Method for preparing lanthanum-cerium rare earth permanent magnet material through grain boundary diffusion

Through the grain boundary diffusion method, the coating of acrylate oligomer and grain boundary diffusion powder is used to form a continuous grain boundary phase in the lanthanum cerium rare earth permanent magnet material, which solves the problem of coercive force control of the lanthanum cerium iron boron permanent magnet material and realizes More uniform diffusion and higher magnetic properties.

CN118737602AInactive Publication Date: 2024-10-01GANZHOU JIATON ADVANCED MATERIALS

Patent Information

Application Number
CN202410814965.8
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Filing Date
2024-06-24
Publication Date
2024-10-01
Estimated Expiration
Not applicable · inactive patent

AI Technical Summary

Technical Problem

The existing technology cannot accurately control the coercive force of the lanthanum cerium iron boron permanent magnet material. The coating powder has poor binding force with the magnet, resulting in uneven diffusion at high temperatures, and cannot effectively improve the magnetic properties of the magnet.

Method used

Using the grain boundary diffusion method, the alloy powder is molded into a magnet body, coated with a coating mixed with acrylate oligomer and grain boundary diffusion powder, and formed through magnetron sputtering and heat treatment to form a continuous grain boundary phase with a different melting point to promote Diffusion of rare earth elements.

Benefits of technology

The coercive force and magnetic properties of the lanthanum cerium rare earth permanent magnet material are improved, ensuring the uniformity and stability of diffusion, avoiding the problem of powder shedding, and improving the overall performance of the magnet.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN118737602A_ABST
    Figure CN118737602A_ABST
Patent Text Reader

Abstract

The invention discloses a method for preparing a lanthanum-cerium rare earth permanent magnet material through grain boundary diffusion, and relates to the technical field of rare earth permanent magnet materials. According to the method for preparing the lanthanum-cerium rare earth permanent magnet material through grain boundary diffusion, after alloy powder is subjected to compression molding, the surface of the alloy powder is coated with a coating, and grain boundary diffusion treatment is carried out; the coating comprises grain boundary diffusion powder and an acrylate oligomer, the acrylate oligomer is prepared by polymerizing hexafluorobutyl acrylate, hydroxyethyl methylacrylate and ethyl acetate, so that the alloy powder is prevented from falling off during grain boundary diffusion, and the coercive force of the permanent magnet material is improved; the coating is coated on the surface of compression-molded alloy powder to obtain a low-melting-point continuous grain boundary phase, so that the diffusion magnet has a smooth diffusion channel, and the coercive force of the permanent magnet material is improved.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The invention relates to the technical field of permanent magnet material preparation, in particular to a method for preparing lanthanum cerium rare earth permanent magnet material by grain boundary diffusion. Background Art

[0002] With the development of information technology, automation technology and new energy technology, the production of NdFeB permanent magnet materials has continued to increase, which has greatly increased the use of metal neodymium. Rare earth ores are mostly associated ores, and the main rare earth elements they contain are lanthanum and cerium, of which cerium accounts for about 50% of all rare earth elements. The mining and use of metal neodymium has caused a large backlog of rare earth metals lanthanum and cerium, and the relatively low price has prompted people to start researching lanthanum cerium iron boron permanent magnet materials.

[0003] The usual coating process is to coat the heavy rare earth powder and then perform heat treatment to increase the coercive force of the magnet, but this method cannot accurately control the coercive force of the magnet, let alone increase the coercive force as needed. The key problem is that the powder coated on the magnet has a poor bonding force with the magnet. At low temperatures, the powder can be bonded to the surface of the magnet by an adhesive, but as the temperature rises, the adhesive evaporates and is sucked away by the vacuum system. The loose powder originally bonded to the surface of the magnet may fall off or become dusty. The total amount of rare earth powder diffused at high temperatures cannot be well controlled. Therefore, the usual heavy rare earth powder coating method cannot accurately control the increase in coercive force.

[0004] For example, the patent application with publication number CN106409497A discloses a method for grain boundary diffusion of NdFeB magnets. The specific operation steps are as follows: prepare the main phase alloy powder by NdFeB powder metallurgy process; prepare the grain boundary powder of low melting point rare earth alloy by grain boundary diffusion powder metallurgy process; mix the main phase alloy powder and the grain boundary powder of low melting point rare earth alloy in proportion; orient and shape in a magnetic field to obtain a blank NdFeB magnet, which can increase the diffusion depth of heavy rare earth elements in the magnet and improve the uniformity of the magnet after diffusion.

