Preparation method of low-hole all-intermetallic compound welding spot

By sequentially depositing a Cu-Zn metal layer, Fe nanocrystalline film and Sn solder layer on the wafer surface, and performing solid-liquid interdiffusion bonding, the reaction between the Fe nanocrystalline film and the Sn solder layer is used to generate a dense initial interface layer. It solves the problem of too fast diffusion rate of Cu atoms, reduces the generation of holes, and improves the reliability of all-intermetallic compound solder joints.

CN118737859APending Publication Date: 2024-10-01CHANGZHOU UNIV
View PDF 0 Cites 0 Cited by

Patent Information

Application Number
CN202410852930.3
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Filing Date
2024-06-28
Publication Date
2024-10-01

AI Technical Summary

Technical Problem

During the solid-liquid interdiffusion bonding process, the diffusion rate of Cu atoms is faster than that of Sn atoms, resulting in a large number of Kirkendall holes inside the all-intermetallic compound solder joints, which affects the reliability of the solder joints.

Method used

Cu-Zn metal layer, Fe nanocrystalline film, Sn solder layer and In solder layer are sequentially deposited on the wafer surface, and solid-liquid interdiffusion bonding is performed. Through the reaction of the Fe nanocrystalline film and the Sn solder layer, a dense The initial interface layer limits the diffusion of Cu atoms, reduces the melting point of the solder through the In solder layer, and inhibits the diffusion rate of Cu atoms.

Benefits of technology

Significantly reduces the formation of holes in all-intermetallic compound solder joints, improves the reliability of solder joints, and ensures that solder joints are almost free of holes.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN118737859A_ABST
    Figure CN118737859A_ABST
Patent Text Reader

Abstract

The invention discloses a preparation method of a low-hole all-intermetallic compound welding spot, which comprises the following steps that: 1) a Cu-Zn metal layer with the thickness of 0.1-5 microns is deposited in a to-be-bonded area on the surface of a wafer, and the mass percent of Zn in the Cu-Zn metal layer is 5-20wt%; 2) depositing a Fe nanocrystalline film with the thickness of 10-50nm on the Cu-Zn metal layer of the wafer obtained in the step 1); (3) a Sn brazing filler metal layer and an In brazing filler metal layer are sequentially deposited on the Fe nanocrystalline film of the wafer obtained in the step (2); and 4) butting the to-be-bonded areas of the two wafers on which the Cu-Zn metal layer, the Fe nanocrystalline film, the Sn brazing filler metal layer and the In brazing filler metal layer are deposited in sequence, and carrying out solid-liquid mutual diffusion bonding treatment to obtain the low-hole all-intermetallic compound welding spot. The all-intermetallic compound welding spot prepared from the brazing filler metal is almost free of holes, and the reliability of the all-intermetallic compound welding spot can be remarkably improved.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The invention belongs to the technical field of chip stacking interconnection, and in particular relates to a method for preparing a low-void all-intermetallic compound solder joint. Background Art

[0002] As electronic products gradually develop in the direction of miniaturization, intelligence and high integration, higher requirements are undoubtedly placed on traditional electronic packaging technology. In this context, three-dimensional packaging technology has been applied. Three-dimensional packaging refers to stacking multiple chips layer by layer in the vertical space. It can not only greatly improve the stacking density but also accelerate the chip transmission speed, becoming the packaging technology with the most application prospects. In three-dimensional packaging technology, the stacking connection between chips is one of the most critical technologies. At present, common chip connection methods are: soldering connection, adhesive connection, hot pressing bonding and solid-liquid interdiffusion bonding. Among them, solid-liquid interdiffusion bonding has become the most widely used connection method for chip stacking because the bonded solder joints are resistant to high temperatures and the bonding temperature and time are suitable. However, in the solid-liquid interdiffusion process, when the bonding temperature is 250°C, the diffusion rate of Cu atoms in the metal layer is 30 times faster than that of Sn atoms. The imbalance of the diffusion rate leads to the appearance of a large number of Kirkendall holes inside the bonded all-metallic compound solder joints, and as the solder joint organization evolves, Cu 6 Sn 5 Cu 3 There is volume shrinkage during the Sn phase transformation process, which further aggravates the formation of voids and seriously affects the reliability of the solder joints.

