Light-transmitting conductive layer and light-transmitting conductive sheet

By designing the uneven thickness structure of the amorphous and crystalline regions in the light-transmissive conductive layer, the problem in the prior art that the light-transmissive conductive layer decreases in bending when thickened is solved, and low resistivity and Combining excellent bending properties.

CN118737529APending Publication Date: 2024-10-01NITTO DENKO CORP
View PDF 2 Cites 0 Cited by

Patent Information

Application Number
CN202410372215.X
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Priority Date
2023-03-30
Filing Date
2024-03-29
Publication Date
2024-10-01

AI Technical Summary

Technical Problem

When the existing light-transmissive conductive layer is thickened, the flexibility will be reduced, making it difficult to achieve low resistivity and excellent flexibility at the same time.

Method used

Design a translucent conductive layer that includes an amorphous first region and a crystalline second region in the thickness direction. The second region is thicker than the first region, and is formed on the base material by sputtering. These regions are configured on the layer to create a structure of uneven thickness.

Benefits of technology

Achieving low resistivity and excellent bendability, it is suitable for the manufacturing of various devices.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN118737529A_ABST
    Figure CN118737529A_ABST
Patent Text Reader

Abstract

Provided are a translucent conductive layer and a translucent conductive sheet. The translucent conductive layer (3) is provided with a first main surface (11) and a second main surface (12) facing each other in the thickness direction. A first region (21) including a first main surface (11) and a second region (22) including a second main surface (12) are provided in this order toward one side in the thickness direction. The main region of the first region (21) is amorphous. The main region of the second region (22) is crystalline. The first region (21) has a non-uniform thickness.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The present invention relates to a light-transmitting conductive layer and a light-transmitting conductive sheet. Background Art

[0002] Conventionally, a light-transmitting conductive sheet including a substrate and a light-transmitting conductive layer in this order has been known. Such a light-transmitting conductive sheet is suitable for use in various devices (for example, a touch sensor).

[0003] As such a light-transmitting conductive sheet, for example, a light-transmitting conductive sheet has been proposed which includes a resin layer and a light-transmitting conductive layer in sequence toward one side in the thickness direction, and the light-transmitting conductive layer includes an amorphous first region and a crystalline second region in sequence toward one side in the thickness direction (for example, refer to Patent Document 1).

[0004] Existing patent literature

[0005] Patent Literature

[0006] Patent Document 1: Handbook of International Publication No. 2021 / 241118 Summary of the invention

[0007] Problem that the invention aims to solve

[0008] On the other hand, the light-transmitting conductive layer is required to have a lower resistivity. From the viewpoint of reducing the resistivity, increasing the thickness of the light-transmitting conductive layer has been studied. However, increasing the thickness of the light-transmitting conductive layer has the disadvantage of reduced bendability.

[0009] The present invention provides a light-transmitting conductive layer having a low resistivity and excellent bendability, and a light-transmitting conductive sheet having the light-transmitting conductive layer.

[0010] Solutions for solving problems

[0011] The present invention [1] is a light-transmitting conductive layer, which has a first main surface and a second main surface opposite to each other in the thickness direction, and has a first region including the first main surface and a second region including the second main surface in sequence toward one side in the thickness direction, the main area of ​​the first region is amorphous, the main area of ​​the second region is crystalline, and the first region has an uneven thickness.

[0012] The present invention [2] comprises the light-transmitting conductive layer described in [1] above, wherein the thickness of the second region is thicker than the thickness of the first region.

[0013] The present invention [3] includes a light-transmitting conductive sheet comprising the light-transmitting conductive layer according to [1] or [2] above, and a base material layer located on the first main surface side of the light-transmitting conductive layer.

[0014] Effects of the Invention

[0015] The light-transmitting conductive layer of the present invention has a crystalline second region, and thus has a low resistivity. In addition, in the light-transmitting conductive layer, the amorphous first region has a non-uniform thickness, and thus has excellent bendability.

[0016] The light-transmitting conductive sheet of the present invention includes the light-transmitting conductive layer of the present invention, and therefore has a low resistivity and excellent bendability. BRIEF DESCRIPTION OF THE DRAWINGS

[0017] Figure 1 One embodiment of the light-transmitting conductive layer and the light-transmitting conductive sheet of the present invention is shown.

[0018] Figure 2 middle, Figure 2 A~ Figure 2 C represents an embodiment of a method for producing a light-transmitting conductive layer and a light-transmitting conductive sheet. Figure 2 A represents the first step of preparing a base material layer. Figure 2 B represents a third step of disposing the first region on one surface in the thickness direction of the base layer in the second step. Figure 2 C represents a fourth step of configuring the second region on one surface in the thickness direction of the first region in the second step.