[0005] The patent application with publication number CN111091944A discloses a lanthanum-rich cerium-yttrium multi-phase fine-grained rare earth permanent magnet material and its preparation method. Based on the characteristics of spark plasma sintering technology, such as fast heating speed, short heating time and short holding time, the mutual diffusion and chemical heterogeneity of the internal elements of the lanthanum-rich cerium-yttrium multi-phase magnet are controlled, and various core-shell morphologies, magnetic hardening and pinning effects are precisely controlled to improve the coercive force of the magnet.

[0006] Although the permanent magnetic material prepared by the above patent application reduces the production cost, the comprehensive magnetic properties of the prepared permanent magnetic material still need to be improved. Therefore, the present invention studies a lanthanum-cerium rare earth permanent magnetic material prepared by grain boundary diffusion. Summary of the invention

[0007] The object of the present invention is to provide a method for preparing lanthanum-cerium rare earth permanent magnet materials by grain boundary diffusion, so as to solve the problems raised in the above background technology.

[0008] In order to solve the above technical problems, the present invention provides the following technical solutions: a method for preparing lanthanum-cerium rare earth permanent magnet material by grain boundary diffusion, wherein the lanthanum-cerium rare earth permanent magnet material is prepared by coating component B on the surface of component A and then subjecting it to magnetron sputtering; component A is a magnet blank formed by molding alloy powder; component B is a coating; the alloy powder includes neodymium powder, iron powder, boron powder, aluminum powder, lanthanum powder and cerium powder; the average particle size of the alloy powder is 1 to 4 μm; the coating includes grain boundary diffusion powder and acrylate oligomer.

[0009] Preferably, the grain boundary diffusion powder is aluminum, calcium and neodymium in a mass ratio of 1 to 2:8:40.

[0010] Preferably, the acrylate oligomer is prepared by polymerization of hexafluorobutyl acrylate, hydroxyethyl methacrylate and ethyl acetate.

[0011] Preferably, the method for preparing lanthanum-cerium rare earth permanent magnet material by grain boundary diffusion comprises the following specific steps:

[0012] S1: putting alloy powder into a mold, and pressing it at 35-40 MPa to obtain a magnet blank;

[0013] S2: mixing the grain boundary diffusion powder and the acrylate oligomer in a mass ratio of 50-80:1-3, stirring evenly, and preparing a coating;

[0014] S3 uniformly coating the coating on the surface of the magnet blank, with the mass ratio of the coating to the magnet being 3 to 6:100, to obtain a magnet;

[0015] S4 places the magnet in a vacuum furnace, performs heat treatment at 500-600°C for 30-90 minutes, performs grain boundary diffusion treatment, and finally performs low temperature tempering at 450-480°C to obtain lanthanum-cerium rare earth permanent magnet material.

[0016] Preferably, in the above step S1: the alloy powder is obtained by mixing neodymium powder, iron powder, boron powder, aluminum powder, lanthanum powder and cerium powder, and mechanically crushing and grinding them.

[0017] Preferably, in the above step S2: the preparation method of the acrylate oligomer is: under a nitrogen atmosphere, the mixed liquid is heated to 62-65° C., 0.2-0.4 times of 2-mercaptoethanol and 0.03-0.06 times of the total volume of the mixed liquid are added dropwise at a rate of 1-3 ml / min. After reacting for 2-3 hours, 0.01-0.02 times of the total volume of the mixed liquid is continued to be added dropwise with the initiator, and 0.4-0.5 times of the total volume of the mixed liquid is added dropwise at a rate of 1-3 ml / min. After continuing the reaction for 2-3 hours, rotary evaporation is performed to obtain the acrylate oligomer.

[0018] Preferably, the mixed liquid is prepared by mixing hexafluorobutyl acrylate, hydroxyethyl methacrylate and ethyl acetate in a mass ratio of 1:2-4:4-6; the initiator is prepared by mixing 4,4'-azobis(4-cyanopentanol) and ethanol in a mass ratio of 1:5-7 and stirring evenly.