[0003] In the prior art, the diffusion rate of Cu atoms and Sn atoms is mainly controlled by electroplating a barrier layer on the Cu metal layer or adding a small amount of alloy elements to the Sn solder, thereby reducing the appearance of holes. However, due to the long bonding time, the electroplating barrier layer has limited ability to inhibit the diffusion rate of Cu atoms in the metal layer, and the added alloy elements are easily evaporated or squeezed out, resulting in a gradual increase in the diffusion rate of Cu atoms in the later stage of bonding, and many holes still exist in the fully prepared intermetallic compound solder joint. Summary of the invention

[0004] In order to solve the above technical problems, the present invention provides a method for preparing a low-void all-intermetallic compound solder joint, by sequentially depositing a Cu-Zn metal layer, a Fe nanocrystalline film, a Sn solder layer and an In solder layer on the bonding area on the surface of a wafer, and performing solid-liquid interdiffusion bonding to prepare a nearly void-free all-intermetallic compound solder joint.

[0005] The technical solution adopted by the present invention is as follows:

[0006] 1) depositing a Cu-Zn metal layer on the surface of the wafer in the bonding area;

[0007] 2) depositing a Fe nanocrystalline film on the Cu-Zn metal layer of the wafer obtained in step 1);

[0008] 3) depositing a Sn solder layer and an In solder layer in sequence on the Fe nanocrystalline film of the wafer obtained in step 2);

[0009] 4) The bonding areas of two wafers on which the Cu-Zn metal layer, the Fe nanocrystalline film, the Sn solder layer and the In solder layer are sequentially deposited are butt-jointed, and solid-liquid interdiffusion bonding treatment is performed to obtain a low-porous all-metallic compound solder joint.

[0010] Furthermore, in step 1), the thickness of the Cu-Zn metal layer is 0.1 to 5 μm.

[0011] Furthermore, in the Cu-Zn metal layer, the mass percentage of Zn is 5 to 20 wt %.

[0012] Furthermore, in step 1), the Cu-Zn layer is deposited by magnetron sputtering technology, and the magnetron sputtering process parameters are: sputtering power 100-200W, sputtering pressure 1.1-4.5Pa, sputtering gas flow 20-50sccm, and sputtering time 0.1-3h.

[0013] Furthermore, in step 2), the thickness of the Fe nanocrystalline film is 10 to 50 nm.

[0014] Furthermore, in step 2), magnetron sputtering technology is used to deposit Fe nanocrystalline film, and the magnetron sputtering process parameters are: sputtering power 50-150 W, sputtering pressure 1.1-4.5 Pa, sputtering gas flow 20-50 sccm, and sputtering time 0.02-0.5 h.

[0015] Furthermore, in step 3), the total thickness of the Sn solder layer and the In solder layer is 5 to 50 μm, and the thickness ratio of the Sn solder layer to the In solder layer is 1:1.08.

[0016] Furthermore, in step 3), the Sn solder layer is deposited by magnetron sputtering technology, and the magnetron sputtering process parameters are: sputtering power 100-300W, sputtering pressure 1.1-4.5Pa, sputtering gas flow 20-50sccm, and sputtering time 0.5-5h.

[0017] Furthermore, in step 3), the In solder layer is deposited by magnetron sputtering technology, and the magnetron sputtering process parameters are: sputtering power 100-300 W, sputtering pressure 1.1-4.5 Pa, sputtering gas flow 20-50 sccm, and sputtering time 0.5-5 h.

[0018] Furthermore, in step 4), the solid-liquid interdiffusion bonding process parameters are: bonding temperature 150-250°C, bonding time 0.5-3h, vacuum degree 2.0×10-3 ~5.0×10 -5 Pa.