[0019] Description of Reference Numerals

[0020] 1Transparent conductive sheet

[0021] 2. Base material layer

[0022] 3Transparent conductive layer

[0023] 11 Main side 1

[0024] 12Second Main Side

[0025] 21 Area 1

[0026] 22 Area 2 DETAILED DESCRIPTION

[0027] refer to Figure 1 , describing an embodiment of the light-transmitting conductive layer and the light-transmitting conductive sheet of the present invention.

[0028] Figure 1 In the figure, the up-down direction of the paper is the up-down direction (thickness direction). In addition, the upper side of the paper is the upper side (one side in the thickness direction). In addition, the lower side of the paper is the lower side (the other side in the thickness direction). In addition, the left-right direction of the paper and the depth direction are the surface directions orthogonal to the up-down direction. Specifically, the directions of each figure are based on the arrows.

[0029] The light-transmitting conductive sheet 1 has a film shape (including a sheet shape) having a predetermined thickness. The light-transmitting conductive sheet 1 extends in a plane direction perpendicular to the thickness direction. The light-transmitting conductive sheet 1 has a flat upper surface and a flat lower surface. The light-transmitting conductive sheet 1 is preferably flexible.

[0030] like Figure 1 As shown in , the light-transmitting conductive sheet 1 includes a substrate layer 2 and a light-transmitting conductive layer 3 disposed on one side in the thickness direction of the substrate layer 2. In other words, the light-transmitting conductive sheet 1 includes the light-transmitting conductive layer 3 and the substrate layer 2 located on the first principal surface 11 (described later) side of the light-transmitting conductive layer 3. In addition, specifically, the light-transmitting conductive sheet 1 includes the substrate layer 2 and the light-transmitting conductive layer 3 disposed directly on the upper surface (one side in the thickness direction) of the substrate layer 2. The light-transmitting conductive sheet 1 preferably includes the substrate layer 2 and the light-transmitting conductive layer 3.

[0031] The thickness of the light-transmitting conductive sheet 1 is, for example, 400 μm or less, or preferably 200 μm or less, and, for example, 1 μm or more, or preferably 5 μm or more.

[0032] <Base material layer>

[0033] The base layer 2 has a film shape. The base layer 2 is preferably flexible. The base layer 2 is disposed on the entire lower surface of the light-transmitting conductive layer 3 so as to contact the lower surface of the light-transmitting conductive layer 3. The base layer 2 is the lowermost layer of the light-transmitting conductive sheet 1.

[0034] The base material layer 2 includes a base material 10 . The base material layer 2 is formed of the base material 10 .

[0035] [Base material]

[0036] Examples of the substrate 10 include polymer films and glass. Preferred examples of the substrate 2 include polymer films from the viewpoint of flexibility.

[0037] As materials for polymer films, for example, polyester resins, (meth) acrylic resins, olefin resins, polycarbonate resins, polyethersulfone resins, polyarylate resins, melamine resins, polyamide resins, polyimide resins, cellulose resins, and polystyrene resins can be cited. As polyester resins, for example, polyethylene terephthalate, polybutylene terephthalate, and polyethylene naphthalate can be cited. As (meth) acrylic resins, for example, polymethyl methacrylate can be cited. As olefin resins, for example, polyethylene, polypropylene, and cycloolefin polymers can be cited. As cellulose resins, for example, cellulose triacetate can be cited.

[0038] As a material for the polymer film, preferably, polyester resin can be used, and as a material for the polymer film, more preferably, polyethylene terephthalate can be used.

[0039] The thickness of the substrate 10 is, for example, 1 μm or more, preferably 5 μm or more, more preferably 10 μm or more, and, for example, 200 μm or less, preferably 150 μm or less, more preferably 130 μm or less.

[0040] The thickness of the substrate 10 can be measured using a direct-reading thickness gauge (“DG-205” manufactured by PEACOCK).

[0041] Furthermore, the substrate 10 preferably has transparency. Specifically, the total light transmittance (JIS K7375-2008) of the substrate layer 2 is, for example, 50% or more, preferably 70% or more, more preferably 80% or more, and preferably 85% or more.

[0042] <Light-transmitting conductive layer>

[0043] The light-transmitting conductive layer 3 has a thin film shape and is disposed on the entire upper surface of the base layer 2 so as to contact the upper surface of the base layer 2. The light-transmitting conductive layer 3 is the uppermost layer of the light-transmitting conductive sheet 1.

[0044] The light-transmitting conductive layer 3 includes a first main surface 11 and a second main surface 12 that are opposed to each other in the thickness direction.

[0045] The first main surface 11 is a flat surface and contacts one surface of the base material layer 2 in the thickness direction.