[0019] Preferably, in the above step S4: the temperature during grain boundary diffusion is 850-950° C., and the time is 2-6 hours.

[0020] Preferably, the lanthanum-cerium rare earth permanent magnet material prepared by grain boundary diffusion according to the method for preparing lanthanum-cerium rare earth permanent magnet material by grain boundary diffusion comprises the following components in mass percentage: 49-51% neodymium, 24-25% iron, 18-20% boron, 0.2-0.6% aluminum, 1-3% lanthanum, 0.6-0.8% cerium and 1-2% calcium.

[0021] Compared with the prior art, the beneficial effects achieved by the present invention are:

[0022] The lanthanum-cerium rare earth permanent magnet material is prepared by grain boundary diffusion in the present invention, wherein component B is coated on the surface of component A and then subjected to magnetron sputtering, component A is a magnet blank formed by molding alloy powder, and component B is a coating;

[0023] The coating comprises grain boundary diffusion powder and acrylate oligomer; the acrylate oligomer is prepared by polymerization of hexafluorobutyl acrylate, hydroxyethyl methacrylate and ethyl acetate; the grain boundary diffusion powder and the acrylate oligomer are mixed to form a coating which adheres to the surface of the magnet blank, so that the grain boundary diffusion powder is combined with the magnet, thereby avoiding the falling off of the alloy powder during grain boundary diffusion and improving the coercive force of the permanent magnet material;

[0024] The coating is applied to the surface of the magnet to form a continuous grain boundary phase with a melting point difference. During the heat treatment process, the surface grain boundary diffusion powder is in a semi-molten state and then continuously diffuses along the molten grain boundaries into the internal grain boundaries and the surface of the grains of the magnet to obtain a continuous grain boundary phase with a low melting point, thereby ensuring that the diffusion magnet has a smooth diffusion channel and improving the coercive force of the permanent magnet material. BRIEF DESCRIPTION OF THE DRAWINGS

[0025] Figure 1 This is a microscopic image of the lanthanum-cerium rare earth permanent magnet material prepared by grain boundary diffusion in Example 2 of the present invention. DETAILED DESCRIPTION

[0026] The technical solution of the present invention will be clearly and completely described below in conjunction with the embodiments of the present invention. Obviously, the described embodiments are only part of the embodiments of the present invention, not all of the embodiments. Based on the embodiments of the present invention, all other embodiments obtained by ordinary technicians in this field without creative work are within the scope of protection of the present invention.

[0027] Example 1

[0028] The present embodiment includes the following components in mass percentage: 49% neodymium, 24% iron, 18% boron, 0.6% aluminum, 3% lanthanum, 0.8% cerium and 1% calcium;

[0029] The method for preparing lanthanum-cerium rare earth permanent magnet material by grain boundary diffusion in this embodiment is as follows:

[0030] S1: mixing neodymium powder, iron powder, boron powder, aluminum powder, lanthanum powder and cerium powder, mechanically crushing and grinding to obtain alloy powder; placing the alloy powder into a mold, and performing compression molding at 35 MPa to obtain a magnet blank;

[0031] S2: Hexafluorobutyl acrylate, hydroxyethyl methacrylate and ethyl acetate are mixed in a mass ratio of 1:2:4 to obtain a mixed liquid; 4,4'-azobis(4-cyanopentanol) and ethanol are mixed in a mass ratio of 1:5 and stirred to obtain an initiator; under a nitrogen atmosphere, the mixed liquid is heated to 62°C, 0.2 times of 2-mercaptoethanol and 0.03 times of the total volume of the mixed liquid are added dropwise at a rate of 1 ml / min, and after reacting for 2 hours, 0.01 times of the total volume of the mixed liquid are added dropwise, and 0.4 times of the total volume of the mixed liquid are added dropwise at a rate of 1 ml / min, and after continuing to react for 2 hours, rotary evaporation is performed to obtain an acrylate oligomer; grain boundary diffusion powder and acrylate oligomer are mixed in a mass ratio of 50:1, stirred to obtain a coating, and the grain boundary diffusion powder is aluminum, calcium and neodymium in a mass ratio of 1:5:40;

[0032] S3 uniformly coating the coating on the surface of the magnet blank, with the mass ratio of the coating to the magnet being 3:100, to obtain a magnet;

[0033] S4 places the magnet in a vacuum furnace and performs heat treatment at 500°C for 30 minutes, then performs grain boundary diffusion treatment at a temperature of 850°C for 2 hours, and finally performs low-temperature tempering at 450°C to obtain lanthanum-cerium rare earth permanent magnet material.

