Conductive film with high adhesive force and preparation process thereof
By arranging a copper-nickel-titanium mixed layer and an adhesion layer in the ITO conductive film, the problem of conductive film delamination is solved, the adhesion and stability of the coating are improved, and the market demand for high adhesion and high conductivity is met.
Patent Information
- Application Number
- CN202411072561.2
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Filing Date
- 2024-08-06
- Publication Date
- 2024-10-01
AI Technical Summary
Traditional ITO conductive films are prone to delamination problems after improving conductivity, lack of stability in use, and cannot meet the market demand for high adhesion and high conductivity.
By setting a copper-nickel-titanium mixed layer in the ITO conductive film, combined with the adhesion layer and the base layer, and using a specific molar ratio and thickness configuration, the adhesion between the plating layers is improved and the occurrence of delamination is reduced.
It significantly improves the coating adhesion of the conductive film, enhances the stability of use, reduces the occurrence of delamination, and meets the needs of high adhesion and high conductivity.
Smart Images

Figure CN118737532A_ABST
Abstract
Description
Technical Field
[0001] The invention belongs to the technical field of conductive films, and in particular relates to a conductive film with high adhesion and a preparation process thereof. Background Art
[0002] ITO conductive film, i.e. indium tin oxide conductive film, has excellent conductive properties, high visible light transmittance, good film processing performance, and is easy to etch. It is widely used in touch screens. With the rise of smart terminals and large-size touch screens, the requirements for conductivity are getting higher and higher, and the conductivity of traditional ITO conductive film can no longer meet market demand. In order to improve the conductivity of ITO conductive film, setting a metal layer on the ITO conductive film has become an effective and feasible solution, but the problem that comes with it is that the ITO conductive film with a metal layer is prone to stratification problems, and the stability of use needs to be further improved.
[0003] The information disclosed in this background technology section is only intended to enhance the understanding of the overall background of the invention and should not be regarded as an acknowledgment or any form of suggestion that the information constitutes the prior art already known to a person skilled in the art. Summary of the invention
[0004] The object of the present invention is to provide a conductive film with high adhesion and a preparation process thereof, wherein the conductive film has excellent adhesion between the plating layers, so that the conductive film has better stability in use.
[0005] In order to achieve the above object, a technical solution provided by a specific embodiment of the present invention is as follows:
[0006] A high-adhesion conductive film comprises a substrate layer, wherein the substrate layer is sequentially stacked with an upper coating layer, a primer layer, a silicon-aluminum mixed layer, an ITO layer, an adhesion layer, a copper-nickel-titanium mixed layer and a copper layer;
[0007] The molar ratio of copper, nickel and titanium in the copper-nickel-titanium mixed layer is (20-45): (50-70): (1-10).
[0008] In one or more embodiments of the present invention, the copper-nickel-titanium mixed layer has a thickness of 2-100 nm.
[0009] In one or more embodiments of the present invention, the material of the adhesion layer is SiO 2 、Ti、TiO 2 、Si、Al 2 O 3 MgF 2 、SiO、HfO 2 SnO 2 and Y 2 O 3; and / or, the thickness of the adhesion layer is 1-20nm.
[0010] In one or more embodiments of the present invention, the base material is selected from SiO 2 、Ti、TiO 2 、Si、Al 2 O 3 MgF 2 、SiO、HfO 2 SnO 2 and Y 2 O 3 ; and / or, the thickness of the base layer is 0.2-20nm.
[0011] In one or more embodiments of the present invention, the molar ratio of silicon to aluminum in the silicon-aluminum mixed layer is (75-99): (1-25); and / or the thickness of the silicon-aluminum mixed layer is 2-80 nm.
[0012] In one or more embodiments of the present invention, the substrate layer is selected from a PET layer, a transparent PI layer, a TAC layer, a COP layer and a PC layer; and / or the thickness of the substrate layer is 5.7-250 μm; and / or the thickness of the ITO layer is 5-100 nm; and / or the thickness of the copper layer is 100-1000 nm.
[0013] Another specific embodiment of the present invention provides a technical solution as follows:
[0014] The preparation process of the conductive film with high adhesion includes the following steps:
[0015] An upper coating layer and a lower coating layer are respectively arranged on both sides of the substrate layer, and a high temperature protective film is arranged on the lower coating layer;
[0016] A primer layer, a silicon-aluminum mixed layer, an ITO layer, an adhesion layer, a copper-nickel-titanium mixed layer and a copper layer are sequentially plated on the upper coating layer;
[0017] A positive protective film is provided on the copper layer.