[0046] The second main surface 12 is exposed on one side in the thickness direction. The second main surface 12 is a flat surface substantially parallel to the first main surface 11 .

[0047] As a material of the light-transmitting conductive layer 3, for example, conductive oxides can be cited. As conductive oxides, for example, metal oxides containing at least one metal or semimetal selected from the group consisting of In, Sn, Zn, Ga, Sb, Ti, Si, Zr, Mg, Al, Au, Ag, Cu, Pd and W can be cited. If necessary, the metal oxides can also be doped with metal atoms or semimetal atoms shown in the above group.

[0048] Examples of the conductive oxide include metal oxides, such as indium zinc composite oxide (IZO), indium gallium zinc composite oxide (IGZO), indium gallium composite oxide (IGO), indium tin composite oxide (ITO), and antimony tin composite oxide (ATO).

[0049] As the conductive oxide, indium tin composite oxide (ITO) is preferably used from the viewpoint of improving transparency and conductivity. In the following description, the case where the material of the light-transmitting conductive layer 3 is indium tin composite oxide (ITO) is described in detail.

[0050] In indium tin composite oxide (ITO), the concentration of tin oxide is, for example, 0.1 mass % or more, preferably 1 mass % or more, preferably 5 mass % or more, more preferably 10 mass % or more, for example, 30 mass % or less, preferably 15 mass % or less.

[0051] The light-transmitting conductive layer 3 includes a first region 21 and a second region 22 in this order toward one side in the thickness direction.

[0052] [Area 1]

[0053] The first region 21 includes the first main surface 11. The first region 21 is a portion on the other side in the thickness direction of the light-transmitting conductive layer 3. The first region 21 includes the other surface of the light-transmitting conductive layer 3 in the thickness direction.

[0054] Furthermore, the first region 21 is formed over the entire surface direction of the light-transmitting conductive layer 3. The first main surface 11 is the other surface of the first region 21 in the thickness direction.

[0055] The main area of ​​the first region 21 is amorphous (non-crystalline). Specifically, the first region 21 includes an amorphous area as the main area in cross-sectional observation. Specifically, as such a mode of the first region 21, for example, a mode in which all areas in the first region 21 are amorphous in cross-sectional observation, for example, a mode in which the main area in the first region 21 is amorphous in cross-sectional observation and the remaining small area is crystalline.

[0056] The amorphous nature of the first region 21 is confirmed by observing the cross-sectional TEM image. In addition, by observing the presence or absence of the lattice pattern and the proportion of the region where the lattice pattern is confirmed using a high-magnification cross-sectional TEM, it can be determined that the first region 21 is amorphous and / or is mainly amorphous.

[0057] In cross-sectional observation, the area ratio of the main region (area ratio of the amorphous material) in the first region 21 is, for example, 0.6 or more, preferably 0.8 or more, more preferably 0.9 or more, and for example, 1 or less.

[0058] Furthermore, the first region 21 has a non-uniform thickness. Specifically, the first surface 13 on the opposite side to the first main surface 11 in the first region 21 has a non-uniform surface.

[0059] More specifically, the non-uniform thickness of the first region 21 means that, in the cross-sectional image of the light-transmitting conductive layer 3, the difference between the thickness at the thickest position of the first region 21 and the thickness at the thinnest position of the first region 21 is 5 nm or more. The thickness of the first region 21 is obtained from the difference between the first surface 13 and the first main surface 11. Specifically, it will be described in detail in the embodiments described later.

[0060] Such a first region 21 can be formed, for example, by setting the partial pressure of water in sputtering described later to a predetermined range.

[0061] The minimum thickness of the first region 21 is preferably thinner than the thickness (minimum thickness) of the second region 22 described later, for example, greater than 1 nm, preferably greater than 3 nm, more preferably greater than 5 nm, and for example, less than 50 nm, preferably less than 30 nm, more preferably less than 20 nm.

[0062] The ratio of the thickness (minimum thickness) of the first region 21 to the thickness (minimum thickness) of the light-transmitting conductive layer 3 is, for example, greater than 0.02, preferably greater than 0.04, and for example, less than 0.10, preferably less than 0.08, and more preferably less than 0.05.

[0063] When the ratio is within the above range, the resistivity is low and the bendability can be improved.

[0064] In addition, the method of measuring the thickness (minimum thickness) of the first region 21 will be described in detail in the examples described later.

[0065] [Area 2]

[0066] The second region 22 includes the second main surface 12. The second region 22 is a portion on one side in the thickness direction of the light-transmitting conductive layer 3. The second region 22 includes one side of the light-transmitting conductive layer 3 in the thickness direction.

[0067] The second region 22 is continuous on one side in the thickness direction of the first region 21. The second region 22 is formed over the entire surface direction of the light-transmitting conductive layer 3. The second main surface 12 is one surface of the second region 22 in the thickness direction.

