Preparation method of semiconductor device and semiconductor device
By forming a three-layer ohmic contact metal layer on the surface of the silicon carbide epitaxial wafer, including a metal silicide and a reducing non-metal element compound conductive layer, the problem of poor conductivity in the existing technology is solved and the efficiency of the silicon carbide device is improved. and switching rate.
Patent Information
- Application Number
- CN202410692038.3
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Filing Date
- 2024-05-30
- Publication Date
- 2024-10-01
AI Technical Summary
In existing silicon carbide devices, there is a problem of poor conductivity when the ohmic contact metal layer is combined with subsequent metal connections, resulting in poor efficiency and switching rate of the device.
An ohmic contact metal layer is formed on the surface of the silicon carbide epitaxial wafer, including an ohmic contact layer, a metal buffer layer and a metal conductive layer. The ohmic contact layer is composed of metal silicide, and the metal conductive layer is composed of compounds composed of reducing non-metallic elements and metals. Metal The buffer layer serves as a stress buffer layer to improve the interface bonding effect.
Through the excellent conductivity and stress buffer layer design, the interface combination between the ohmic contact metal layer and the metal wiring is improved, and the efficiency and switching rate of the device are improved.
Smart Images

Figure CN118737819A_ABST
Abstract
Description
Technical Field
[0001] The present application relates to the field of semiconductor technology, and in particular to a method for preparing a semiconductor device and a semiconductor device thereof. Background Art
[0002] Taking silicon carbide compound semiconductor devices as an example, the ohmic contact formed at the interface between silicon carbide (SiC) and metal provides a transmission path between the device and external electrical signals. The performance of its ohmic contact is directly related to the operating efficiency and reliability of the device.
[0003] At present, in silicon carbide devices, ohmic contacts are mainly formed by metal and SiC with high concentration of N-type or P-type doping on the surface of the wafer epitaxial layer under high temperature annealing conditions to form a metal silicide alloy. However, the metal silicide alloy prepared by the above method has the problem of poor conductivity when combined with subsequent metal connections. Summary of the invention
[0004] The semiconductor device preparation method and semiconductor device provided in the present application can solve the problem of poor conductivity when the existing ohmic contact metal layer is combined with the subsequent metal connection.
[0005] In order to solve the above technical problems, a technical solution adopted in the present application is: to provide a method for preparing a semiconductor device, comprising:
[0006] Providing a silicon carbide epitaxial wafer;
[0007] forming an ohmic contact metal layer on a surface of the silicon carbide epitaxial wafer;
[0008] Among them, the ohmic contact metal layer includes an ohmic contact layer, a metal buffer layer and a metal conductive layer. The ohmic contact layer is arranged on the silicon carbide epitaxial wafer, the metal buffer layer is arranged on the ohmic contact layer, the metal conductive layer is arranged on the metal buffer layer, and the metal buffer layer is located between the ohmic contact layer and the metal conductive layer; the material of the ohmic contact layer includes metal silicide, and the metal conductive layer includes a compound layer composed of reducing non-metallic elements and metals.
[0009] In order to solve the above technical problems, another technical solution adopted by the present application is: to provide a semiconductor device, comprising:
[0010] Silicon carbide epitaxial wafers;
[0011] An ohmic contact metal layer, comprising an ohmic contact layer, a metal buffer layer and a metal conductive layer, wherein the ohmic contact layer is disposed on the silicon carbide epitaxial wafer, the metal buffer layer is disposed on the ohmic contact layer, the metal conductive layer is disposed on the metal buffer layer, and the metal buffer layer is located between the ohmic contact layer and the metal conductive layer;
[0012] The material of the ohmic contact layer includes metal silicide, and the metal conductive layer includes a compound layer composed of a reducing non-metallic element and a metal.
[0013] Different from the prior art, the beneficial effect of the present application is that in the preparation method of the semiconductor device provided by the present application, an ohmic contact metal layer is formed on the surface of the silicon carbide epitaxial wafer, and the ohmic contact metal layer includes an ohmic contact layer, a metal buffer layer and a metal conductive layer, wherein the material of the ohmic contact layer includes metal silicide, and the metal conductive layer includes a compound composed of a reducing non-metallic element and a metal. Specifically, the metal compound conductive layer having a reducing non-metallic element has excellent conductivity, thereby improving the problem of poor conductivity when the ohmic contact metal layer is combined with subsequent metal wiring; and the metal buffer layer serves as a stress buffer layer between the ohmic contact layer and the metal conductive layer, so that the two have good contact, thereby improving the interface bonding effect between the ohmic contact metal layer and the subsequent metal wiring, which is beneficial to the device's utilization efficiency, gain and switching rate. BRIEF DESCRIPTION OF THE DRAWINGS
[0014] In order to more clearly illustrate the technical solutions in the embodiments of the present application, the drawings required for use in the description of the embodiments are briefly introduced below. Obviously, the drawings described below are only some embodiments of the present application. For those skilled in the art, other drawings can be obtained based on these drawings without creative work, among which:
[0015] Figure 1 A schematic diagram of a process for preparing a semiconductor device according to an embodiment of the present application;
[0016] Figure 2 for Figure 1 A schematic flow chart of an embodiment of step S2;
[0017] Figure 3 for Figure 2 A schematic flow chart of an embodiment of step S22;
[0018] Figure 4 for Figure 2 A schematic flow chart of another embodiment of step S22;
[0019] Figure 5 for Figure 1 A schematic diagram of a wafer fabrication structure of an embodiment after step S1;
[0020] Figure 6 for Figure 2 A schematic diagram of a wafer fabrication structure of an embodiment after step S21;
[0021] Figure 7 for Figure 3 A schematic diagram of a wafer fabrication structure of an embodiment after step S101;
[0022] Figure 8 for Figure 3 A schematic diagram of a wafer fabrication structure of an embodiment after step S102;
[0023] Fig. 9 for Figure 4 A schematic diagram of a wafer fabrication structure of an embodiment after step S103;
[0024] Fig.10 for Figure 4 A schematic diagram of a wafer fabrication structure of an embodiment after step S104;
[0025] Fig.11 A schematic diagram of a portion of the structure of a semiconductor device provided in an embodiment of the present application. Description of the drawings:
[0027] Silicon carbide epitaxial wafer-11; substrate-111; silicon carbide epitaxial layer-112; ohmic contact metal layer-12; ohmic contact layer-121; metal buffer layer-122; metal conductive layer-123; metal layer-13; carbon-containing layer-14; metal connection layer-15.