[0019] Beneficial effects of the present invention:

[0020] 1) The present invention deposits a Cu-Zn metal layer on the wafer to be bonded, and controls the diffusion rate of Cu atoms into the Sn solder during the bonding process by changing the concentration of Cu in the Cu-Zn metal layer, thereby reducing the Kirkendall holes caused by the imbalance of the diffusion rates of Cu and Sn atoms.

[0021] 2) In the present invention, a Fe nanocrystalline film is deposited on the Cu-Zn metal layer, and during the bonding process, the Fe nanocrystalline film reacts with the Sn solder layer to generate a dense and fine FeSn with a preferred orientation. 2 The initial interface layer further limits the diffusion of Cu atoms and vertically fine FeSn 2 The grains provide a stable diffusion channel for the diffusion of Cu atoms, thus facilitating the diffusion of Cu atoms in the later stage of bonding. 6 (Sn,In) 5 +Cu 6 (Sn,Zn) 5 The uniform growth of the mixed phase creates conditions that reduce the generation of voids.

[0022] 3) The present invention can form Sn52In eutectic solder by sequentially depositing Sn solder layer and In solder layer on Fe nanocrystalline film, thereby reducing the melting point of solder and the bonding temperature, and once again suppressing the diffusion rate of Cu atoms into Sn solder. In addition, the In solder layer reacts metallurgically with the Sn solder layer and Cu-Zn metal layer to form a more stable Cu 6 (Sn,In) 5 +Cu 6 (Sn,Zn) 5 The mixed phase hinders the volume shrinkage caused by the phase transformation of the intermetallic compound.

[0023] In summary, the present invention deposits a Cu-Zn metal layer, a Fe nanocrystalline film, a Sn solder layer and an In solder layer in sequence on the wafer surface to be bonded, and the full intermetallic compound solder joint prepared by solid-liquid interdiffusion bonding is almost free of holes, which can significantly improve the reliability of the full intermetallic compound solder joint. BRIEF DESCRIPTION OF THE DRAWINGS

[0024] Figure 1 It is a schematic diagram of the structure in which different structural layers are deposited in sequence in the wafer bonding area of ​​the present invention.

[0025] Figure 2 It is a schematic diagram of the process of solid-liquid interdiffusion bonding of two wafers of the present invention.

[0026] Figure 3 This is an electron microscope image of the low-void all-intermetallic compound solder joint obtained in Example 1.

[0027] Figure 4 In the bonding process of Example 1, the Fe nanocrystalline film reacts with the Sn solder layer to form an initial interface layer FeSn 2 Electron microscope image of .

[0028] Figure 5 The initial interface layer FeSn of Example 1 2 Electron microscope image.

[0029] Figure 6 This is an electron microscope image of the void-free all-intermetallic compound solder joint obtained in Example 2.

[0030] Figure 7 This is an electron microscope image of the void-free all-intermetallic compound solder joint obtained in Example 3. DETAILED DESCRIPTION

[0031] In order to make the purpose, technical solution and advantages of the present invention more clearly understood, the present invention is further described in detail below in conjunction with the accompanying drawings and embodiments. The specific embodiments are only used to explain the present invention, but are not limited to these embodiments.

[0032] Example 1

[0033] A method for preparing a low-void all-intermetallic compound solder joint, the steps are as follows:

[0034] 1) Deposit a Cu-Zn metal layer on the wafer surface in the bonding area:

[0035] 1.1) First, pre-treat the wafer by ultrasonically cleaning the wafer in an acetone solution for 6 minutes to remove organic matter, then cleaning it in an isopropanol solution for 6 minutes to remove acetone and acetone-soluble organic matter, and then ultrasonically cleaning it in alcohol for 6 minutes. Rinse it continuously with deionized water, blow it dry with a nitrogen gun, and put it in a drying oven for use.

[0036] 1.2) A Cu-Zn metal layer is deposited on the bonding area of ​​the pretreated wafer surface by magnetron sputtering technology, wherein the Cu target and the Zn target are spliced ​​into a circular target by a target splicing method, that is, 3 / 4 of the Cu target and 1 / 4 of the Zn target are spliced ​​into a circular target. The sputtering power is 100 W, the sputtering pressure is 1.1 Pa, the sputtering argon gas flow is 20 sccm, and the sputtering time is 0.1 h, to obtain a 0.1 μm thick Cu-Zn metal layer, and the mass percentage of Zn in the Cu-Zn metal layer is 5wt%.