[0068] The main region of the second region 22 is crystalline (crystallinity). Specifically, in cross-sectional observation, the second region 22 includes a crystalline region as the main region. Specifically, as such a second region 22, for example, in cross-sectional observation, all regions in the second region 22 are crystalline, for example, in cross-sectional observation, the main region in the second region 22 is crystalline, and the remaining small region is amorphous.

[0069] The crystallinity in the second region 22 is confirmed by observing the cross-sectional TEM image. In addition, by observing the presence or absence of the lattice pattern and the proportion of the region where the lattice pattern is confirmed using a high-magnification cross-sectional TEM, it can be determined that the second region 22 is crystalline and / or the crystalline is the main region. In addition, when the second region 22 is crystalline, for example, the second region 22 is immersed in a 5% by mass hydrochloric acid aqueous solution for 15 minutes, washed with water and dried, and the two-terminal resistance between about 15 mm on the surface of the second region 22 is measured, and the two-terminal resistance is 10 kΩ or less.

[0070] In cross-sectional observation, the area ratio of the main region (area ratio of crystalline matter) in the second region 22 is, for example, 0.7 or more, preferably 0.8 or more, more preferably 0.9 or more, and for example, 1 or less.

[0071] The second region 22 has a non-uniform thickness. Specifically, the second surface 14 on the opposite side to the second main surface 12 in the second region 22 has a non-uniform surface corresponding to the first surface 13 described above.

[0072] The second region 22 is disposed on one surface of the first region 21 in the thickness direction. Therefore, if the first region 21 has a non-uniform thickness, the second region 22 also has a non-uniform thickness.

[0073] From the viewpoint of low resistivity and bendability, the thickness (minimum thickness) of the second region 22 is preferably thicker than the thickness (minimum thickness) of the first region 21, for example, greater than 70 nm, preferably greater than 80 nm, more preferably greater than 90 nm, and, for example, less than 150 nm, preferably less than 120 nm, more preferably less than 110 nm.

[0074] The ratio of the thickness (minimum thickness) of the second region 22 to the thickness (minimum thickness) of the light-transmitting conductive layer 3 is, for example, greater than 0.90, preferably greater than 0.92, more preferably greater than 0.95, and for example, less than 0.98, preferably less than 0.96.

[0075] When the ratio is within the above range, the resistivity is low and the bendability can be improved.

[0076] The method for measuring the thickness (minimum thickness) of the second region 22 will be described in detail in Examples described later.

[0077] If the thickness (minimum thickness) of the second region 22 is thicker than the thickness (minimum thickness) of the first region, the bendability can be further improved.

[0078] Furthermore, the ratio of the thickness (minimum thickness) of the second region 22 to the thickness (minimum thickness) of the first region 21 is, for example, greater than 1, preferably greater than 2.0, more preferably greater than 4.0, further preferably greater than 7, particularly preferably greater than 15, and, for example, less than 50, preferably less than 25.

[0079] When the ratio is within the above range, the resistivity is low and the bendability can be improved.

[0080] [Physical properties of light-transmitting conductive layer]

[0081] The thickness (minimum thickness) of the light-transmitting conductive layer 3 is the sum of the thickness of the first region 21 and the thickness of the second region 22. From the perspective of low resistance, it is, for example, greater than 80 nm, preferably greater than 100 nm, and, for example, less than 200 nm, preferably less than 150 nm, and more preferably less than 120 nm.

[0082] The total light transmittance (JIS K 7375-2008) of the light-transmitting conductive layer 3 is, for example, 60% or more, preferably 80% or more, more preferably 85% or more, and, for example, 100% or less.

[0083] The surface resistance of the light-transmitting conductive layer 3 is, for example, 40 Ω / □ or less, preferably 35 Ω / □ or less, and, for example, exceeds 0 Ω / □. The surface resistance can be measured by a four-probe method in accordance with JIS K7194.

[0084] The resistivity of the light-transmitting conductive layer 3 is, for example, 2.8×10 -4 Ωcm or less, more preferably 2.5×10 -4 Ωcm or less, and for example, more than 0 Ωcm, preferably 0.1×10 -4 Ωcm or more, more preferably 1.0×10 -4 Ωcm or more. The resistivity can be obtained by multiplying the surface resistance by the thickness.

[0085] <Method for producing light-transmitting conductive sheet>

[0086] refer to Figure 2 A~ Figure 2 C, a method for manufacturing the light-transmitting conductive sheet 1 is described.