[0028] Silicon carbide epitaxial wafer-21; substrate-211; silicon carbide epitaxial layer-212; ohmic contact gold layer-22; ohmic contact layer-221; metal buffer layer-222; metal conductive layer-223; semiconductor cell-30; first base region-301; second base region-302; first source region-303; first contact region-304; second source region-305; second contact region-306; metal connection layer-23; gate structure-24; source structure-25; drain structure-26; insulating layer-27. DETAILED DESCRIPTION
[0029] The following will be combined with the drawings in the embodiments of the present application to clearly and completely describe the technical solutions in the embodiments of the present application. Obviously, the described embodiments are only part of the embodiments of the present application, not all of the embodiments. Based on the embodiments in the present application, all other embodiments obtained by ordinary technicians in this field without creative work are within the scope of protection of this application.
[0030] The terms "first", "second", "third" in this application are only used for descriptive purposes, and cannot be understood as indicating or implying relative importance or implicitly indicating the number of indicated technical features. Thus, the features defined as "first", "second", "third" can expressly or implicitly include at least one of the features. In the description of this application, the meaning of "multiple" is at least two, such as two, three, etc., unless otherwise clearly and specifically defined. In the embodiments of this application, all directional indications (such as up, down, left, right, front, back...) are only used to explain the relative position relationship, movement, etc. between the components under a certain specific posture (as shown in the accompanying drawings). If the specific posture changes, the directional indication also changes accordingly. In addition, the terms "including" and "having" and any of their variations are intended to cover non-exclusive inclusions. For example, a process, method, system, product or device comprising a series of steps or units is not limited to the steps or units listed, but optionally also includes steps or units that are not listed, or optionally also includes other steps or units inherent to these processes, methods, products or devices.
[0031] Reference to "embodiments" herein means that a particular feature, structure, or characteristic described in conjunction with the embodiments may be included in at least one embodiment of the present application. The appearance of the phrase in various locations in the specification does not necessarily refer to the same embodiment, nor is it an independent or alternative embodiment that is mutually exclusive with other embodiments. It is explicitly and implicitly understood by those skilled in the art that the embodiments described herein may be combined with other embodiments.
[0032] The present application is described in detail below with reference to the accompanying drawings and embodiments.
[0033] The ohmic contact formed at the interface between SiC and metal in the structure of wide-bandgap silicon carbide compound semiconductor devices provides a transmission path between the device and external electrical signals, and the performance of its ohmic contact is directly related to the operating efficiency and reliability of the device. At present, in silicon carbide semiconductor devices, the ohmic contact is mainly formed by metal and high-concentration SiC on the surface of the wafer epitaxial layer under high-temperature annealing conditions to form a metal silicide alloy. For example, in the commonly used ohmic contact nickel (Ni) metal system, it is a nickel-silicide alloy (Ni-silicide) obtained by heat treatment at 900 degrees Celsius in a high-temperature furnace tube, and acts as the ohmic contact layer of silicon carbide, which is connected to the subsequently deposited aluminum wire and provides an electrical signal transmission path.
[0034] However, the applicant has found that when the existing ohmic contact metal layer is combined with the subsequent metal connection, the interface bonding effect and the electrical conductivity of the metal silicide are poor when the metal silicide is combined with the metal connection. The reason is that after high-temperature heat treatment, a metal silicide alloy with a hard texture and poor electrical conductivity is formed by silicon carbide and metal. The silicide alloy is prone to grain agglomeration, resulting in poor interface bonding when combined with the subsequent metal connection. Nickel metal silicide also faces the problem of poor electrical conductivity, which ultimately affects the device's efficiency, gain and switching rate.
[0035] See also Figure 1-Figure 10 , Figure 1 A schematic diagram of a process for preparing a semiconductor device according to an embodiment of the present application; Figure 2 for Figure 1 A schematic flow chart of an embodiment of step S2; Figure 3 for Figure 2 A schematic flow chart of an embodiment of step S22; Figure 4 for Figure 2 A schematic flow chart of another embodiment of step S22; Figure 5 for Figure 1 A schematic diagram of a wafer fabrication structure of an embodiment after step S1; Figure 6 for Figure 2 A schematic diagram of a wafer fabrication structure of an embodiment after step S21; Figure 7 for Figure 3 A schematic diagram of a wafer fabrication structure of an embodiment after step S101; Figure 8 for Figure 3 A schematic diagram of a wafer fabrication structure of an embodiment after step S102; Fig. 9 for Figure 4 A schematic diagram of a wafer fabrication structure of an embodiment after step S103; Fig.10 for Figure 4 FIG. 1 is a schematic diagram of a wafer fabrication structure of an embodiment after step S104.
[0036] To solve the above problems, see Figure 1 , an embodiment of the present application provides a method for preparing a semiconductor device, comprising:
[0037] Step S1: providing a silicon carbide epitaxial wafer 11.
[0038] The silicon carbide epitaxial wafer 11 may be subjected to full-surface ion implantation to achieve a concentration of 10 18~19 / cm 3 The N-type or P-type doped silicon carbide epitaxial wafer 11. The silicon carbide epitaxial wafer 11 may also be a structure including a substrate and a silicon carbide epitaxial layer grown on the substrate.
[0039] The silicon carbide epitaxial wafer 11 may be a silicon carbide wafer taped out, or may not be a silicon carbide wafer taped out. For ease of description, the present application embodiment takes a silicon carbide wafer taped out as an example of the silicon carbide epitaxial wafer 11 for illustration. Figure 5 It can be understood that since the silicon carbide epitaxial wafer 11 is a test wafer and is used only as an example, no interval partition doping is performed in the wafer to form a specific functional cell structure.
[0040] Step S2 : forming an ohmic contact metal layer 12 on the surface of the silicon carbide epitaxial wafer 11 .
[0041] See Fig. 9 , wherein the ohmic contact metal layer 12 includes an ohmic contact layer 121, a metal buffer layer 122 and a metal conductive layer 123, the ohmic contact layer 121 is arranged on the silicon carbide epitaxial wafer 11, the metal buffer layer 122 is arranged on the ohmic contact layer 121, the metal conductive layer 123 is arranged on the metal buffer layer 122, and the metal buffer layer 122 is located between the ohmic contact layer 121 and the metal conductive layer 123; the material of the ohmic contact layer 121 includes metal silicide, and the metal conductive layer 123 includes a compound composed of a reducing non-metallic element and a metal.