[0018] In one or more embodiments of the present invention, the vacuum degree during plating is 1*10 -4 Below pa.
[0019] In one or more embodiments of the present invention, the water vapor value is 9*10 -5 Below pa.
[0020] In one or more embodiments of the present invention, during plating, the reaction gas is a mixed gas of argon, nitrogen and oxygen, and the flow ratio of argon, nitrogen and oxygen is (60-80): (20-35): (5-10).
[0021] Compared with the prior art, the conductive film of the present invention greatly improves the adhesion between the coatings by providing a copper-nickel-titanium mixed layer, and effectively reduces the situation in which the conductive film is delaminated during use and affects the stability of use. BRIEF DESCRIPTION OF THE DRAWINGS
[0022] In order to more clearly illustrate the embodiments of the present invention or the technical solutions in the prior art, the drawings required for use in the embodiments or the description of the prior art will be briefly introduced below. Obviously, the drawings described below are only some embodiments recorded in the present invention. For ordinary technicians in this field, other drawings can be obtained based on these drawings without paying creative work.
[0023] Figure 1 A structural diagram of a conductive film with high adhesion according to an embodiment of the present invention;
[0024] Description of main reference numerals:
[0025] 1-high temperature protective film, 2-lower coating layer, 3-substrate layer, 4-upper coating layer, 5-base layer, 6-silicon-aluminum mixed layer, 7-ITO layer, 8-adhesion layer, 9-copper-nickel-titanium mixed layer, 10-copper layer, 11-positive protective film. DETAILED DESCRIPTION
[0026] In order to enable those skilled in the art to better understand the technical solutions in the present invention, the technical solutions in the embodiments of the present invention will be clearly and completely described below in conjunction with the drawings in the embodiments of the present invention. Obviously, the described embodiments are only part of the embodiments of the present invention, not all of the embodiments. Based on the embodiments of the present invention, all other embodiments obtained by ordinary technicians in this field without creative work should fall within the scope of protection of the present invention.
[0027] A specific embodiment of the present invention provides a high-adhesion conductive film, including a substrate layer, wherein the substrate layer is sequentially stacked with an upper coating layer, a primer layer, a silicon-aluminum mixed layer, an ITO layer, an adhesion layer, a copper-nickel-titanium mixed layer and a copper layer; wherein the molar ratio of copper, nickel and titanium in the copper-nickel-titanium mixed layer is (20-45): (50-70): (1-10).
[0028] Specifically, a copper-nickel-titanium mixed layer is provided between the ITO layer and the copper layer to enhance the adhesion between the coatings. The copper-nickel-titanium mixed layer is mainly nickel, supplemented by copper, and a small amount of titanium is added, so that the copper-nickel-titanium mixed layer effectively plays a role in improving the adhesion of the coatings. In addition, an adhesion layer is provided to further improve the adhesion between the coatings, and combined with a base layer, the overall stability of the conductive film is greatly improved, reducing the occurrence of stratification.
[0029] In a specific embodiment, the copper-nickel-titanium mixed layer has a thickness of 2-100 nm.
[0030] Specifically, by controlling the thickness of the copper-nickel-titanium mixed layer, the adhesion of the coating can be effectively improved.
[0031] In one specific embodiment, the adhesion layer is made of SiO 2 、Ti、TiO 2 、Si、Al 2 O 3 MgF 2 、SiO、HfO 2 SnO 2 and Y 2 O 3 ; The thickness of the adhesion layer is 1-20nm; The base material is selected from SiO 2 、Ti、TiO 2 、Si、Al 2 O 3 MgF 2 、SiO、HfO 2 SnO 2 and Y 2 O 3 ; The thickness of the base layer is 0.2-20nm.
[0032] Specifically, the material and thickness of the adhesion layer and the base layer will affect the adhesion between the coatings. 2 (silicon dioxide), Ti (titanium), TiO 2 (titanium dioxide), Si (silicon), Al 2 O 3 (alumina), MgF 2 (magnesium fluoride), SiO (silicon monoxide), HfO 2 (Hafnium dioxide), SnO 2 (tin oxide) and Y 2 O 3 (Yttrium oxide) material is plated with an adhesion layer and a base layer, while controlling the thickness, which has a significant effect on improving the adhesion between the coatings.