[0087] The method for producing the light-transmitting conductive sheet 1 comprises a first step of preparing a substrate layer 2, and a second step of disposing a light-transmitting conductive layer 3 on one surface in the thickness direction of the substrate layer 2 by sputtering. In this method, each layer is sequentially disposed in a roll-to-roll manner, for example. In this case, the conveying speed is, for example, 1.0 m / min or more, and, for example, 20.0 m / min or less.

[0088] [1st step]

[0089] In the first step, the base material layer 2 is prepared.

[0090] When preparing the substrate layer 2, as Figure 2 As shown in A, a substrate 10 is prepared.

[0091] [Step 2]

[0092] In the second step, the light-transmitting conductive layer 3 is disposed on one surface in the thickness direction of the base layer 2 by sputtering.

[0093] Specifically, the second step includes a third step of arranging the first region 21 on one surface in the thickness direction of the base layer 2 , a fourth step of arranging the second region 22 on one surface in the thickness direction of the first region 21 , and a fifth step of crystallizing the second region 22 by heating.

[0094] (Step 3)

[0095] In the third step, if Figure 2 As shown in FIG. 1B , the first region 21 is arranged on one surface in the thickness direction of the base layer 2 by sputtering.

[0096] When the first region 21 is disposed on one surface in the thickness direction of the base layer 2 by sputtering, the one surface in the thickness direction of the base layer 2 is subjected to a surface treatment as necessary.

[0097] Examples of the surface treatment include corona treatment, plasma treatment, flame treatment, ozone treatment, primer treatment, glow treatment, and saponification treatment.

[0098] Then, in the sputtering method, the target (the material of the first region 21) and the base layer 2 are arranged to face each other in a vacuum chamber. In addition, during the sputtering, the base layer 2 is closely attached to the circumferential direction of the film-forming roller.

[0099] Then, a sputtering gas is supplied and a voltage is applied from a power source to accelerate gas ions and irradiate the target, thereby ejecting the target material from the target surface and depositing the target material on the surface (one surface in the thickness direction) of the base layer 2 to form the first region 21 .

[0100] As the sputtering gas, for example, an inert gas (such as krypton gas, argon gas) and oxygen gas can be cited. As the sputtering gas, it is preferable to use an inert gas and oxygen gas in combination. As the inert gas, it is preferable to argon gas. When argon gas is used as the inert gas, the first region 21 contains argon atoms.

[0101] The amount of oxygen introduced relative to the total amount of the inert gas and oxygen is, for example, 1.0 flow % or more, preferably 2.0 flow % or more, and, for example, 5.0 flow % or less, preferably 3.0 flow % or less.

[0102] The gas pressure during sputtering is, for example, 0.1 Pa or more, preferably 0.2 Pa or more, and, for example, 2.0 Pa or less, preferably 1.0 Pa or less.

[0103] The water partial pressure during sputtering is, for example, greater than 0.5×10 -4 Pa, preferably 0.6×10 -4 Pa or more, more preferably 0.6×10 -4 Pa or more, for example, 1.8×10 -4 Pa or less, preferably 1.5×10 -4 Pa or less, more preferably 1.0×10 -4 Below Pa.

[0104] If the partial pressure of water during sputtering is within the above range, the first region 21 having a non-uniform thickness can be reliably formed.

[0105] Furthermore, if the water partial pressure during sputtering is within the above range, the first region 21 can be maintained amorphous in the fifth step.

[0106] The power source may be, for example, any of a DC power source, an AC power source, an MF power source, and an RF power source, or a combination of these.

[0107] The discharge output is, for example, 1.0 kW or more, preferably 10.0 kW or more, and, for example, 20 kW or less.

[0108] The horizontal magnetic field intensity of the target is, for example, 10 mT or more, preferably 20 mT or more, and, for example, 100 mT or less, preferably 50 mT or less.

[0109] The temperature of the film-forming roller is, for example, 20° C. or lower, preferably 10° C. or lower, more preferably 0° C. or lower, and, for example, -50° C. or higher, preferably -25° C. or higher.

[0110] (Step 4)

[0111] In the fourth step, if Figure 2 As shown in C, the second region 22 is arranged on one surface in the thickness direction of the first region 21 by sputtering.

[0112] Then, in the sputtering method, the target (material of the second region 22) and the first region 21 are arranged opposite to each other in a vacuum chamber. Then, a sputtering gas is supplied and a voltage is applied from a power supply to accelerate gas ions and irradiate the target, so that the target material is ejected from the target surface. And, the target material is deposited on the surface (one side in the thickness direction) of the first region 21 to form the second region 22. In addition, during sputtering, the base layer 2 is closely attached to the circumferential direction of the film-forming roller.

[0113] In addition, as the sputtering gas, for example, inert gas (such as krypton gas, argon gas) and oxygen gas can be cited. As the inert gas, argon gas can be preferably cited. When argon gas is used as the inert gas, the second region 22 contains argon atoms.