[0042] Among them, the ohmic contact layer 121 can be arranged on the surface of the silicon carbide epitaxial wafer 11; the metal buffer layer 122 can be arranged on the surface of the ohmic contact layer 121 away from the silicon carbide epitaxial wafer 11; the metal conductive layer 123 can be arranged on the surface of the metal buffer layer 122 away from the silicon carbide epitaxial wafer 11.
[0043] Specifically, the metal compound conductive layer having a reducing non-metallic element (i.e., the metal conductive layer 123) has excellent electrical conductivity, which can improve the problem of poor conductivity when combined with subsequent metal wiring, and the metal buffer layer 122 serves as a stress buffer layer between the bottom ohmic contact layer 121 and the top metal conductive layer 123, so that the two have good contact, thereby improving the interface bonding effect between the ohmic contact metal layer 12 and the subsequent metal wiring, which is beneficial to the device's utilization efficiency, gain and switching rate.
[0044] The metal buffer layer 123 may be a single metal layer, a mixed metal layer including multiple single metal layers stacked together, or a metal compound layer. As long as it can achieve a buffering effect, it is not limited here.
[0045] Combination Figure 2 In one embodiment, step S2 includes:
[0046] Step S21 : forming a metal layer 13 on the surface of the silicon carbide epitaxial wafer 11 .
[0047] See Figure 6 In one embodiment, the material of the metal layer 13 includes but is not limited to at least one of nickel, molybdenum, titanium, cobalt and aluminum. Specifically, the material properties of the metal layer 13 have the characteristics of small film stress, low hardness, high conductivity, etc., so that the ohmic contact layer 121, metal buffer layer 122 and metal conductive layer 123 formed by subsequent reactions all have good conductivity, and the formed metal buffer layer 122 can buffer the stress between the ohmic contact layer 121 and the metal conductive layer 123, so that the two have good contact, thereby improving the interface bonding effect between the ohmic contact metal layer 12 and the subsequent metal wiring.
[0048] Specifically, as long as the above-mentioned metal component can be thermally reduced with the subsequent reducing non-metallic element to form a corresponding high-conductivity metal compound structure, and at the same time, the metal can form a metal silicide with SiC, no limitation is made here.
[0049] In one embodiment of the present application, the metal layer 13 is a single metal layer, and the metal layer 13 is grown by magnetron sputtering. Of course, in other embodiments, the metal layer 13 can also be formed by chemical vapor deposition, which is not limited here.
[0050] Among them, the metal layer 13 formed by magnetron sputtering has higher adhesiveness, higher deposition rate, better uniformity and adhesion compared with the metal layer 13 formed by vapor deposition.
[0051] Step S22 : using a reducing non-metallic element, thermally reducing the silicon carbide epitaxial wafer 11 on which the metal layer 13 is formed, so as to form an ohmic contact metal layer 12 on the surface of the silicon carbide epitaxial wafer 11 .
[0052] Specifically, by virtue of the strong thermal reduction property of the reducing non-metallic element on the metal, after high-temperature heat treatment, the lower surface of the metal layer 13 can form a metal-silicide alloy with the silicon carbide in the silicon carbide epitaxial wafer 11, acting as the ohmic contact layer 121. At the same time, the upper surface of the metal layer 13 contacts the reducing non-metallic element, and a metal conductive layer 123 is synchronously formed. The metal conductive layer formed at this time has excellent electrical conductivity. When it is connected with the subsequent metal wiring, the metal conductive layer 123 can overcome the problem of poor conductivity when combined with the metal wiring. The middle part of the metal layer 13 is limited by the reduction depth on both sides and still maintains the single metal component, thereby serving as a stress buffer layer between the bottom ohmic contact layer 121 and the top metal conductive layer 123, so that the two have good contact, thereby improving the interface bonding effect between the ohmic contact metal layer 12 and the subsequent metal wiring, which is beneficial to the device's utilization efficiency, gain and switching rate.
[0053] In addition, the present application forms a metal layer on the surface of the silicon carbide epitaxial wafer, and then uses a reducing non-metallic element to perform a thermal reduction treatment on the silicon carbide epitaxial wafer 11 formed with the metal layer 13, so that a three-layer structure of an ohmic contact metal layer 12 can be formed at one time. The process is relatively simple and easy to implement, and the amount of the metal layer is easy to adjust. Therefore, it has the advantages of flexible and controllable process, and adjustable positions of the metal buffer layer and the metal conductive layer.
[0054] Combination Figure 3 In the first embodiment of the present application, step S22 includes:
[0055] Step S101 : forming a carbon-containing layer 14 on a surface of the metal layer 13 that is away from the silicon carbide epitaxial wafer 11 .
[0056] See Figure 7 In the embodiment of the present application, the carbon-containing layer 14 is a carbon layer, and the carbon-containing layer 14 is grown on the surface of the metal layer 13 away from the silicon carbide epitaxial wafer 11 (ie, the first surface) by magnetron sputtering.
[0057] Specifically, the embodiment of the present application uses a carbon film as a reducing non-metallic element, and the formed metal conductive layer 123 includes metal carbides, and metal carbides have excellent conductivity. When connected with subsequent metal wires, they can overcome the problem of high resistivity that is commonly found when metal silicides are connected to metal wires at this stage.
[0058] In the present application, a quantitative relationship can be stipulated that the ratio of the thickness of the metal layer 13 to the thickness of the carbon-containing layer 14 is 1:(0.1-10). For example, the ratio of the thickness of the metal layer 13 to the thickness of the carbon-containing layer 14 is 1:0.1; or the ratio of the thickness of the metal layer 13 to the thickness of the carbon-containing layer 14 is 1:1; the ratio of the thickness of the metal layer 13 to the thickness of the carbon-containing layer 14 is 3:1; or the ratio of the thickness of the metal layer 13 to the thickness of the carbon-containing layer 14 is 5:1; or the ratio of the thickness of the metal layer 13 to the thickness of the carbon-containing layer 14 is 7:1; or the ratio of the thickness of the metal layer 13 to the thickness of the carbon-containing layer 14 is 10:1, etc., which are not limited here.
