hydrochloric acid aqueous solution for 15 minutes, washed with water and dried, and the resistance between the two terminals between about 15 mm on the surface of the second region 22 is measured, and the resistance between the two terminals exceeds 10 kΩ.
[0072] In cross-sectional observation, the area ratio of the main region (area ratio of the amorphous portion) in the second region 22 is, for example, 0.6 or more, preferably 0.8 or more, more preferably 0.9 or more, and for example, 1 or less.
[0073] From the viewpoint of bendability, the thickness of the second region 22 is preferably thicker than the thickness of the first region 21, for example, greater than 70 nm, preferably greater than 80 nm, more preferably greater than 90 nm, and further preferably greater than 100 nm. In addition, from the viewpoint of low resistivity, it is, for example, less than 150 nm, preferably less than 110 nm.
[0074] The ratio of the thickness of the second region 22 to the thickness of the light-transmitting conductive layer 3 is, for example, 0.60 or more, preferably 0.80 or more, more preferably 0.83 or more, and, for example, 0.90 or less, preferably 0.85 or less.
[0075] When the ratio is within the above range, the resistivity is low and the bendability can be improved.
[0076] The method for measuring the thickness of the second region 22 will be described in detail in the examples described later.
[0077] If the thickness of the second region 22 is thicker than the thickness of the first region, the bendability can be further improved.
[0078] Furthermore, the ratio of the thickness of the second region 22 to the thickness of the first region 21 is, for example, greater than 1, preferably greater than 2.0, more preferably greater than 4.0, and further preferably greater than 4.5, and is, for example, less than 150, preferably less than 100, more preferably less than 10, and further preferably less than 5.0.
[0079] When the ratio is within the above range, the resistivity is low and the bendability can be improved.
[0080] [Physical properties of light-transmitting conductive layer]
[0081] The thickness of the light-transmitting conductive layer 3 is the sum of the thickness of the first region 21 and the second region 22 , and is, from the viewpoint of low resistance, for example, 100 nm or more, preferably 110 nm or more, more preferably 125 nm or more, and for example, 200 nm or less, preferably 150 nm or less.
[0082] The total light transmittance (JIS K 7375-2008) of the light-transmitting conductive layer 3 is, for example, 60% or more, preferably 80% or more, more preferably 85% or more, and, for example, 100% or less.
[0083] The surface resistance of the light-transmitting conductive layer 3 is, for example, 40 Ω / □ or less, preferably 35 Ω / □ or less, and, for example, exceeds 0 Ω / □. The surface resistance can be measured by a four-probe method in accordance with JIS K7194.
[0084] The resistivity of the light-transmitting conductive layer 3 is, for example, 2.8×10 -4 Ωcm or less, more preferably 2.5×10 -4 Ωcm or less, and for example, more than 0 Ωcm, preferably 0.1×10 -4 Ωcm or more, more preferably 1.0×10 -4 Ωcm or more. The resistivity can be obtained by multiplying the surface resistance by the thickness.
[0085] <Method for producing light-transmitting conductive sheet>
[0086] refer to Figure 2 A~ Figure 2 D, a method for manufacturing the light-transmitting conductive sheet 1 is described.
[0087] The method for producing the light-transmitting conductive sheet 1 comprises a first step of preparing a substrate layer 2, and a second step of disposing a light-transmitting conductive layer 3 on one surface in the thickness direction of the substrate layer 2 by sputtering. In this method, each layer is sequentially disposed in a roll-to-roll manner, for example. In this case, the conveying speed is, for example, 1.0 m / min or more, and, for example, 20.0 m / min or less.
[0088] [1st step]
[0089] In the first step, the base material layer 2 is prepared.
[0090] When preparing the substrate layer 2, as Figure 2 As shown in A, a substrate 11 is prepared.
[0091] Then, if Figure 2 As shown in FIG. 1B , a cured resin layer 12 (dielectric layer) is disposed on one surface in the thickness direction of the substrate 11 .
[0092] When the cured resin layer 12 (dielectric layer) is disposed on one side in the thickness direction of the substrate 11, the dielectric layer composition is applied on one side in the thickness direction of the substrate 11, and dried and cured as needed. Thus, the cured resin layer 12 (dielectric layer) is disposed on one side in the thickness direction of the substrate 11, and the substrate layer 2 is prepared.
[0093] [Step 2]
[0094] In the second step, the light-transmitting conductive layer 3 is disposed on one surface in the thickness direction of the base layer 2 by sputtering.
[0095] Specifically, the second step includes a third step of arranging the first region 21 on one surface in the thickness direction of the base layer 2 , and a fourth step of arranging the second region 22 on one surface in the thickness direction of the first region 21 .