[0033] In a specific embodiment, the substrate layer is selected from a PET layer, a transparent PI layer, a TAC layer, a COP layer and a PC layer; the thickness of the substrate layer is 5.7-250 μm; the thickness of the ITO layer is 5-100 nm; and the thickness of the copper layer is 100-1000 nm.
[0034] Specifically, controlling the thickness of the ITO layer and the copper layer can ensure that the conductive film has excellent conductivity, and at the same time, the coating layers can maintain a high adhesion to reduce the occurrence of delamination. The PET layer is a polyethylene terephthalate layer, the PI layer is a polyimide layer, the TAC layer is a triacetyl cellulose layer, the COP layer is a cycloolefin polymer layer, and the PC layer is a polycarbonate layer. Selecting the above types of substrate layers can ensure that the conductive film has good light transmittance and can also promote the effective adhesion of the base layer on the substrate layer.
[0035] Another specific embodiment of the present invention provides a preparation process for a high-adhesion conductive film, comprising the following steps: respectively providing an upper coating layer and a lower coating layer on both sides of a substrate layer, and providing a high-temperature protective film on the lower coating layer; sequentially plating a primer layer, a silicon-aluminum mixed layer, an ITO layer, an adhesion layer, a copper-nickel-titanium mixed layer and a copper layer on the upper coating layer; and providing a positive protective film on the copper layer.
[0036] Specifically, during plating, the vacuum degree is 1×10 -4 Pa or less, the water vapor value is 9×10 -5 Pa or less, the reaction gas is a mixture of argon, nitrogen and oxygen, and the flow ratio of argon, nitrogen and oxygen is (60-80): (20-35): (5-10). By controlling the vacuum degree, water vapor value and reaction gas, a dense and uniform film layer can be formed during plating, which can promote effective bonding between the coatings and ensure the adhesion of the coating.
[0037] In a specific embodiment, both the upper coating layer and the lower coating layer are formed by coating an acrylic resin coating liquid.
[0038] Specifically, the acrylic resin coating liquid is a conventional product in the art, and coating the acrylic resin coating liquid can improve the heat and humidity resistance and visible light transmittance of the conductive film.
[0039] The present invention is further described in detail below in conjunction with specific embodiments.
[0040] Example 1
[0041] The high-adhesion conductive film includes, from bottom to top, a 60μm thick PET film, a 20nm thick lower coating layer, a 50μm thick substrate layer, a 40nm thick upper coating layer, a 0.2nm thick primer layer, a 10nm thick silicon-aluminum mixed layer, a 30nm thick ITO layer, a 10nm thick adhesion layer, a 15nm thick copper-nickel-titanium mixed layer, a 300nm thick copper layer, and a 50μm thick CPP film. The upper coating layer and the lower coating layer are both formed by coating an acrylic resin coating liquid, the substrate layer is a PET layer, and the primer layer is made of SiO 2 The molar ratio of silicon to aluminum in the silicon-aluminum mixed layer is 75:25, and the material of the adhesion layer is TiO 2The molar ratio of copper, nickel and titanium in the copper-nickel-titanium mixed layer is 20:70:10.
[0042] During the preparation process, magnetron sputtering technology was used to plate the coating layer, the primer layer, the silicon-aluminum mixed layer, the ITO layer, the adhesion layer, the copper-nickel-titanium mixed layer and the copper layer on the substrate layer. During the plating, the vacuum degree was controlled to 1×10 -5 pa, the water vapor value is controlled at 8.5×10 -5 pa, the reaction gas is a mixed gas of argon, nitrogen and oxygen, and the flow ratio of argon, nitrogen and oxygen is 60:35:10.
[0043] Example 2
[0044] The conductive film with high adhesion includes, from bottom to top, a 120μm thick PET film, a 300nm thick lower coating layer, a 100μm thick substrate layer, a 200nm thick upper coating layer, a 9nm thick primer layer, a 2nm thick silicon-aluminum mixed layer, a 5nm thick ITO layer, a 1nm thick adhesion layer, a 2nm thick copper-nickel-titanium mixed layer, a 100nm thick copper layer, and a 50μm thick CPP film. The upper coating layer and the lower coating layer are both formed by coating an acrylic resin coating liquid, the substrate layer is a PET layer, and the primer layer is made of SiO 2 The molar ratio of silicon to aluminum in the silicon-aluminum mixed layer is 99:1, and the material of the adhesion layer is TiO 2 The molar ratio of copper, nickel and titanium in the copper-nickel-titanium mixed layer is 20:70:10.