[0059] Among them, considering the influence of factors such as the high-temperature reaction kinetics between the metal layer 13 and the carbon-containing layer 14, the stoichiometric ratio of the deposited carbon-containing layer 14 when forming metal carbide is often excessive. Therefore, the ratio of the thickness of the metal layer 13 to the thickness of the carbon-containing layer 14 is set to 1: (0.1~10).
[0060] In addition, since the carbon-containing layer 14 is easier to be removed in the subsequent process than the metal film, in the present application, an excess of the carbon-containing layer 14 is deposited. Of course, in some other specific embodiments, the stoichiometric ratio of the deposited carbon-containing layer 14 may not be excessive.
[0061] Specifically, in the embodiment of the present application, the thickness of the metal layer 13 is 50 to 500 nanometers, for example, the thickness of the metal layer 13 can be 50 nanometers, 150 nanometers, 250 nanometers, 450 nanometers or 500 nanometers. The thickness of the carbon-containing layer 14 is 50 to 500 nanometers, for example, the thickness of the carbon-containing layer 14 can be 50 nanometers, 150 nanometers, 250, 450 nanometers or 500 nanometers, etc., which can be based on the stoichiometric ratio of the carbon element in the carbon-containing layer 14 when the metal carbide is formed, and is not limited here.
[0062] Step S102 : heat-treating the silicon carbide epitaxial wafer 11 on which the metal layer 13 and the carbon-containing layer 14 are formed, so as to form an ohmic contact metal layer 12 on the surface of the silicon carbide epitaxial wafer 11 .
[0063] See Figure 8 or Fig. 9 Specifically, the ohmic contact layer 121 is formed by thermal reaction between the metal layer 13 and the silicon carbide epitaxial wafer 11 , so the material of the ohmic contact layer 121 includes metal silicide to achieve ohmic contact with the silicon carbide epitaxial wafer 11 .
[0064] The metal conductive layer 123 is formed by thermal reaction between the metal layer 13 and the carbon-containing layer 14. Therefore, the material of the metal conductive layer 123 includes metal carbide, which can overcome the problem of poor conductivity when subsequently combined with metal wiring. Among them, the conductivity of the metal conductive layer 123 is greater than 1.0E106 s / m.
[0065] Among them, the unreacted part (i.e., the remaining part) of the metal layer 13 serves as a metal buffer layer 122 between the ohmic contact layer 121 and the metal conductive layer 123. It can be understood that in the present application, the middle part of the metal layer 13 (i.e., the metal buffer layer 122) is limited by the reduction depth on both sides, and still maintains a single metal component, and the material of the metal buffer layer 122 is the same as that of the metal layer 13, such as the material of the metal buffer layer 122 includes nickel, molybdenum, titanium, cobalt or aluminum, which has the characteristics of small film stress, low hardness, and high conductivity, so as to serve as a stress buffer layer between the bottom ohmic contact layer 121 and the top metal conductive layer 123, so that the two have good contact, thereby improving the interface bonding effect between the ohmic contact metal layer 12 and the subsequent metal wiring, which is beneficial to the device's use efficiency, gain and switching rate.
[0066] The embodiment of the present application forms a carbon-containing layer on the surface of the metal layer away from the silicon carbide epitaxial wafer, and then prepares an ohmic contact metal layer by heat treatment, so that the carbon content in the metal layer contact is sufficient, thereby being able to effectively form a complete metal carbide on the surface of the metal layer away from the silicon carbide epitaxial wafer, and the amount of the carbon-containing layer is flexibly adjustable, thereby making the process more flexible and controllable, and the position of the metal buffer layer and the metal conductive layer more adjustable.
[0067] In one embodiment, the silicon carbide epitaxial wafer 11 formed with the metal layer 13 and the carbon-containing layer 14 is subjected to a heat treatment, specifically comprising:
[0068] The silicon carbide epitaxial wafer 11 having the metal layer 13 and the carbon-containing layer 14 is heated at 800-1200 degrees Celsius for 10-500 minutes in an oxygen-free condition to form an ohmic contact layer 121 , a metal buffer layer 122 and a metal conductive layer 123 on the silicon carbide epitaxial wafer 11 .
[0069] Specifically, by using the above process conditions to perform thermal reduction treatment on the silicon carbide epitaxial wafer 11 formed with the metal layer 13 and the carbon-containing layer 14, a three-layer structure of the ohmic contact metal layer 12 can be formed at one time. The process is relatively simple and easy to implement.
[0070] Combination Figure 4 and Figure 8 In one embodiment, after forming the ohmic contact metal layer 12, the method further includes:
[0071] Step S103 : removing the remaining carbon-containing layer 14 on the surface of the metal conductive layer 123 facing away from the silicon carbide epitaxial wafer 11 .
[0072] See Fig. 9 It can be seen from the stoichiometric excess of carbon in the carbon-containing layer 14 when depositing the carbon-containing layer 14 in the above step S101 that a stoichiometric excess of carbon is deposited. Therefore, after the thermal reaction is completed, there will still be residual carbon components. Considering that the conductivity of the carbon-containing layer is weaker than that of metal carbides, and the bonding force between the carbon-containing layer and the metal layer is weaker than that of metal carbides, the remaining carbon-containing layer 14 (remaining carbon components) on the surface of the metal conductive layer 123 away from the silicon carbide epitaxial wafer 11 can be removed to improve the conductivity and bonding of the ohmic contact metal layer, avoid affecting the subsequent connection between the ohmic contact metal layer 12 and the metal wiring, and reduce the probability of subsequent cracking.
[0073] In one embodiment, step S103 includes:
[0074] Plasma etching is used to remove the remaining carbon-containing layer 14 on the surface of the metal conductive layer 123 facing away from the silicon carbide epitaxial wafer 11 .
[0075] Specifically, after the heat treatment, the residual carbon-containing layer 14 on the metal conductive layer 123 is removed by plasma etching to avoid affecting the subsequent connection between the ohmic contact metal layer 12 and the metal connection line. Specifically, plasma etching can achieve anisotropic etching with better controllability and uniformity.
[0076] Of course, if no carbon-containing layer 14 remains after the ohmic contact metal layer 14 is formed, step 103 is not necessary.
[0077] Step 104 : forming a metal connection layer 15 on the surface of the metal conductive layer 123 facing away from the silicon carbide epitaxial wafer 11 .