[0034] Example 2

[0035] The present embodiment includes the following components in mass percentage: 50% neodymium, 25% iron, 19% boron, 0.4% aluminum, 2% lanthanum, 0.7% cerium and 1.5% calcium;

[0036] The method for preparing lanthanum-cerium rare earth permanent magnet material by grain boundary diffusion in this embodiment is as follows:

[0037] S1: mixing neodymium powder, iron powder, boron powder, aluminum powder, lanthanum powder and cerium powder, mechanically crushing and grinding to obtain alloy powder; placing the alloy powder into a mold, and performing compression molding at 38 MPa to obtain a magnet blank;

[0038] S2: Hexafluorobutyl acrylate, hydroxyethyl methacrylate and ethyl acetate are mixed in a mass ratio of 1:3:5 to obtain a mixed liquid; 4,4'-azobis(4-cyanopentanol) and ethanol are mixed in a mass ratio of 1:6 and stirred to obtain an initiator; under a nitrogen atmosphere, the mixed liquid is heated to 64°C, 0.3 times of 2-mercaptoethanol and 0.045 times of the total volume of the mixed liquid are added dropwise at a rate of 2 ml / min, and after reacting for 2.5 hours, 0.01 to 0.02 times of the total volume of the mixed liquid are added dropwise, and 0.45 times of the total volume of the mixed liquid are added dropwise at a rate of 2 ml / min, and after continuing to react for 2.5 hours, rotary evaporation is performed to obtain an acrylate oligomer; grain boundary diffusion powder and acrylate oligomer are mixed in a mass ratio of 65:2, stirred to obtain a coating, and the grain boundary diffusion powder is aluminum, calcium and neodymium in a mass ratio of 1.5:5:40;

[0039] S3 uniformly coating the coating on the surface of the magnet blank, with the mass ratio of the coating to the magnet being 4:100, to obtain a magnet;

[0040] S4 places the magnet in a vacuum furnace and performs heat treatment at 550°C for 60 minutes, then performs grain boundary diffusion treatment at a temperature of 900°C for 4 hours, and finally performs low-temperature tempering at 465°C to obtain lanthanum-cerium rare earth permanent magnet material.

[0041] Example 3

[0042] The present embodiment includes the following components in mass percentage: 51% neodymium, 25% iron, 20% boron, 0.2% aluminum, 1% lanthanum, 0.6% cerium and 2% calcium;

[0043] The method for preparing lanthanum-cerium rare earth permanent magnet material by grain boundary diffusion in this embodiment is as follows:

[0044] S1: mixing neodymium powder, iron powder, boron powder, aluminum powder, lanthanum powder and cerium powder, mechanically crushing and grinding to obtain alloy powder; placing the alloy powder into a mold, and performing compression molding at 40 MPa to obtain a magnet blank;

[0045] S2: Hexafluorobutyl acrylate, hydroxyethyl methacrylate and ethyl acetate are mixed in a mass ratio of 1:4:6 to obtain a mixed liquid; 4,4'-azobis(4-cyanopentanol) and ethanol are mixed in a mass ratio of 1:7 and stirred to obtain an initiator; under a nitrogen atmosphere, the mixed liquid is heated to 65°C, 0.4 times of 2-mercaptoethanol and 0.06 times of the total volume of the mixed liquid are added dropwise at a rate of 3 ml / min, and after reacting for 3 hours, 0.02 times of the total volume of the mixed liquid are added dropwise, and 0.5 times of the total volume of the mixed liquid are added dropwise at a rate of 3 ml / min, and after continuing to react for 3 hours, rotary evaporation is performed to obtain an acrylate oligomer; grain boundary diffusion powder and acrylate oligomer are mixed in a mass ratio of 80:3, stirred to obtain a coating, and the grain boundary diffusion powder is aluminum, calcium and neodymium in a mass ratio of 2:5:40;

[0046] S3 uniformly coating the coating on the surface of the magnet blank, with the mass ratio of the coating to the magnet being 6:100, to obtain a magnet;

[0047] S4 places the magnet in a vacuum furnace and performs heat treatment at 600°C for 90 minutes, then performs grain boundary diffusion treatment at a temperature of 950°C for 6 hours, and finally performs low-temperature tempering at 480°C to obtain lanthanum-cerium rare earth permanent magnet material.