[0037] 2) Depositing an Fe nanocrystalline film on the Cu-Zn metal layer of the wafer obtained in step 1) by direct current magnetron sputtering technology, with a sputtering power of 50 W, a sputtering pressure of 1.3 Pa, a sputtering argon gas flow of 20 sccm, and a sputtering time of 0.05 h to obtain a 10 nm thick Fe nanocrystalline film.

[0038] 3) depositing a Sn solder layer on the Fe nanocrystalline film of the wafer obtained in step 2) by magnetron sputtering technology, with a sputtering power of 100 W, a sputtering pressure of 2.0 Pa, a sputtering argon gas flow of 20 sccm, and a sputtering time of 0.6 h, to obtain a 2.4 μm thick Sn solder layer;

[0039] Then the In target was opened, and the In solder layer was deposited on the Sn solder layer by magnetron sputtering technology. The sputtering power was 120 W, the sputtering pressure was 2.0 Pa, the sputtering argon gas flow was 50 sccm, and the sputtering time was 0.5 h. A 2.6 μm thick In solder layer was obtained. The wafer structure of the Cu-Zn metal layer, Fe nanocrystalline film, Sn solder layer and In solder layer was deposited in sequence is shown in FIG. Figure 1 .

[0040] 4) See Figure 2 The bonding areas of two wafers on which Cu-Zn metal layer, Fe nanocrystalline film, Sn solder layer and In solder layer were deposited in sequence were butt-jointed and solid-liquid interdiffusion bonding was performed. The bonding temperature was 150 °C, the bonding time was 0.5 h, and the vacuum degree was 2.0 × 10 -5 Pa, and naturally cool after bonding to obtain a low-void full intermetallic compound solder joint.

[0041] The obtained low-void all-metallic compound solder joint was observed by electron microscope. Figure 3 ,from Figure 3 It can be seen that there are almost no holes in the solder joints.

[0042] During the solid-liquid interdiffusion bonding process, the Fe nanocrystalline film reacts with the Sn solder layer to form FeSn 2 Initial interface layer. At this time, the two bonded wafers are taken out and observed by electron microscope. The electron microscope image is shown in Figure 4 ,from Figure 4 It can be seen that the Fe nanocrystalline film reacts with the Sn solder layer to form a very thin layer of FeSn 2 Initial interface layer, FeSn 2 The initial interface layer can limit the diffusion rate of Cu atoms in the Cu-Zn metal layer into Sn.

[0043] Place the two wafers along the FeSn 2 Initial interface layer segmentation, FeSn observed by electron microscopy 2 Initial interface layer, electron microscope image see Figure 5,from Figure 5 It can be seen that the fine FeSn 2 The grains grow vertically to the Fe nanocrystalline film, which can provide a stable diffusion channel for the diffusion of Cu atoms.

[0044] Example 2

[0045] A method for preparing a low-void all-intermetallic compound solder joint, the steps are as follows:

[0046] 1) depositing a Cu-Zn metal layer on the surface of the wafer in the bonding area;

[0047] 1.1) First, pre-treat the wafer by ultrasonically cleaning the wafer in an acetone solution for 6 minutes to remove organic matter, then cleaning it in an isopropanol solution for 6 minutes to remove acetone and acetone-soluble organic matter, and then ultrasonically cleaning it in alcohol for 6 minutes. Rinse it continuously with deionized water, blow it dry with a nitrogen gun, and put it in a drying oven for use.

[0048] 1.2) A Cu-Zn metal layer was deposited on the bonding area of ​​the pretreated wafer surface by magnetron sputtering technology, wherein the Cu target and the Zn target were spliced ​​into a circular target by a target splicing method, i.e., 3 / 4 of the Cu target and 1 / 4 of the Zn target were spliced ​​into a circular target. The sputtering power was 150 W, the sputtering pressure was 3.0 Pa, the sputtering argon gas flow was 30 sccm, the sputtering time was 1 h, and a 1.0 μm thick Cu-Zn metal layer was obtained, and the mass percentage of Zn in the Cu-Zn metal layer was 15 wt%.