[0078] See Fig.10 The metal connection layer 15 is used as a metal connection line for electrically connecting the device to an external device. The material of the metal connection layer 15 is a conductive metal, wherein the material of the metal connection layer 15 includes but is not limited to metal aluminum, metal copper, and the like.
[0079] In one embodiment, step S104 includes:
[0080] The metal connection layer 15 is grown on the surface of the metal conductive layer 123 away from the silicon carbide epitaxial wafer 11 by magnetron sputtering.
[0081] In some embodiments, a magnetron sputtering method or a vapor deposition method may be used to grow a metal connection layer 15 on the surface of the metal conductive layer 123 away from the silicon carbide epitaxial wafer 11. Compared with forming the metal connection layer 15 by vapor deposition, the metal connection layer 15 grown by magnetron sputtering has higher adhesion, higher deposition rate, better uniformity and adhesion.
[0082] Specifically, the preparation method of the semiconductor device provided in the first embodiment of the present application forms a carbon-containing layer 14 by growing on the surface of the metal layer 13 away from the silicon carbide epitaxial wafer 11. With the help of the strong thermal reduction property of the carbon-containing layer 14 to the metal, after high-temperature heat treatment, the lower surface of the metal layer 13 can form a metal-silicide alloy with silicon carbide to serve as an ohmic contact layer 121. At the same time, the upper surface of the metal layer 13 contacts the carbon-containing layer 14 to synchronously form a metal conductive layer 123 having metal carbide. The metal carbide formed at this time has excellent conductivity. When it is connected to the subsequent metal wire, the metal carbide can overcome the problem of poor conductivity when combined with the metal wire. The middle part of the metal layer 13 is limited by the reduction depth on both sides and still maintains the single metal component, thereby serving as a stress buffer layer between the bottom ohmic contact layer 121 and the top metal carbide, so that the two have good contact, thereby improving the interface bonding effect between the ohmic contact metal layer 12 and the subsequent metal wire, which is beneficial to the device's use efficiency, gain and switching rate.
[0083] In the second embodiment of the present application, step S22 includes:
[0084] The silicon carbide epitaxial wafer 1 having the metal layer 13 formed thereon is subjected to a heat treatment in a reducing atmosphere to form an ohmic contact metal layer 12 on the surface of the silicon carbide epitaxial wafer 11 .
[0085] Combination Figure 6Specifically, the ohmic contact layer 121 is formed by thermal reaction between the metal layer 13 and the silicon carbide epitaxial wafer 11 . Therefore, the material of the ohmic contact layer 121 includes metal silicide to achieve ohmic contact with the silicon carbide epitaxial wafer 11 .
[0086] In some embodiments, the reducing atmosphere includes ammonia, sulfur vapor, selenium vapor or phosphine. The metal conductive layer 123 is obtained by reacting the metal layer 13 with the reducing atmosphere. Therefore, the material of the metal conductive layer 123 includes at least one of the corresponding metal nitride, metal sulfide, metal phosphide and metal selenide, and the above metal compound has excellent electrical conductivity, which can overcome the problem of poor electrical conductivity when combined with metal wiring, wherein the electrical conductivity of the metal conductive layer 123 is greater than 1.0E106 s / m.
[0087] Specifically, ammonia, sulfur vapor, selenium vapor and anions in phosphine can be used as equivalent replacements for the carbon film in the first embodiment to construct a highly conductive metal conductive layer 123, thereby overcoming the common problem of high resistivity when metal silicides are connected to metal wires at this stage.
[0088] Among them, the unreacted part (i.e., the remaining part) of the metal layer 13 serves as a metal buffer layer 122. It can be understood that in the present application, the middle part of the metal layer 13 (i.e., the metal buffer layer 122) is limited by the reduction depth on both sides, and still maintains a single metal component, and the material of the metal buffer layer 122 is the same as that of the metal layer 13, such as the material of the metal buffer layer 122 includes nickel, molybdenum, titanium, cobalt or aluminum, which has the characteristics of small film stress, low hardness, and high conductivity, so as to serve as a stress buffer layer between the bottom ohmic contact layer 121 and the top metal conductive layer 123, so that the two have good contact.
[0089] The embodiment of the present application forms a metal layer on the surface of the silicon carbide epitaxial wafer and prepares an ohmic contact metal layer by performing heat treatment in a reducing atmosphere, so that the reducing element content in contact with the metal layer is sufficient, so that a complete compound composed of reducing non-metallic elements and metals can be effectively formed on the surface of the metal layer away from the silicon carbide epitaxial wafer, and the reducing element content can be adjusted by adjusting the reducing atmosphere content, thereby making the process more flexible and controllable, and the position of the metal buffer layer and the metal conductive layer more adjustable.
[0090] In the second embodiment, after forming the ohmic contact metal layer 12, the method further includes:
[0091] A metal connection layer 15 is grown on the surface of the metal conductive layer 123 away from the metal buffer layer 122 .
[0092] Among them, the material and formation method of the metal connection layer 15 in this embodiment can be the same as those of the metal connection layer 15 in the first embodiment of the present application, and will not be repeated here.
[0093] Specifically, the preparation method of the semiconductor device provided in the second embodiment of the present application, with the help of the thermal reduction property of the reducing atmosphere, after high-temperature heat treatment, the lower surface of the metal layer 13 can form a metal-silicide alloy with the silicon carbide in the silicon carbide epitaxial layer 11, serving as the ohmic contact layer 121. At the same time, the upper surface of the metal layer 13 reacts with the reducing atmosphere to synchronously form a metal conductive layer 123 (including at least one of metal nitride, metal sulfide, metal phosphide and metal selenide). The metal conductive layer 123 can overcome the problem of poor conductivity when combined with metal wiring, and the middle part of the metal layer 13 is limited by the reduction depth on both sides and still maintains the single metal component, thereby serving as a stress buffer layer between the bottom ohmic contact layer 121 and the top metal conductive layer 123, so that the two have good contact, thereby improving the interface bonding effect between the ohmic contact metal layer 12 and the subsequent metal wiring, which is beneficial to the device's utilization efficiency, gain and switching rate.
[0094] In addition, compared with the first embodiment, the second embodiment of the present application does not need to remove the residual carbon-containing layer 14 after forming the ohmic contact metal layer 12, thereby simplifying the process flow and improving production efficiency.