[0096] (Step 3)
[0097] In the third step, Figure 2 As shown in C, the first region 21 is arranged on one side in the thickness direction of the base layer 2 by sputtering. Specifically, the third region 31 and the fourth region 32 are arranged in sequence on one side in the thickness direction of the base layer 2 by sputtering, and then the third region 31 and the fourth region 32 are crystallized.
[0098] Before the third region 31 and the fourth region 32 are sequentially arranged on one surface in the thickness direction of the base layer 2 by sputtering, the one surface in the thickness direction of the base layer 2 is subjected to a surface treatment as necessary.
[0099] Examples of the surface treatment include corona treatment, plasma treatment, flame treatment, ozone treatment, primer treatment, glow treatment, and saponification treatment.
[0100] Then, in the sputtering method, in each of the two vacuum chambers arranged along the conveying direction of the substrate layer 2, the material of the third region 31 and the material of the fourth region 32 are sequentially arranged as targets along the conveying direction of the substrate layer 2. In addition, the target can be arranged in a manner opposite to the substrate layer 2. In addition, during sputtering, the substrate layer 2 is closely attached to the circumferential direction of the film-forming roller.
[0101] Then, a sputtering gas is supplied and a voltage is applied from a power source to accelerate gas ions and irradiate the target, thereby ejecting the target material from the target surface. The target material is deposited on the surface (one side in the thickness direction) of the substrate layer 2, and the third region 31 and the fourth region 32 are sequentially arranged.
[0102] As the sputtering gas, for example, an inert gas (for example, krypton gas, argon gas) and oxygen gas can be cited. As the sputtering gas, it is preferred to use an inert gas and oxygen gas in combination. As the inert gas, it is preferred to cite krypton gas. When krypton gas is used as the inert gas, the first region 21 (the third region 31 and the fourth region 32) contains krypton atoms.
[0103] The amount of oxygen introduced relative to the total amount of the inert gas and oxygen is, for example, 1.0 flow % or more, preferably 1.5 flow % or more, and, for example, 5.0 flow % or less, preferably 2.0 flow % or less.
[0104] The gas pressure during sputtering is, for example, 0.1 Pa or more, preferably 0.2 Pa or more, and, for example, 2.0 Pa or less.
[0105] The power source may be, for example, any of a DC power source, an AC power source, an MF power source, and an RF power source, or a combination of these.
[0106] The discharge output is, for example, 1.0 kW or more, preferably 10.0 kW or more, and, for example, 20 kW or less.
[0107] The horizontal magnetic field intensity of the target is, for example, 10 mT or more, preferably 60 mT or more, and, for example, 200 mT or less, preferably 100 mT or less.
[0108] The temperature of the film-forming roller is, for example, 20° C. or lower, preferably 10° C. or lower, more preferably 0° C. or lower, and, for example, -50° C. or higher, preferably -25° C. or higher.
[0109] Then, the third region 31 and the fourth region 32 are crystallized.
[0110] When the third region 31 and the fourth region 32 are crystallized, the third region 31 and the fourth region 32 are heated. Specifically, the third region 31 and the fourth region 32 are heated using a heating roller after sputtering.
[0111] As heating conditions, the heating temperature is, for example, 120° C. or higher, preferably 150° C. or higher, and for example, 250° C. or lower, preferably 200° C. or lower, and the heating time is 30 seconds or longer, and for example, 120 seconds or lower.
[0112] Thus, the third region 31 and the fourth region 32 are crystallized to obtain the first region 21. As described above, the first region 21 is arranged on one surface of the base layer 2 in the thickness direction.
[0113] (Step 4)
[0114] In the fourth step, if Figure 2 As shown in D, the second region 22 is arranged on one surface in the thickness direction of the first region 21 by sputtering.
[0115] Then, in the sputtering method, the target (material of the second region 22) and the first region 21 are arranged opposite to each other in a vacuum chamber. Then, a sputtering gas is supplied and a voltage is applied from a power supply to accelerate gas ions and irradiate the target, so that the target material is ejected from the target surface. And, the target material is deposited on the surface (one side in the thickness direction) of the first region 21 to form the second region 22. In addition, during sputtering, the base material layer 2 is closely attached to the circumferential direction of the film-forming roller.
[0116] In addition, as the sputtering gas, for example, inert gas (such as krypton gas, argon gas) and oxygen gas can be cited. As the inert gas, argon gas can be preferably cited. When argon gas is used as the inert gas, the second region 22 contains argon atoms.