[0048] Comparative Example 1

[0049] This comparative example includes the following components in mass percentage: 51% neodymium, 25% iron, 19% boron, 0.4% aluminum, 2% lanthanum, and 0.7% cerium;

[0050] The method for preparing lanthanum-cerium rare earth permanent magnet material by grain boundary diffusion in this comparative example is:

[0051] S1: mixing neodymium powder, iron powder, boron powder, aluminum powder, lanthanum powder and cerium powder, mechanically crushing and grinding to obtain alloy powder; placing the alloy powder into a mold, and performing compression molding at 38 MPa to obtain a magnet blank;

[0052] S2: Hexafluorobutyl acrylate, hydroxyethyl methacrylate and ethyl acetate are mixed in a mass ratio of 1:3:5 to obtain a mixed solution; 4,4'-azobis(4-cyanopentanol) and ethanol are mixed in a mass ratio of 1:6 and stirred to obtain an initiator; under a nitrogen atmosphere, the mixed solution is heated to 64°C, 0.3 times of 2-mercaptoethanol and 0.045 times of the total volume of the mixed solution are added dropwise at a rate of 2 ml / min, and after reacting for 2.5 hours, 0.01 to 0.02 times of the total volume of the mixed solution are continued to be added dropwise, and 0.45 times of the total volume of the mixed solution are added dropwise at a rate of 2 ml / min, and after continuing to react for 2.5 hours, rotary evaporation is performed to obtain an acrylate oligomer;

[0053] S3: uniformly coating the acrylate oligomer on the surface of the magnet blank, wherein the mass ratio of the acrylate oligomer to the magnet is 4:100, to obtain a magnet;

[0054] S4 places the magnet in a vacuum furnace and performs heat treatment at 550°C for 60 minutes, then performs grain boundary diffusion treatment at a temperature of 900°C for 4 hours, and finally performs low-temperature tempering at 465°C to obtain lanthanum-cerium rare earth permanent magnet material.

[0055] Comparative Example 2

[0056] The comparative example includes the following components in mass percentage: 50% neodymium, 25% iron, 19% boron, 0.4% aluminum, 2% lanthanum, 0.7% cerium and 1.5% calcium.

[0057] The method for preparing lanthanum-cerium rare earth permanent magnet material by grain boundary diffusion in this comparative example is:

[0058] S1: mixing neodymium powder, iron powder, boron powder, aluminum powder, lanthanum powder and cerium powder, mechanically crushing and grinding to obtain alloy powder; placing the alloy powder into a mold, and performing compression molding at 38 MPa to obtain a magnet blank;

[0059] S2: mixing grain boundary diffusion powder and 502 adhesive in a mass ratio of 65:2, stirring evenly, and preparing a coating, wherein the grain boundary diffusion powder is aluminum, calcium and neodymium in a mass ratio of 1.5:5:40;

[0060] S3 uniformly coating the coating on the surface of the magnet blank, with the mass ratio of the coating to the magnet being 4:100, to obtain a magnet;

[0061] S4 places the magnet in a vacuum furnace and performs heat treatment at 550°C for 60 minutes, then performs grain boundary diffusion treatment at a temperature of 900°C for 4 hours, and finally performs low-temperature tempering at 465°C to obtain lanthanum-cerium rare earth permanent magnet material.

[0062] Comparative Example 3

[0063] This comparative example includes the following components in mass percentage: 50% neodymium, 25% iron, 19% boron, 0.4% aluminum, 2% lanthanum, 0.7% cerium, and 1.5% calcium;

[0064] The method for preparing lanthanum-cerium rare earth permanent magnet material by grain boundary diffusion in this comparative example is:

[0065] S1: mixing neodymium powder, iron powder, boron powder, aluminum powder, lanthanum powder and cerium powder, mechanically crushing and grinding to obtain alloy powder; placing the alloy powder into a mold, and performing compression molding at 38 MPa to obtain a magnet blank;

[0066] S2 places the magnet blank in a vacuum furnace, performs heat treatment at 550°C for 60 minutes, performs grain boundary diffusion treatment at a temperature of 900°C for 4 hours, and finally performs low-temperature tempering at 465°C to obtain lanthanum-cerium rare earth permanent magnet material.