[0114] The amount of oxygen introduced relative to the total amount of the inert gas and oxygen is, for example, 0.05 flow % or more, preferably 0.1 flow % or more, and, for example, 5.0 flow % or less, preferably 3.0 flow % or less.

[0115] The gas pressure during sputtering is, for example, 0.1 Pa or more, preferably 0.2 Pa or more, and, for example, 2.0 Pa or less, preferably 1.0 Pa or less.

[0116] The water partial pressure during sputtering is preferably higher than that in the third step, for example, more than 1.8×10 -4 Pa, preferably 2.0×10 -4 Pa or more, for example, 4.0×10 -4 Pa or less, preferably 3.0×10 -4 Pa or less, more preferably 2.5×10 -4 Below Pa.

[0117] If the water partial pressure during sputtering is within the above range, the second region 22 can be reliably crystallized in the fifth step.

[0118] The power source may be, for example, any of a DC power source, an AC power source, an MF power source, and an RF power source, or a combination of these.

[0119] The discharge output is, for example, 1.0 kW or more, preferably 10.0 kW or more, and, for example, 20 kW or less.

[0120] The horizontal magnetic field intensity of the target is, for example, 10 mT or more, and for example, 200 mT or less, preferably 100 mT or less, and more preferably 40 mT or less.

[0121] The temperature of the film-forming roller is, for example, 20° C. or lower, preferably 10° C. or lower, more preferably 0° C. or lower, and, for example, -50° C. or higher, preferably -25° C. or higher.

[0122] (5th step)

[0123] In the fifth step, the second region 22 is crystallized by heating.

[0124] When the second region 22 is crystallized, the second region 22 is heated. Specifically, the second region 22 is heated using a heating roller after sputtering.

[0125] As heating conditions, the heating temperature is, for example, 100° C. or higher, preferably 120° C. or higher, and for example, 250° C. or lower, preferably 200° C. or lower, and the heating time is 10 minutes or longer, and for example, 120 minutes or lower.

[0126] Thus, the second region 22 is crystallized. On the other hand, the first region 21 is not crystallized but maintained in an amorphous state. Specifically, if the partial pressure of water in the third step is within the above range, the total amount of the impurity gas derived from the rare gas and water is at a level suitable for maintaining an amorphous state, so that the first region 21 is not crystallized but maintained in an amorphous state. Furthermore, if the partial pressure of water in the fourth step is within the above range, the amount of impurities is suitable for obtaining crystallinity, so that the second region 22 is crystallized.

[0127] As described above, the light-transmitting conductive sheet 1 can be obtained.

[0128] <Effects>

[0129] The light-transmitting conductive layer 3 includes the crystalline second region 22, and thus has a low resistivity. In addition, the amorphous first region 21 in the light-transmitting conductive layer 3 has a non-uniform thickness, and thus has excellent bendability.

[0130] Specifically, in the light-transmitting conductive layer 3, when the amorphous first region 21 has a non-uniform thickness, stress due to bending is relieved by the first region 21. As a result, the bendability can be improved.

[0131] The light-transmitting conductive sheet 1 includes the light-transmitting conductive layer 3. Therefore, it has a low resistivity and excellent bendability.

[0132] <Modification>

[0133] In the modification, for the same components and processes as those of the first embodiment, the same reference numerals are used and their specific description is omitted. In addition, unless otherwise specified, the modification can achieve the same effects as the first embodiment. In addition, the first embodiment and its modification can be appropriately combined.

[0134] In the above description, the base material layer 2 is formed of the base material 10, and the base material layer 2 may further include a cured resin layer. In this case, the base material layer 2 includes the base material 10 and the cured resin layer in this order toward one side in the thickness direction.

[0135] Examples of the cured resin layer include a dielectric layer and a hard coat layer.

[0136] In addition, in the above description, the crystallization state of the first region 21 and the second region 22 is adjusted by adjusting the water partial pressure in the third process and the fourth process within a prescribed range, but the crystallization state of the first region 21 and the second region 22 can also be adjusted by adjusting the power density in the third process and the fourth process within a prescribed range, for example.

[0137] In the above description, the first surface 13 on the opposite side of the first main surface 11 in the first region 21 has an uneven surface, but the first surface 13 may not have an uneven surface (that is, have a flat surface), and the first main surface 11 may have an uneven surface. In this case, the first region 21 has an uneven thickness. In this case, the second surface 14 in the second region 22 has a flat surface.

[0138] Furthermore, in the first region 21, the first main surface 11 and the first surface 13 may have non-uniform surfaces. In this case, the first region 21 also has a non-uniform thickness. Furthermore, in this case, the second surface 14 in the second region 22 has a non-uniform surface.