[0095] See also Fig.11 , Fig.11 A schematic diagram of a portion of the structure of a semiconductor device provided in an embodiment of the present application.
[0096] In order to solve the above problems, an embodiment of the present application further provides a semiconductor device, which includes: a silicon carbide epitaxial wafer 21 and an ohmic contact metal layer 22 .
[0097] In one embodiment, the silicon carbide epitaxial wafer 21 may include a substrate 211 and a silicon carbide epitaxial layer 212 grown on the substrate 211. The substrate 211 and the silicon carbide epitaxial layer 212 have the same conductivity type, which may be both P-type or both N-type.
[0098] The silicon carbide epitaxial wafer 21 may have a top surface and a bottom surface that are disposed opposite to each other, the top surface of the silicon carbide epitaxial wafer 21 may be provided with an ohmic contact metal layer 22, and the bottom surface of the silicon carbide epitaxial wafer 21 may also be provided with an ohmic contact metal layer 22, which is not limited in the embodiment of the present invention. When the silicon carbide epitaxial wafer 21 includes a substrate 211 and a silicon carbide epitaxial layer 212 grown on the substrate 211, the surface of the substrate 211 that is away from the silicon carbide epitaxial layer 212 may be regarded as the bottom surface of the silicon carbide epitaxial wafer 21, and the surface of the silicon carbide epitaxial layer 212 that is away from the substrate 211 may be regarded as the top surface of the silicon carbide epitaxial wafer 21.
[0099] Among them, a number of semiconductor cells 30 are arranged in the silicon carbide epitaxial wafer 21, each semiconductor cell 30 is provided with a first base region 301 and a second base region 302 arranged at intervals, the first base region 301 is provided with a first source region 303 and a first contact region 304 connected to each other, and the second base region 302 is provided with a second source region 305 and a second contact region 306 connected to each other.
[0100] In one embodiment, the silicon carbide epitaxial wafer 21 , the first source region 303 and the second source region 305 all have the first conductivity type, wherein the ion doping concentrations of the first source region 303 and the second source region 305 are the same and greater than the ion doping concentration of the silicon carbide epitaxial wafer 21 .
[0101] The first base region 301 and the second base region 302, the first contact region 304 and the second contact region 306 all have the first conductivity type, wherein the ion doping concentrations of the first base region 301 and the second base region 302 are the same, the ion doping concentrations of the first contact region 304 and the second contact region 306 are the same, and the ion doping concentration of the first contact region 304 is greater than the ion doping concentration of the first base region 301, and the ion doping concentration of the second contact region 306 is greater than the ion doping concentration of the second base region 302.
[0102] The first conductivity type is one of a P-type doped semiconductor and an N-type doped semiconductor, and the second conductivity type is the other of the P-type doped semiconductor and the N-type doped semiconductor.
[0103] The ohmic contact metal layer 22 includes an ohmic contact layer 221, a metal buffer layer 222 and a metal conductive layer 223. The ohmic contact layer 221 is disposed on the silicon carbide epitaxial wafer 21, the metal buffer layer 222 is disposed on the ohmic contact layer 221, the metal conductive layer 223 is disposed on the metal buffer layer 222, and the metal buffer layer 222 is located between the ohmic contact layer 221 and the metal conductive layer 223. The material of the ohmic contact layer 221 includes metal silicide, and the metal conductive layer 223 includes a compound composed of a reducing non-metallic element and a metal.
[0104] It can be understood that when a number of semiconductor cells 30 are arranged in the silicon carbide epitaxial wafer 21, the semiconductor device includes a plurality of ohmic contact metal layers 22 arranged at intervals, wherein an ohmic contact metal layer 22 is respectively arranged on the first source region 303 and the second source region 305 in each cell 30 to provide a transmission path between the device and external electrical signals.
[0105] Specifically, the ohmic contact layer 221 is formed by the reaction of the silicon carbide epitaxial wafer 11 and the metal sheet 13, so the ohmic contact layer 221 includes metal silicide. When the semiconductor device is prepared by the preparation method provided in the first embodiment of the present application, the material of the metal conductive layer 223 includes metal carbide; when the semiconductor device is prepared by the preparation method provided in the second embodiment of the present application, the material of the metal conductive layer 223 includes at least one of metal nitride, metal sulfide, metal phosphide and metal selenide. Specifically, the material of the metal conductive layer 223 in the present application includes metal carbide, metal nitride, metal sulfide, metal phosphide, or metal selenide. The above-mentioned metal compound conductive layer (i.e., the metal conductive layer 223) composed of reducing non-metallic elements and metals can overcome the problem of poor conductivity when combined with metal wiring; in addition, the metal buffer layer 222 serves as a stress buffer layer between the ohmic contact layer 221 and the metal conductive layer 223, so that the two have good contact, thereby improving the interface bonding effect between the ohmic contact metal layer 22 and the subsequent metal wiring, and in the present application, the ohmic contact metal layer 22 is arranged on the first source region 303 and the second source region 305, which is beneficial to the device's utilization efficiency, gain and switching rate.
[0106] In one embodiment, the metal buffer layer 222 includes but is not limited to at least one of nickel, molybdenum, titanium, cobalt and aluminum. Specifically, the material properties of the metal buffer layer 222 have the characteristics of small film stress, low hardness, high conductivity, etc., which can buffer the stress between the ohmic contact layer 121 and the metal conductive layer 123, so that the two have good contact, thereby improving the interface bonding effect between the ohmic contact metal layer 12 and the subsequent metal connection. As long as the above-mentioned metal component can form a corresponding high-conductivity metal compound structure after thermal reduction treatment with the carbon-containing layer or reducing atmosphere, it is not limited here.
[0107] Among them, when the metal sheet 13 is a single metal sheet, or the metal sheet 13 is multi-layered and the material of the top metal layer is the same as that of the bottom metal layer, since the ohmic contact layer 221 is formed by the reaction of the silicon carbide epitaxial wafer 21 and the top metal layer of the metal sheet 13, and the metal conductive layer 223 is formed by the reaction of the carbon-containing layer 14 or the reducing atmosphere and the bottom metal layer of the metal sheet 13, the ohmic contact layer 221, the metal buffer layer 222 and the metal conductive layer 223 contain the same metal elements.