[0049] 2) Depositing an Fe nanocrystalline film on the Cu-Zn metal layer of the wafer obtained in step 1) by direct current magnetron sputtering technology, with a sputtering power of 80 W, a sputtering pressure of 2.5 Pa, a sputtering argon gas flow of 30 sccm, and a sputtering time of 0.16 h to obtain a 25 nm thick Fe nanocrystalline film.

[0050] 3) depositing a Sn solder layer on the Fe nanocrystalline film of the wafer obtained in step 2) by magnetron sputtering technology, with a sputtering power of 200 W, a sputtering pressure of 3.0 Pa, a sputtering argon gas flow of 30 sccm, and a sputtering time of 1 h, to obtain a 10 μm thick Sn solder layer;

[0051] Then the In target was opened, and the In solder layer was deposited on the Sn solder layer by magnetron sputtering technology. The sputtering power was 150 W, the sputtering pressure was 3.0 Pa, the sputtering argon gas flow was 50 sccm, and the sputtering time was 1.3 h. A 10.8 μm thick In solder layer was obtained. The wafer structure of the Cu-Zn metal layer, Fe nanocrystalline film, Sn solder layer and In solder layer was deposited in sequence is shown in FIG. Figure 1 .

[0052] 4) See Figure 2The bonding areas of two wafers on which Cu-Zn metal layer, Fe nanocrystalline film, Sn solder layer and In solder layer were deposited in sequence were butt-jointed and solid-liquid interdiffusion bonding was performed. The bonding temperature was 200 °C, the bonding time was 1.5 h, and the vacuum degree was 4.0×10 -5 Pa, after the bonding is completed, it is cooled naturally to obtain a void-free full intermetallic compound solder joint.

[0053] The obtained hole-free full metal intermetallic compound solder joint was observed by electron microscope. Figure 6 ,from Figure 6 It can be seen that no holes are visible in the solder joint.

[0054] Example 3

[0055] A method for preparing a low-void all-intermetallic compound solder joint, the steps are as follows:

[0056] 1) Deposit a Cu-Zn metal layer on the wafer surface in the bonding area:

[0057] 1.1) First, pre-treat the wafer by ultrasonically cleaning the wafer in an acetone solution for 6 minutes to remove organic matter, then cleaning it in an isopropanol solution for 6 minutes to remove acetone and acetone-soluble organic matter, and then ultrasonically cleaning it in alcohol for 6 minutes. Rinse it continuously with deionized water, blow it dry with a nitrogen gun, and put it in a drying oven for use.

[0058] 1.2) A Cu-Zn metal layer is deposited on the bonding area of ​​the pretreated wafer surface by magnetron sputtering technology, wherein the Cu target and the Zn target are spliced ​​into a circular target by a target splicing method, that is, 3 / 4 of the Cu target and 1 / 4 of the Zn target are spliced ​​into a circular target. The sputtering power is 200 W, the sputtering pressure is 4.5 Pa, the sputtering argon gas flow is 30 sccm, and the sputtering time is 3.0 h, to obtain a 5.0 μm thick Cu-Zn metal layer, and the mass percentage of Zn in the Cu-Zn metal layer is 20 wt%.

[0059] 2) Depositing an Fe nanocrystalline film on the Cu-Zn metal layer of the wafer obtained in step 1) by direct current magnetron sputtering technology, with a sputtering power of 150 W, a sputtering pressure of 4.0 Pa, a sputtering argon gas flow of 50 sccm, and a sputtering time of 0.25 h to obtain a 50 nm thick Fe nanocrystalline film.