[0067] Effect example

[0068] Referring to the GB / T3217 test standard, the NIM-10000H of the China Institute of Metrology and the NIM200C of the China Institute of Metrology for measuring different temperature curves of permanent magnet materials were used to measure the remanence (Br), coercive force (Hcj) and irreversible loss of magnetic flux (irr). The following Table 1 shows the performance analysis results of the lanthanum cerium rare earth permanent magnet materials prepared by grain boundary diffusion of Examples 1 to 3 of the present invention and Comparative Examples 1 to 5:

[0069] Table 1 Performance test data of lanthanum, cerium and rare earth permanent magnet materials

[0070] Br(kGs) Hcj(kOe) irr200℃(%) irr240℃(%) Example 1 12.94 28.79 1.24 2.96 Example 2 12.96 28.85 1.18 2.84 Example 3 12.91 28.83 1.20 2.90 Comparative Example 1 13.84 23.31 1.58 3.65 Comparative Example 2 12.45 24.98 1.94 3.72 Comparative Example 3 12.43 22.33 2.04 3.99

[0071] By comparing the experimental data of the embodiments and the comparative examples in Table 1, it can be clearly found that the lanthanum-cerium rare earth permanent magnet materials prepared by grain boundary diffusion using embodiments 1, 2 and 3 have relatively excellent performance.

[0072] From the comparison of the experimental data of Example 1, Example 2, Example 3 and Comparative Example 1, it can be found that the acrylate oligomer prepared by polymerization of hexafluorobutyl acrylate, hydroxyethyl methacrylate and ethyl acetate is directly coated on the surface of the magnet blank and subjected to advanced diffusion. Although the remanence is high, the coercive force and the irreversible loss of magnetic flux are poor, indicating that adding grain boundary diffusion powder to the coating and conducting advanced diffusion can improve the performance of lanthanum cerium rare earth permanent magnet materials;

[0073] From the comparison of the experimental data of Example 1, Example 2, Example 3 and Comparative Example 2, it can be found that when the grain boundary diffusion powder in the coating is directly added to the alloy powder to form a magnet blank and the magnet blank is subjected to grain boundary diffusion treatment, the performance of the obtained lanthanum-cerium rare earth permanent magnet material is poor.

[0074] From the comparison of the experimental data of Example 1, Example 2, Example 3 and Comparative Example 3, it can be found that the coercive force of the permanent magnetic material is improved; the coating is applied to the surface of the magnet to form a continuous grain boundary phase with a melting point difference. During the heat treatment process, the surface grain boundary diffusion powder is in a semi-molten state and then continuously diffuses along the molten grain boundaries into the internal grain boundaries and the surface layer of the grains of the magnet to obtain a continuous grain boundary phase with a low melting point, thereby ensuring that the diffused magnet has a smooth diffusion channel and improving the coercive force of the permanent magnetic material.

[0075] Obviously, the above embodiments are merely examples for clearly illustrating the embodiments of the present invention, and are not intended to limit the embodiments of the present invention. For those skilled in the art, other different forms of changes or modifications can be made based on the above description. It is not necessary and impossible to list all the embodiments here. However, these obvious changes or modifications derived from the spirit of the present invention are still within the scope of protection of the present invention.

Claims

1. A method for preparing lanthanum-cerium rare earth permanent magnet materials by grain boundary diffusion, characterized in that: The lanthanum-cerium rare earth permanent magnet material is prepared by coating component B on the surface of component A and then magnetron sputtering; component A is a magnet blank formed by die-pressing alloy powder; component B is a coating; the alloy powder includes neodymium powder, iron powder, boron powder, aluminum powder, lanthanum powder and cerium powder; the average particle size of the alloy powder is 1 to 4 μm; and the coating includes grain boundary diffusion powder and acrylate oligomer.

2. The method for preparing lanthanum-cerium rare earth permanent magnet material by grain boundary diffusion according to claim 1, characterized in that: The grain boundary diffusion powder is aluminum, calcium and neodymium in a mass ratio of 1 to 2:8:

40.