[0108] In one embodiment, to simplify the preparation process, the metal buffer layer 222 is a single metal layer, the ohmic contact layer 221 contains only one metal element, and the metal conductive layer 223 contains only one metal element. The metal element contained in the ohmic contact layer 221 and the metal conductive layer 223 is the same as the metal element contained in the metal buffer layer 222.
[0109] The ohmic contact layer 221 is an intermediate layer between the highly doped region (the first source region 303 and the second source region 305) and the metal wiring in the silicon carbide epitaxial wafer 21, and plays the role of a potential barrier transition between metal and semiconductor, thereby improving its conductivity and reducing electrical loss. Therefore, the ohmic contact layer 221 should not be too thick to ensure the stability of the physical properties in all directions.
[0110] In addition, the metal buffer layer 222 acts as a stress buffer layer between the ohmic contact layer 221 and the metal conductive layer 223. Because the above two exist in the form of large-sized grains, they have poor adhesion and stress matching. Therefore, the thickness of the metal buffer layer 222 here can achieve the stress buffering effect. Specifically, as the thickness of the metal buffer layer 222 increases, the buffering effect becomes more obvious. If the thickness of the metal buffer layer 222 is too low, the buffering requirements cannot be met. If the thickness of the metal buffer layer 222 is too high, the overall resistivity of the device unit is increased. Therefore, the thickness of the metal buffer layer 222 needs to be reasonably designed according to actual conditions.
[0111] Finally, the metal conductive layer 223 is formed by a high-temperature reaction between a single metal and the carbon-containing layer 14 or a reducing atmosphere. Due to factors such as reaction time and kinetic regulation, its thickness needs to be maintained within an appropriate range.
[0112] To meet the above conditions, in some embodiments of the present application, the thickness of the metal buffer layer 222 is greater than or equal to the thickness of the metal conductive layer 223 ; and the thickness of the metal buffer layer 222 is greater than or equal to the thickness of the ohmic contact layer 221 .
[0113] In one embodiment, the ratio of the thickness of the ohmic contact layer 221 , the thickness of the metal buffer layer 222 , and the thickness of the metal conductive layer 223 is (1-10):(3-45):(1-10). For example, the ratio of the thickness of the ohmic contact layer 221, the thickness of the metal buffer layer 222 and the thickness of the metal conductive layer 223 is 1:3:1; or the ratio of the thickness of the ohmic contact layer 221, the thickness of the metal buffer layer 222 and the thickness of the metal conductive layer 223 is 10:3:10; or the ratio of the thickness of the ohmic contact layer 221, the thickness of the metal buffer layer 222 and the thickness of the metal conductive layer 223 is 1:3:10; or the ratio of the thickness of the ohmic contact layer 221, the thickness of the metal buffer layer 222 and the thickness of the metal conductive layer 223 is 1:20:1; or the ratio of the thickness of the ohmic contact layer 221, the thickness of the metal buffer layer 222 and the thickness of the metal conductive layer 223 is 1:45:1; or the ratio of the thickness of the ohmic contact layer 221, the thickness of the metal buffer layer 222 and the thickness of the metal conductive layer 223 is 5:15:5, etc., which is not limited here and can be designed according to actual needs.
[0114] In some embodiments, the thickness of the ohmic contact layer 221 is 10-100 nanometers. For example, the thickness of the ohmic contact layer 221 is 10 nanometers; or the thickness of the ohmic contact layer 221 is 50 nanometers; or the thickness of the ohmic contact layer 221 is 100 nanometers, etc., which are not limited here and can be designed according to actual needs.
[0115] The thickness of the metal buffer layer 222 is 30-450 nanometers. For example, the thickness of the metal buffer layer 222 is 30 nanometers; or the thickness of the metal buffer layer 222 is 100 nanometers; or the thickness of the metal buffer layer 222 is 300 nanometers; or the thickness of the metal buffer layer 222 is 450 nanometers, etc., which are not limited here and can be designed according to actual needs.
[0116] In some embodiments, the thickness of the metal conductive layer 223 is 10-100 nanometers. For example, the thickness of the metal conductive layer 223 is 10 nanometers; or the thickness of the metal conductive layer 223 is 50 nanometers; or the thickness of the metal conductive layer 223 is 100 nanometers, etc., which is not limited here and can be designed according to actual needs.
[0117] Specifically, the design of the thickness range of each of the above-mentioned film layers is specifically based on the film layer function, process cost, time, and taking into account the stability of its electrical performance and other aspects.
[0118] In one embodiment, the semiconductor device further includes a metal connection layer 23, which is disposed on a surface of the metal conductive layer 223 that is away from the metal buffer layer 222. Specifically, the metal connection layer 23 serves as a metal connection of the device, and the material of the metal connection layer 23 is a conductive metal, wherein the material of the metal connection layer 23 includes but is not limited to metal aluminum, metal copper, etc., and is used to correspond to and electrically connect each ohmic contact metal layer 22 one by one.
[0119] The number of the metal connection layers 23 is the same as the number of the ohmic contact metal layers 22 to provide a transmission path between the device and external electrical signals.
[0120] Wherein, based on the design size of the semiconductor device, the thickness of each metal connection layer 23 is 2-4 microns. For example, the thickness of each gold metal connection layer 23 is 2 microns; or the thickness of each metal connection layer 23 is 3 microns; or the thickness of each metal connection layer 23 is 4 microns, etc., which will not be described in detail here, and can be specifically designed according to actual needs.
[0121] In one embodiment, the semiconductor device further includes a gate structure 24, a source structure 25, a drain structure 26, etc., arranged corresponding to each semiconductor cell 30, and an insulating layer 27 for device insulation. The functions and structures thereof are the same as those of the prior art, and are not described in detail here.
[0122] The above description is only an implementation method of the present application, and does not limit the patent scope of the present application. Any equivalent structure or equivalent process transformation made using the contents of the present application specification and drawings, or directly or indirectly used in other related technical fields, are also included in the patent protection scope of the present application.
Claims
1. A method for preparing a semiconductor device, characterized in that: include: Providing a silicon carbide epitaxial wafer; forming an ohmic contact metal layer on the surface of the silicon carbide epitaxial wafer; Among them, the ohmic contact metal layer includes an ohmic contact layer, a metal buffer layer and a metal conductive layer, the ohmic contact layer is arranged on the silicon carbide epitaxial wafer, the metal buffer layer is arranged on the ohmic contact layer, the metal conductive layer is arranged on the metal buffer layer, and the metal buffer layer is located between the ohmic contact layer and the metal conductive layer; the ohmic contact layer includes metal silicide, and the metal conductive layer includes a compound composed of a reducing non-metallic element and a metal.