[0117] The amount of oxygen introduced relative to the total amount of the inert gas and oxygen is, for example, 0.05 flow % or more, preferably 0.1 flow % or more, and, for example, 2.0 flow % or less, preferably 1.0 flow % or less.
[0118] The gas pressure during sputtering is, for example, 0.1 Pa or more, preferably 0.2 Pa or more, and, for example, 2.0 Pa or less.
[0119] The power source may be, for example, any of a DC power source, an AC power source, an MF power source, and an RF power source, or a combination of these.
[0120] The discharge output is, for example, 1.0 kW or more, preferably 10.0 kW or more, and, for example, 20 kW or less.
[0121] The horizontal magnetic field intensity of the target is, for example, 10 mT or more, and for example, 200 mT or less, preferably 100 mT or less, and more preferably 40 mT or less.
[0122] The temperature of the film-forming roller is, for example, 20° C. or lower, preferably 10° C. or lower, more preferably 0° C. or lower, and, for example, -50° C. or higher, preferably -25° C. or higher.
[0123] Thus, the second region 22 is arranged on one surface in the thickness direction of the first region 21. As described above, the light-transmitting conductive sheet 1 can be obtained.
[0124] <Effects>
[0125] The light-transmitting conductive sheet 1 includes a base material layer 2 and a light-transmitting conductive layer 3 in order toward one side in the thickness direction. In addition, in the light-transmitting conductive sheet 1, the light-transmitting conductive layer 3 includes a first region 21 whose main region is crystalline and a second region 22 whose main region is amorphous in order toward one side in the thickness direction. Therefore, the light-transmitting conductive sheet has a low resistivity and excellent bendability.
[0126] Specifically, the light-transmitting conductive layer 3 is required to have a lower resistivity. However, if the thickness of the light-transmitting conductive layer 3 is increased from the viewpoint of reducing the resistivity, there is a disadvantage that the bendability is reduced.
[0127] On the other hand, in the light-transmitting conductive sheet 1, the first region 21 and the second region 22 are arranged in a predetermined order. Therefore, the light-transmitting conductive sheet 1 has a low resistivity and excellent bendability.
[0128] <Modification>
[0129] In the modification, for the same components and processes as those of the first embodiment, the same reference numerals are used and their specific description is omitted. In addition, unless otherwise specified, the modification can achieve the same effects as the first embodiment. In addition, the first embodiment and its modification can be appropriately combined.
[0130] In the above description, the cured resin layer 12 is a dielectric layer, but the cured resin layer 12 may also be a hard coat layer.
[0131] The hard coat layer is a scratch protection layer for making the light-transmitting conductive layer 3 less susceptible to scratches.
[0132] Examples of the hard coat layer include cured products of hard coat compositions (acrylic resins, polyurethane resins, and the like) described in Japanese Unexamined Patent Application Publication No. 2016-179686.
[0133] The hard coat layer is formed by applying a hard coat composition on one surface in the thickness direction of the substrate 11 and drying and curing the composition as necessary.
[0134] The thickness of the hard coat layer is, for example, 0.1 μm or more, preferably 0.5 μm or more, and, for example, 10 μm or less, preferably 5 μm or less.
[0135] In the above description, the base material layer 2 includes the base material 11 and the cured resin layer 12 . However, the base material layer 2 may include only the base material 11 without including the cured resin layer 12 .
[0136] In the above description, the first region 21 includes the third region 31 and the fourth region 32 in this order toward one side in the thickness direction, but may include only one of the third region 31 and the fourth region 32. Preferably, the first region 21 includes the third region 31 and the fourth region 32 in this order toward one side in the thickness direction.
[0137] Example
[0138] Embodiment and comparative example are shown below, and the present invention is further specifically described.It should be noted that the present invention is not limited to any embodiment and comparative example.In addition, the specific numerical values such as the blending ratio (containing ratio), physical property value, parameter used in the following description can replace the upper limit value (as the numerical value defined as "below", "not enough") or the lower limit value (as the numerical value defined as "above", "exceeding") of the blending ratio (containing ratio), physical property value, parameter, etc. recorded in the above-mentioned "specific embodiments", corresponding thereto.
[0139] <Manufacturing of light-transmitting conductive sheet>
[0140] Example 1
[0141] [1st step]
[0142] A long PET film (thickness 50 μm, manufactured by Toray Industries, Inc.) was prepared as a substrate.
[0143] Then, a dielectric layer composition (a thermosetting resin (optical refractive index n=1.54) with a weight ratio of melamine resin:alkyd resin:organosilane condensate of 2:2:1) was applied on one side of the substrate in the thickness direction and cured to form a dielectric layer (thickness: 35 nm). Thus, a substrate layer was prepared.