3. The method for preparing lanthanum-cerium rare earth permanent magnet material by grain boundary diffusion according to claim 1, characterized in that: The acrylate oligomer is prepared by polymerizing hexafluorobutyl acrylate, hydroxyethyl methacrylate and ethyl acetate.

4. The method for preparing lanthanum-cerium rare earth permanent magnet material by grain boundary diffusion according to claim 1, characterized in that: The specific steps include: S1: putting alloy powder into a mold and pressing it at 35-40 MPa to obtain a magnet blank; S2: mixing the grain boundary diffusion powder and the acrylate oligomer in a mass ratio of 50-80:1-3, stirring evenly, and preparing a coating; S3: uniformly coating the coating on the surface of the magnet blank, with the mass ratio of the coating to the magnet being 3 to 6:100, to obtain a magnet; S4 places the magnet in a vacuum furnace, performs heat treatment at 500-600°C for 30-90 minutes, performs grain boundary diffusion treatment, and finally performs low-temperature tempering at 450-480°C to obtain lanthanum-cerium rare earth permanent magnet material.

5. The method for preparing lanthanum-cerium rare earth permanent magnet material by grain boundary diffusion according to claim 4, characterized in that: In the above step S1 , the alloy powder is prepared by mixing neodymium powder, iron powder, boron powder, aluminum powder, lanthanum powder and cerium powder, and mechanically crushing and grinding the mixture.

6. The method for preparing lanthanum-cerium rare earth permanent magnet material by grain boundary diffusion according to claim 4, characterized in that: In the above step S2: the preparation method of the acrylate oligomer is: under a nitrogen atmosphere, the mixed solution is heated to 62-65°C, 0.2-0.4 times the volume of the mixed solution of 2-mercaptoethanol and 0.03-0.06 times the total volume of the mixed solution of initiator are added dropwise at a rate of 1-3 ml / min, and after reacting for 2-3 hours, 0.01-0.02 times the total volume of the mixed solution of initiator are continued to be added dropwise, and 0.4-0.5 times the total volume of the mixed solution is added dropwise at a rate of 1-3 ml / min, and the reaction is continued for 2-3 hours, and then rotary evaporation is performed to obtain the acrylate oligomer.

7. The method for preparing lanthanum-cerium rare earth permanent magnet material by grain boundary diffusion according to claim 6, characterized in that: The mixed liquid is prepared by mixing hexafluorobutyl acrylate, hydroxyethyl methacrylate and ethyl acetate in a mass ratio of 1:2-4:4-6; the initiator is prepared by mixing 4,4'-azobis(4-cyanopentanol) and ethanol in a mass ratio of 1:5-7 and stirring uniformly.

8. The method for preparing lanthanum-cerium rare earth permanent magnet material by grain boundary diffusion according to claim 4, characterized in that: In the above step S4, the temperature during grain boundary diffusion is 850-950° C. and the time is 2-6 hours.

9. A method for preparing lanthanum-cerium rare earth permanent magnet material by grain boundary diffusion as claimed in claim 1, characterized in that: The lanthanum-cerium rare earth permanent magnet material prepared by grain boundary diffusion according to the method for preparing lanthanum-cerium rare earth permanent magnet material by grain boundary diffusion comprises the following components in mass percentage: 49-51% neodymium, 24-25% iron, 18-20% boron, 0.2-0.6% aluminum, 1-3% lanthanum, 0.6-0.8% cerium and 1-2% calcium.

Citation Information

Patent Citations

  • Method for improving magnet coercive force

    CN105070498A

  • High-coercivity neodymium iron boron magnet surface coating slurry and neodymium iron boron magnet preparation method

    CN108630368A

  • Rare earth magnet and preparation method thereof

    CN114927302A

  • Diffusion slurry, rare earth permanent magnet material and preparation method and application of rare earth permanent magnet material

    CN116377377A

  • Grain boundary diffusion magnet manufacturing methods and grain boundary diffusion magnet manufactured using it

    KR102098270B1

Cited By

  • Spin-coating dispersing agent for grain boundary diffusion of cerium-rich neodymium-iron-boron magnet and use method of spin-coating dispersing agent

    CN121583761A