2. The preparation method according to claim 1, characterized in that: The forming of an ohmic contact metal layer on the surface of the silicon carbide epitaxial wafer comprises: forming a metal layer on the surface of the silicon carbide epitaxial wafer; The silicon carbide epitaxial wafer having the metal layer formed thereon is subjected to a thermal reduction treatment using a reducing non-metallic element, so as to form the ohmic contact metal layer on the surface of the silicon carbide epitaxial wafer.
3. The preparation method according to claim 2, characterized in that: The step of using a reducing non-metallic element to perform a thermal reduction treatment on the silicon carbide epitaxial wafer having the metal layer formed thereon to form the ohmic contact metal layer on the surface of the silicon carbide epitaxial wafer comprises: forming a carbon-containing layer on a surface of the metal layer away from the silicon carbide epitaxial wafer; thermally treating the silicon carbide epitaxial wafer having the metal layer and the carbon-containing layer formed thereon, so as to form the ohmic contact metal layer on the surface of the silicon carbide epitaxial wafer; The ohmic contact layer is formed by thermal reaction between the metal layer and the silicon carbide epitaxial wafer, the metal conductive layer is formed by thermal reaction between the metal layer and the carbon-containing layer, and the unreacted portion of the metal layer serves as the metal buffer layer.
4. The preparation method according to claim 3, characterized in that: The ratio of the thickness of the metal layer to the thickness of the carbon-containing layer is 1:(0.1-10); and / or, The thickness of the metal layer is 50 to 500 nanometers; the thickness of the carbon-containing layer is 50 to 500 nanometers.
5. The preparation method according to claim 3, characterized in that: Also includes: removing the carbon-containing layer remaining on the surface of the metal conductive layer away from the silicon carbide epitaxial wafer; A metal connection layer is formed on a surface of the metal conductive layer facing away from the silicon carbide epitaxial wafer.
6. The preparation method according to claim 5, characterized in that: The metal layer is a single metal layer; the metal layer is grown by magnetron sputtering; The carbon-containing layer is a carbon layer; the carbon-containing layer is grown by magnetron sputtering; The step of heat treating the silicon carbide epitaxial wafer having the metal layer and the carbon-containing layer formed thereon comprises: Under oxygen-free conditions, heating the silicon carbide epitaxial wafer having the metal layer and the carbon-containing layer formed thereon at 800-1200 degrees Celsius for 10-500 minutes to form the ohmic contact layer, the metal buffer layer and the metal conductive layer on the silicon carbide epitaxial wafer; The removing of the carbon-containing layer remaining on the surface of the metal conductive layer away from the silicon carbide epitaxial wafer comprises: Using plasma etching to remove the carbon-containing layer remaining on the surface of the metal conductive layer away from the silicon carbide epitaxial wafer; The forming of a metal connection layer on a surface of the metal conductive layer away from the silicon carbide epitaxial wafer comprises: The metal connection layer is grown on the surface of the metal conductive layer away from the silicon carbide epitaxial wafer by magnetron sputtering.
7. The preparation method according to claim 2, characterized in that: The step of using a reducing non-metallic element to perform a thermal reduction treatment on the silicon carbide epitaxial wafer having the metal layer formed thereon to form the ohmic contact metal layer on the surface of the silicon carbide epitaxial wafer comprises: thermally treating the silicon carbide epitaxial wafer having the metal layer formed thereon in a reducing atmosphere to form the ohmic contact metal layer on the surface of the silicon carbide epitaxial wafer; The ohmic contact layer is formed by thermal reaction between the metal layer and the silicon carbide epitaxial wafer, the metal conductive layer is formed by thermal reaction between the metal layer and the reducing atmosphere, and the unreacted portion of the metal layer serves as the metal buffer layer.
8. The preparation method according to claim 7, characterized in that: The metal layer is a single metal layer; the reducing atmosphere includes ammonia, sulfur vapor, selenium vapor or phosphine.
9. The preparation method according to claim 2, characterized in that: The metal layer includes at least one of nickel, molybdenum, titanium, cobalt, and aluminum.
10. A semiconductor device, characterized in that: include: Silicon carbide epitaxial wafers; An ohmic contact metal layer, comprising an ohmic contact layer, a metal buffer layer and a metal conductive layer, wherein the ohmic contact layer is disposed on the silicon carbide epitaxial wafer, the metal buffer layer is disposed on the ohmic contact layer, the metal conductive layer is disposed on the metal buffer layer, and the metal buffer layer is located between the ohmic contact layer and the metal conductive layer; Wherein, the ohmic contact layer includes metal silicide, and the metal conductive layer includes a compound composed of a reducing non-metallic element and a metal.
11. The semiconductor device according to claim 10, characterized in that The ratio of the thickness of the ohmic contact layer, the thickness of the metal buffer layer and the thickness of the metal conductive layer is (1-10):(3-45):(1-10); and / or, The thickness of the ohmic contact layer is 10-100 nanometers; the thickness of the metal buffer layer is 30-450 nanometers; and the thickness of the metal conductive layer is 10-100 nanometers.
12. The semiconductor device according to claim 10, characterized in that The metal buffer layer includes at least one of nickel, molybdenum, titanium, cobalt and aluminum; The metal conductive layer includes at least one of metal carbide, metal nitride, metal sulfide, metal phosphide and metal selenide.
13. The semiconductor device according to claim 12, characterized in that The ohmic contact layer, the metal buffer layer and the metal conductive layer contain the same metal element; and / or, The ohmic contact layer contains only one metal element, the metal buffer layer is a single metal layer, and the metal conductive layer contains only one metal element.
14. The semiconductor device according to claim 10, characterized in that A plurality of semiconductor cells are arranged in the silicon carbide epitaxial wafer, each of the semiconductor cells comprises a first base region and a second base region arranged at intervals, a first source region and a first contact region connected to each other are arranged in the first base region, and a second source region and a second contact region connected to each other are arranged in the second base region; The semiconductor device comprises a plurality of ohmic contact metal layers arranged at intervals, and one ohmic contact metal layer is respectively arranged on the first source region and the second source region in each of the cells.