[0144] [Step 2]
[0145] The first region is disposed on one surface of the substrate layer in the thickness direction by a reactive sputtering method. In the reactive sputtering method, a sputtering film forming apparatus (DC magnetron sputtering apparatus) capable of performing a film forming process by a roll-to-roll method is used.
[0146] (Step 3)
[0147] Specifically, first, the amorphous third region is arranged on one surface in the thickness direction of the base material layer.
[0148] Specifically, a sintered body of indium oxide and tin oxide (tin oxide concentration of 10 mass%) was used as a target. A DC power supply was used as a power source for applying voltage to the target. The horizontal magnetic field intensity on the target was set to 90 mT. In the sputtering device, the substrate layer was closely attached along the circumferential direction of the film-forming roller. The temperature of the film-forming roller was set to -5°C. In addition, the sputtering film-forming device was evacuated to a vacuum degree of 0.9×10 -4 After 0.5 Pa, krypton gas as a sputtering gas and oxygen gas as a reactive gas were introduced into the sputtering film forming apparatus, and the gas pressure in the sputtering film forming apparatus was set to 0.2 Pa. The ratio of the oxygen gas introduction amount to the total introduction amount of krypton gas and oxygen gas introduced into the sputtering film forming apparatus was about 1.8% by flow rate. Thus, the amorphous third region (11 nm) was arranged on one side in the thickness direction of the substrate layer.
[0149] Then, the amorphous fourth region is arranged on one surface in the thickness direction of the third region.
[0150] Specifically, a sintered body of indium oxide and tin oxide (tin oxide concentration is 3% by mass) is used as a target. A DC power supply is used as a power source for applying voltage to the target. The horizontal magnetic field intensity on the target is set to 90mT. In the sputtering device, the substrate layer is closely attached to the circumferential direction of the film-forming roller. The temperature of the film-forming roller is set to -5°C. Krypton gas as a sputtering gas and oxygen gas as a reactive gas are introduced, and the gas pressure in the sputtering film-forming device is set to 0.2Pa. The ratio of the oxygen gas introduction amount to the total amount of krypton gas and oxygen gas introduced into the sputtering film-forming device is approximately 1.8% of the flow rate. Thus, an amorphous fourth region (11nm) is arranged on one side in the thickness direction of the third region.
[0151] Then, the substrate layer having the third region and the fourth region was brought into contact with a heating roller in a vacuum heating device. Thus, the third region and the fourth region were crystallized. The heating temperature was 160° C. and the heating time was 1 minute. Thus, the first region was arranged on one surface in the thickness direction of the substrate layer.
[0152] (Step 4)
[0153] The amorphous second region is arranged on one surface in the thickness direction of the first region.
[0154] Specifically, a sintered body of indium oxide and tin oxide (tin oxide concentration of 12 mass%) was used as a target. A DC power supply was used as a power source for applying voltage to the target. The horizontal magnetic field intensity on the target was set to 30 mT. In the sputtering device, the substrate layer was closely attached along the circumferential direction of the film-forming roller. The temperature of the film-forming roller was set to -5°C. In addition, the sputtering film-forming device was evacuated to a vacuum degree of 0.9×10 -4After 0.05 Pa, argon gas as a sputtering gas and oxygen gas as a reactive gas are introduced into the sputtering film forming device, and the gas pressure in the sputtering film forming device is set to 0.2 Pa. The ratio of the oxygen gas introduction amount to the total amount of argon gas and oxygen gas introduced into the sputtering film forming device is about 0.1% by flow rate. Thus, an amorphous second region (108 nm) is arranged on one side in the thickness direction of the first region. Based on the above, a light-transmitting conductive sheet is manufactured.
[0155] Example 2
[0156] A light-transmitting conductive sheet was produced according to the same procedure as in Example 1. However, the thickness of the second region was changed.
[0157] Comparative Example 1
[0158] A light-transmitting conductive sheet was manufactured based on the same steps as in Example 1. However, step 3 was not performed. In step 4, the ratio of the amount of oxygen introduced to the total amount of argon and oxygen introduced into the sputtering film forming apparatus was changed to about 2.4 flow %, and the thickness of the second region was changed.
[0159] Comparative Example 2
[0160] A light-transmitting conductive sheet was produced according to the same procedure as in Example 1. However, the fourth step was not performed.
[0161] Comparative Example 3
[0162] A light-transmitting conductive sheet was produced according to the same procedure as in Example 1. However, in the third step, the amorphous third region (120 nm) and the amorphous fourth region (10 nm) were sequentially arranged and then crystallized. The fourth step was not performed.