[0045] During the preparation process, magnetron sputtering technology was used to plate the coating layer, the primer layer, the silicon-aluminum mixed layer, the ITO layer, the adhesion layer, the copper-nickel-titanium mixed layer and the copper layer on the substrate layer. During the plating, the vacuum degree was controlled to 1×10 -5 pa, the water vapor value is controlled at 8.5×10 -5 pa, the reaction gas is a mixed gas of argon, nitrogen and oxygen, and the flow ratio of argon, nitrogen and oxygen is 80:20:5.
[0046] Example 3
[0047] The conductive film with high adhesion includes, from bottom to top, a 30μm thick PET film, a 650nm thick lower coating layer, a 38μm thick substrate layer, a 600nm thick upper coating layer, a 14nm thick primer layer, a 45nm thick silicon-aluminum mixed layer, a 60nm thick ITO layer, a 20nm thick adhesion layer, a 100nm thick copper-nickel-titanium mixed layer, a 750nm thick copper layer and a 50μm thick CPP film. The upper coating layer and the lower coating layer are both formed by coating an acrylic resin coating liquid, the substrate layer is a PET layer, and the primer layer is made of SiO 2 The molar ratio of silicon to aluminum in the silicon-aluminum mixed layer is 75:25, and the material of the adhesion layer is TiO 2The molar ratio of copper, nickel and titanium in the copper-nickel-titanium mixed layer is 20:70:10.
[0048] During the preparation process, magnetron sputtering technology was used to plate the coating layer, the primer layer, the silicon-aluminum mixed layer, the ITO layer, the adhesion layer, the copper-nickel-titanium mixed layer and the copper layer on the substrate layer. During the plating, the vacuum degree was controlled to 1×10 -5 pa, the water vapor value is controlled at 8.5×10 -5 pa, the reaction gas is a mixed gas of argon, nitrogen and oxygen, and the flow ratio of argon, nitrogen and oxygen is 60:35:10.
[0049] Example 4
[0050] The conductive film with high adhesion includes, from bottom to top, a 188μm thick PET film, a 1200nm thick lower coating layer, a 250μm thick substrate layer, a 1200nm thick upper coating layer, a 20nm thick primer layer, an 80nm thick silicon-aluminum mixed layer, a 100nm thick ITO layer, a 13nm thick adhesion layer, a 65nm thick copper-nickel-titanium mixed layer, a 1000nm thick copper layer and a 50μm thick CPP film. The upper coating layer and the lower coating layer are both formed by coating an acrylic resin coating liquid, the substrate layer is a PET layer, and the primer layer is made of SiO 2 The molar ratio of silicon to aluminum in the silicon-aluminum mixed layer is 75:25, and the material of the adhesion layer is TiO 2 The molar ratio of copper, nickel and titanium in the copper-nickel-titanium mixed layer is 20:70:10.
[0051] During the preparation process, magnetron sputtering technology was used to plate the coating layer, the primer layer, the silicon-aluminum mixed layer, the ITO layer, the adhesion layer, the copper-nickel-titanium mixed layer and the copper layer on the substrate layer. During the plating, the vacuum degree was controlled to 1×10 -5 pa, the water vapor value is controlled at 8.5×10 -5 pa, the reaction gas is a mixed gas of argon, nitrogen and oxygen, and the flow ratio of argon, nitrogen and oxygen is 60:35:10.
[0052] Example 5
[0053] The only difference between this embodiment and embodiment 1 is that the molar ratio of copper, nickel and titanium in the copper-nickel-titanium mixed layer is 30:60:5.
[0054] Example 6
[0055] The only difference between this embodiment and embodiment 1 is that the molar ratio of copper, nickel and titanium in the copper-nickel-titanium mixed layer is 45:50:1.
[0056] Example 7
[0057] The only difference between this embodiment and Embodiment 1 is that the thickness of the copper-nickel-titanium mixed layer is 2 nm.
[0058] Example 8
[0059] The only difference between this embodiment and embodiment 1 is that the thickness of the copper-nickel-titanium mixed layer is 100 nm.
[0060] Example 9
[0061] The only difference between this embodiment and embodiment 1 is that the thickness of the copper-nickel-titanium mixed layer is 150 nm.