[0139] From the viewpoint of improving the bendability, it is preferred that the first surface 13 has an uneven surface and the first main surface 11 has a flat surface in the first region 21. In this case, in the second region 22, the second surface 14 in the second region 22 has an uneven surface.

[0140] Example

[0141] Embodiment and comparative example are shown below, and the present invention is further specifically described.It should be noted that the present invention is not limited to any embodiment and comparative example.In addition, the specific numerical values ​​such as the blending ratio (containing ratio), physical property value, parameter used in the following description can replace the upper limit value (as the numerical value defined as "below", "not enough") or the lower limit value (as the numerical value defined as "above", "exceeding") of the blending ratio (containing ratio), physical property value, parameter, etc. recorded in the above-mentioned "specific embodiments", corresponding thereto.

[0142] <Manufacturing of light-transmitting conductive layer and light-transmitting conductive sheet>

[0143] Example 1

[0144] [1st step]

[0145] A long PET film (thickness 125 μm, manufactured by Mitsubishi Chemical Corporation) was prepared as a substrate. Thus, a substrate layer was prepared.

[0146] [Step 2]

[0147] The light-transmitting conductive layer is disposed on one surface of the substrate layer in the thickness direction by a reactive sputtering method. In the reactive sputtering method, a sputtering film forming apparatus (DC magnetron sputtering apparatus) capable of performing a film forming process by a roll-to-roll method is used.

[0148] (Step 3)

[0149] Specifically, first, the first region is arranged on one surface in the thickness direction of the base material layer.

[0150] Specifically, a sintered body of indium oxide and tin oxide (tin oxide concentration of 12.5 mass%) was used as a target. A DC power supply was used as a power source for applying voltage to the target. The horizontal magnetic field strength on the target was set to 30 mT. In the sputtering device, the substrate layer was closely attached along the circumferential direction of the film-forming roller. The temperature of the film-forming roller was set to -5°C. The sputtering film-forming device was evacuated to a vacuum degree of 0.9×10 -4 After the sputtering, argon gas as a sputtering gas and oxygen gas as a reactive gas were introduced into the sputtering film forming equipment, and the gas pressure in the sputtering film forming equipment was set to 0.2 Pa. In addition, the water partial pressure during sputtering was 0.8×10 -4 Sputtering was performed in an environment of 1000 nm Pa. The ratio of the oxygen gas introduced to the total amount of argon gas and oxygen gas introduced into the sputtering film forming apparatus was about 2.4% by flow rate. Thus, the first region (thickness 5 to 20 nm (minimum thickness 5 nm)) was arranged on one surface in the thickness direction of the base layer.

[0151] (Step 4)

[0152] The second region is arranged on one surface in the thickness direction of the first region.

[0153] Specifically, a sintered body of indium oxide and tin oxide (tin oxide concentration of 12.5 mass%) was used as a target. A DC power supply was used as a power source for applying voltage to the target. The horizontal magnetic field strength on the target was set to 30 mT. In the sputtering device, the substrate layer was closely attached along the circumferential direction of the film-forming roller. The temperature of the film-forming roller was set to -5°C. The sputtering film-forming device was evacuated to a vacuum degree of 0.9×10 -4 Pa, argon gas as a sputtering gas and oxygen gas as a reactive gas were introduced into the sputtering film forming device, and the gas pressure in the sputtering film forming device was set to 0.2 Pa. In addition, the water partial pressure during sputtering was 2.1×10 -4 Sputtering was performed in an environment of 100 to 120 nm (minimum thickness 100 nm) with respect to the total amount of argon and oxygen introduced into the sputtering film forming apparatus, and the ratio of the amount of oxygen introduced was about 2.3% by flow rate. Thus, the second region (thickness 100 to 120 nm (minimum thickness 100 nm)) was arranged on one surface in the thickness direction of the first region.

[0154] (5th step)

[0155] The second region is crystallized by heating. Specifically, it is heated by a hot air oven. The heating temperature is set to 140° C. and the heating time is set to 30 minutes. Thus, the second region is crystallized. On the other hand, the first region is not crystallized but remains amorphous. By the above, a light-transmitting conductive layer and a light-transmitting conductive sheet 1 are manufactured.

[0156] Comparative Example 1

[0157] A light-transmitting conductive layer and a light-transmitting conductive sheet were produced by the same procedure as in Example 1. However, the water partial pressure in the third step was changed to 0.5×10 -4 Pa.

[0158] Comparative Example 2

[0159] A light-transmitting conductive layer and a light-transmitting conductive sheet were produced according to the same procedures as in Example 1. However, the third step was not performed.

[0160] Comparative Example 3

[0161] A light-transmitting conductive layer and a light-transmitting conductive sheet were produced according to the same procedures as in Example 1. However, the fifth step was not performed.