[0163] Comparative Example 4
[0164] A light-transmitting conductive sheet was produced according to the same procedure as in Example 1. However, in the second step, the third step was performed after the fourth step. In addition, based on the description in Table 1, the thickness of the first region and the second region were changed.
[0165] <Evaluation>
[0166] [Thickness of light-transmitting conductive layer]
[0167] The thickness of the light-transmitting conductive layer (each region) of each embodiment and each comparative example is measured by FE-TEM observation. Specifically, first, a cross-sectional observation sample of the light-transmitting conductive layer of each embodiment and each comparative example is prepared by FIB microsampling method. A FIB device (trade name "FB2200", manufactured by Hitachi) is used in the FIB microsampling method, and the acceleration voltage is set to 10 kV. Then, the thickness of the light-transmitting conductive layer in the cross-sectional observation sample is measured by FE-TEM observation. A FE-TEM device (trade name "JEM-2800", manufactured by JEOL) is used in the FE-TEM observation, and the acceleration voltage is set to 200 kV.
[0168] In addition, the thickness of the fourth region is calculated by subtracting the thickness of the third region from the thickness of the first region (the sum of the thickness of the third region and the thickness of the fourth region). In addition, the thickness of the second region is calculated by subtracting the thickness of the first region from the thickness of the entire light-transmitting conductive layer. The results are shown in Table 1.
[0169] [Resistance value]
[0170] The resistance value (R0) of the light-transmitting conductive layer of each Example and each Comparative Example was measured by a four-probe method. A resistance value of less than 50Ω was expressed as a real number, and a resistance value of 50Ω or more was expressed as 50Ω or more.
[0171] The results are shown in Table 1.
[0172] [Flexibility]
[0173] The bendability of the light-transmitting conductive sheet of each embodiment and each comparative example was evaluated. Specifically, the light-transmitting conductive sheet of each embodiment and each comparative example was cut into pieces with a width of 10 mm and a length of 150 mm, respectively, to prepare a sample. Then, the sample was placed on a core rod so that the light-transmitting conductive layer was on the outside and the other side of the substrate in the thickness direction was in contact with the core rod. Then, both ends of the long side of the light-transmitting conductive sheet were clamped with a clamp, and a weight of 1000 g was placed in the center of the clamp. That is, a load of 100 g / mm relative to the width of the light-transmitting conductive sheet was applied to the lower side to bend the light-transmitting conductive sheet. This bending state lasted for 10 seconds.
[0174] In this bending state, after applying the marker to the bent portion, the bending state is released and the marker portion is observed under a microscope. In this test method, the diameter of the core rod is changed from a large diameter to a small diameter by 1 mm at a time, and the minimum diameter at which no cracks can be confirmed under the microscope in the marker-coated portion is recorded in Table 1. The smaller this value is, the better the bending resistance is. The results are shown in Table 1.
[0175] It should be noted that in the above test, the diameter of the mandrel was changed from a large diameter to a small diameter by 1 mm at a time, and the sample was changed each time it was changed. That is, in the above test, the number of bends was 1 for one sample, and each time it was bent, it was changed to another sample (another sample manufactured under the same conditions).
[0176] [Table 1]
[0177] Table 1
[0178]
[0179] It should be noted that the above invention is provided as an exemplary embodiment of the present invention, but it is merely an illustration and is not to be construed as limiting. Modifications of the present invention that are obvious to a person skilled in the art are within the scope of the above claims.
[0180] Industrial Applicability
[0181] The light-transmitting conductive sheet of the present invention can be suitably used in the production of various devices such as display panels, touch panels, and solar cells.
Claims
1. A light-transmitting conductive sheet comprising a base layer and a light-transmitting conductive layer in this order toward one side in a thickness direction, The light-transmitting conductive layer includes a first region and a second region in order toward one side in the thickness direction. The main area of the first area is crystalline, A main area of the second region is amorphous.
2. The light-transmitting conductive sheet according to claim 1, wherein The second region is thicker than the first region.
Citation Information
Patent Citations
Light transmitting conductive film
CN111613365A
Light-transmitting conductive layer laminate
CN115428100A
TRANSMISSION CONDUCTIVE SHEET, CONTACT SENSOR, Dimming ELEMENT, PHOTOELECTRIC CONVERSION ELEMENT, HEAT WIRE CONTROL MEMBER, ANTENNA,
CN115666928A
Conductive laminated body
JP2004042476A
Transparent conductive membrane, method for manufacturing transparent conductive film and transparent conductive membrane, and flexible display using transparent conductive membrane
JP2011003456A