[0062] Example 10
[0063] The difference between this embodiment and embodiment 1 is that the material of the adhesion layer is SiO 2 .
[0064] Embodiment 11
[0065] The difference between this embodiment and embodiment 1 is that the material of the adhesion layer is Al 2 O 3 .
[0066] Example 12
[0067] The difference between this embodiment and embodiment 1 is that the material of the adhesion layer is Y 2 O 3 .
[0068] Comparative Example 1
[0069] The only difference between this comparative example and Example 1 is that the molar ratio of copper, nickel and titanium in the copper-nickel-titanium mixed layer is 10:30:20.
[0070] Comparative Example 2
[0071] The only difference between this comparative example and Example 1 is that the copper-nickel-titanium layer is replaced by a copper-nickel layer, and the molar ratio of copper to nickel in the copper-nickel layer is 20:80.
[0072] Comparative Example 3
[0073] The only difference between this comparative example and Example 1 is that the copper-nickel-titanium layer is replaced by a nickel-titanium layer, and the molar ratio of nickel to titanium in the nickel-titanium layer is 90:10.
[0074] Comparative Example 4
[0075] The only difference between this comparative example and Example 1 is that the copper-nickel-titanium layer is replaced by a copper-titanium layer, and the molar ratio of copper to titanium in the copper-titanium layer is 90:10.
[0076] Comparative Example 5
[0077] The only difference between this comparative example and Example 1 is that the copper-nickel-titanium mixed layer is replaced by a nickel layer.
[0078] Comparative Example 6
[0079] The only difference between this comparative example and Example 1 is that the copper-nickel-titanium mixed layer is replaced by a silver layer.
[0080] Comparative Example 7
[0081] The only difference between this comparative example and Example 1 is that the copper-nickel-titanium mixed layer is replaced by a titanium dioxide layer.
[0082] Comparative Example 8
[0083] The only difference between this comparative example and Example 1 is that the copper-nickel-titanium mixed layer is replaced by a nickel-chromium layer, and the molar ratio of nickel to chromium in the nickel-chromium layer is 80:20.
[0084] Comparative Example 9
[0085] The only difference between this comparative example and Example 1 is that the copper-nickel-titanium mixed layer is replaced by a chromium layer.
[0086] Comparative Example 10
[0087] The difference between this comparative example and Example 1 is that the adhesion layer is removed.
[0088] The conductive films in the embodiments and comparative examples were prepared by the above-mentioned preparation method, and the following performance tests were performed:
[0089] (1) After the ITO layer is plated, the conductive film is removed from the machine and placed flat on the table. The surface square resistance is tested with a square resistance meter. The width of the conductive film is 1550 mm. 12 points are taken on average according to the width to test the square resistance. The conductive film is then placed in an oven and crystallized at 155° C. for 5 min. The corresponding square resistance is then tested. Two samples of each of the conductive films in Example 1 and Comparative Example 1 are tested. The results are shown in Table 1.
[0090] Table 1 Square resistance test results after ITO layer plating
[0091]
[0092] Note: The unit in Table 1 is Ω / □.
[0093] (2) After the copper layer is plated, the conductive film is removed from the machine and placed flat on the table. The surface square resistance is tested with a square resistance meter. The width of the conductive film is 1550 mm. 12 points are taken on average according to the width to test the square resistance. Two samples of each of the conductive films in Example 1 and Comparative Example 1 are tested, and the results are shown in Table 2.
[0094] Table 2 Square resistance test results after copper layer plating
[0095]
[0096]
[0097] Note: The unit in Table 2 is Ω / □.
[0098] (3) The width of the conductive film is 1550 mm. It is evenly divided into three sections according to the width of the conductive film. A grid knife is used to cut the grids, and then 3M 600 tape is used. After pressing and laminating, the tape is left to stand for more than 30 seconds and then pulled off. No peeling is 5B, slight peeling is 3-4B, barely OK, and 2B or less is NG. The results are shown in Table 3.
[0099] Table 3 Adhesion test results
[0100]
[0101]
[0102] Combining Table 1 and Table 2, after ITO layer is plated, the coating resistance is required to reach 120-150Ω, and after copper layer is plated, the coating resistance is required to reach 0.2±0.1Ω. It can be seen from Table 1 and Table 2 that the conductive films in Example 1 and Comparative Example 1 meet the requirements, show high stability, and meet the requirements of industrial production.