[0162] <Evaluation>

[0163] [Thickness of light-transmitting conductive layer]

[0164] The thickness of the light-transmitting conductive layer (each region) of each embodiment and each comparative example is measured by FE-TEM observation. Specifically, first, a cross-sectional observation sample of the light-transmitting conductive layer of each embodiment and each comparative example is prepared by FIB microsampling method. A FIB device (trade name "FB2200", manufactured by Hitachi) is used in the FIB microsampling method, and the acceleration voltage is set to 10 kV. Then, the thickness of the light-transmitting conductive layer in the cross-sectional observation sample is measured by FE-TEM observation. A FE-TEM device (trade name "JEM-2800", manufactured by JEOL) is used in the FE-TEM observation, and the acceleration voltage is set to 200 kV.

[0165] The thickness of the second region was calculated by subtracting the thickness of the first region from the thickness of the entire light-transmitting conductive layer.

[0166] [Confirmation of whether the first region 2 has uneven thickness]

[0167] The same operation as the evaluation of the thickness of the above-mentioned light-transmitting conductive layer was performed to confirm the cross-sectional image of FE-TEM. Example 1 in which the observation magnification was set to 500,000 times (the horizontal length of the shooting range was 275 nm) and the difference between the thickness at the thickest position of the first region 2 and the thickness at the thinnest position of the first region 21 was 5 nm or more was determined to have an uneven thickness of the first region 2.

[0168] [Resistance value]

[0169] The resistance value (R0) of the light-transmitting conductive layer of each Example and each Comparative Example was measured by a four-terminal method. The resistance value was evaluated based on the following criteria. The results are shown in Table 1.

[0170] {Benchmark}

[0171] ○: Resistance value is 40Ω / □ or less.

[0172] ×: The resistance value exceeds 40Ω / □.

[0173] [Flexibility]

[0174] The bendability of the light-transmitting conductive sheet of each embodiment and each comparative example was evaluated. Specifically, the light-transmitting conductive sheet of each embodiment and each comparative example was cut into pieces with a width of 10 mm and a length of 150 mm, respectively, to prepare a sample. Then, the sample was placed on a core rod so that the light-transmitting conductive layer was on the outside and the other side of the substrate in the thickness direction was in contact with the core rod. Then, both ends of the long side of the light-transmitting conductive sheet were clamped with a clamp, and a weight of 1000 g was placed in the center of the clamp. That is, a load of 100 g / mm relative to the width of the light-transmitting conductive sheet was applied to the lower side to bend the light-transmitting conductive sheet. This bending state lasted for 10 seconds.

[0175] In this bending state, after applying the marker to the bent portion, the bending state is released and the marker portion is observed under a microscope. In this test method, the diameter of the core rod is changed from a large diameter to a small diameter by 1 mm at a time, and the minimum diameter at which no cracks can be confirmed under the microscope in the marker-coated portion is recorded in Table 1. The smaller this value is, the better the bending resistance is. The results are shown in Table 1.

[0176] It should be noted that in the above test, the diameter of the mandrel was changed from a large diameter to a small diameter by 1 mm at a time, and the sample was changed each time it was changed. That is, in the above test, the number of bends was 1 for one sample, and each time it was bent, it was changed to another sample (another sample manufactured under the same conditions).

[0177] [Table 1]

[0178] Table 1

[0179]

[0180] It should be noted that the above invention is provided as an exemplary embodiment of the present invention, but it is merely an example and should not be interpreted as limiting. Modifications of the present invention that are obvious to those skilled in the art are within the scope of the above claims.

[0181] Industrial Applicability

[0182] The light-transmitting conductive layer and the light-transmitting conductive sheet of the present invention are suitably used in the production of various devices such as display panels, touch panels, and solar cells.

Claims

1. A light-transmitting conductive layer comprising a first main surface and a second main surface facing each other in a thickness direction, The first region including the first main surface and the second region including the second main surface are sequentially provided on one side in the thickness direction. The main area of ​​the first area is amorphous, The main region of the second region is crystalline, The first region has a non-uniform thickness.

2. The light-transmitting conductive layer according to claim 1, wherein The second region is thicker than the first region.

3. A light-transmitting conductive sheet comprising: The light-transmitting conductive layer according to claim 1 or 2, and A base material layer is located on the first main surface side of the light-transmitting conductive layer.

Citation Information

Patent Citations

  • TRANSMISSION CONDUCTIVE SHEET, CONTACT SENSOR, Dimming ELEMENT, PHOTOELECTRIC CONVERSION ELEMENT, HEAT WIRE CONTROL MEMBER, ANTENNA,

    CN115666928A

  • Laminate

    WO2023013734A1