[0103] Referring to Table 3, compared with Comparative Examples 1-9, the conductive film in the embodiment of the present invention exhibits better adhesion, indicating that the adhesion between the conductive film coatings can be significantly improved by providing a copper-nickel-titanium mixed layer and plating at a specific molar ratio.
[0104] It can be seen from Example 1 and Examples 7-9 that the thickness of the copper-nickel-titanium mixed layer will affect the adhesion between the coatings. Setting the thickness according to the thickness disclosed in the present invention can achieve better adhesion between the coatings.
[0105] In combination with Example 1 and Comparative Example 10, by providing an adhesion layer so that the adhesion layer and the copper-nickel-titanium mixed layer cooperate with each other, it can be effectively ensured that the conductive film has better adhesion.
[0106] It will be apparent to those skilled in the art that the invention is not limited to the details of the exemplary embodiments described above and that the invention can be implemented in other specific forms without departing from the spirit or essential features of the invention. Therefore, the embodiments should be considered exemplary and non-limiting in all respects, and the scope of the invention is defined by the appended claims rather than the foregoing description, and it is intended that all variations falling within the meaning and scope of the equivalent elements of the claims be included in the invention. Any reference numeral in a claim should not be considered as limiting the claim to which it relates.
[0107] In addition, it should be understood that although the present specification is described according to implementation modes, not every implementation mode contains only one independent technical solution. This description of the specification is only for the sake of clarity. Those skilled in the art should regard the specification as a whole. The technical solutions in each embodiment may also be appropriately combined to form other implementation modes that can be understood by those skilled in the art.
Claims
1. A highly adhesive conductive film, characterized in that: The method comprises a substrate layer, wherein the substrate layer is sequentially stacked with an upper coating layer, a primer layer, a silicon-aluminum mixed layer, an ITO layer, an adhesion layer, a copper-nickel-titanium mixed layer and a copper layer; The molar ratio of copper, nickel and titanium in the copper-nickel-titanium mixed layer is (20-45): (50-70): (1-10).
2. The conductive film with high adhesion according to claim 1, characterized in that: The thickness of the copper-nickel-titanium mixed layer is 2-100 nm.
3. The highly adhesive conductive film according to claim 1, characterized in that: The material of the adhesion layer is SiO2, Ti, TiO2, Si, Al2O3, MgF2, SiO, HfO2, SnO2 and Y2O3; and / or the thickness of the adhesion layer is 1-20nm.
4. The highly adhesive conductive film according to claim 1, characterized in that: The base layer material is selected from SiO2, Ti, TiO2, Si, Al2O3, MgF2, SiO, HfO2, SnO2 and Y2O3; and / or, the thickness of the base layer is 0.2-20nm.
5. The highly adhesive conductive film according to claim 1, characterized in that: The molar ratio of silicon to aluminum in the silicon-aluminum mixed layer is (75-99): (1-25); and / or the thickness of the silicon-aluminum mixed layer is 2-80 nm.
6. The highly adhesive conductive film according to claim 1, characterized in that: The substrate layer is selected from a PET layer, a transparent PI layer, a TAC layer, a COP layer and a PC layer; and / or the thickness of the substrate layer is 5.7-250 μm; and / or the thickness of the ITO layer is 5-100 nm; and / or the thickness of the copper layer is 100-1000 nm.
7. The process for preparing a conductive film with high adhesion according to any one of claims 1 to 6, characterized in that: The steps include: An upper coating layer and a lower coating layer are respectively arranged on both sides of the substrate layer, and a high temperature protective film is arranged on the lower coating layer; A primer layer, a silicon-aluminum mixed layer, an ITO layer, an adhesion layer, a copper-nickel-titanium mixed layer and a copper layer are sequentially plated on the upper coating layer; A positive protective film is provided on the copper layer.
8. The process for preparing a conductive film with high adhesion according to claim 7, characterized in that: During plating, the vacuum degree is 1×10 -4 Below pa.
9. The process for preparing a conductive film with high adhesion according to claim 7, characterized in that: During plating, the water vapor value is 9×10 -5 Below pa.
10. The process for preparing a conductive film with high adhesion according to claim 7, characterized in that: During plating, the reaction gas is a mixed gas of argon, nitrogen and oxygen, and the flow ratio of argon, nitrogen and oxygen is (60-80): (20-35): (5-10).