[0060] 3) depositing a Sn solder layer on the Fe nanocrystalline film of the wafer obtained in step 2) by magnetron sputtering technology, with a sputtering power of 300 W, a sputtering pressure of 4.5 Pa, a sputtering argon gas flow of 50 sccm, and a sputtering time of 2.4 h, to obtain a 24 μm thick Sn solder layer;

[0061] Then the In target was opened, and the In solder layer was deposited on the Sn solder layer by magnetron sputtering technology. The sputtering power was 300 W, the sputtering pressure was 4.5 Pa, the sputtering argon gas flow was 50 sccm, and the sputtering time was 2.5 h. A 26 μm thick In solder layer was obtained. The wafer structure of the Cu-Zn metal layer, Fe nanocrystalline film, Sn solder layer and In solder layer was deposited in sequence is shown in FIG. Figure 1 .

[0062] 4) See Figure 2 The bonding areas of two wafers on which Cu-Zn metal layer, Fe nanocrystalline film, Sn solder layer and In solder layer were deposited in sequence were butt-jointed and solid-liquid interdiffusion bonding was performed. The bonding temperature was 250 °C, the bonding time was 2 h, and the vacuum degree was 5.0 × 10 -5 Pa, after the bonding is completed, it is cooled naturally to obtain a void-free full intermetallic compound solder joint.

[0063] The obtained hole-free full metal intermetallic compound solder joint was observed by electron microscope. Figure 7 ,from Figure 7 It can be seen that no holes are visible in the solder joint.

[0064] The above description is only a preferred embodiment of the present invention. It should be pointed out that a person skilled in the art can make several improvements without departing from the principle of the present invention, and these improvements should also be regarded as within the protection scope of the present invention.

Claims

1. A method for preparing a low-void all-intermetallic compound solder joint, characterized in that: The steps include: 1) depositing a Cu-Zn metal layer on the surface of the wafer in the bonding area; 2) depositing a Fe nanocrystalline film on the Cu-Zn metal layer of the wafer obtained in step 1); 3) depositing a Sn solder layer and an In solder layer in sequence on the Fe nanocrystalline film of the wafer obtained in step 2); 4) The bonding areas of two wafers on which the Cu-Zn metal layer, the Fe nanocrystalline film, the Sn solder layer and the In solder layer are sequentially deposited are butt-jointed, and solid-liquid interdiffusion bonding treatment is performed to obtain a low-porous all-metallic compound solder joint.

2. The method for preparing a low-void all-intermetallic compound solder joint according to claim 1, characterized in that: In step 1), the thickness of the Cu-Zn metal layer is 0.1-5 μm.

3. A method for preparing a low-void all-intermetallic compound solder joint according to claim 1 or 2, characterized in that: In the Cu-Zn metal layer, the mass percentage of Zn is 5 to 20 wt%.

4. The method for preparing a low-void all-intermetallic compound solder joint according to claim 1, characterized in that: In step 1), the Cu-Zn layer is deposited by magnetron sputtering technology, and the magnetron sputtering process parameters are: sputtering power 100-200W, sputtering pressure 1.1-4.5Pa, sputtering gas flow 20-50sccm, and sputtering time 0.1-3h.

5. The method for preparing a low-void all-intermetallic compound solder joint according to claim 1, characterized in that: In step 2), the thickness of the Fe nanocrystalline film is 10 to 50 nm.

6. The method for preparing a low-void all-intermetallic compound solder joint according to claim 1, characterized in that: In step 2), the Fe nanocrystalline film is deposited by magnetron sputtering technology, and the magnetron sputtering process parameters are: sputtering power 50-150 W, sputtering pressure 1.1-4.5 Pa, sputtering gas flow 20-50 sccm, and sputtering time 0.02-0.5 h.

7. The method for preparing a low-void all-intermetallic compound solder joint according to claim 1, characterized in that: In step 3), the total thickness of the Sn solder layer and the In solder layer is 5 to 50 μm, and the thickness ratio of the Sn solder layer to the In solder layer is 1:1.

08.

8. The method for preparing a low-void all-intermetallic compound solder joint according to claim 1, characterized in that: In step 3), the Sn solder layer is deposited by magnetron sputtering technology, and the magnetron sputtering process parameters are: sputtering power 100-300W, sputtering pressure 1.1-4.5Pa, sputtering gas flow 20-50sccm, and sputtering time 0.5-5h.

9. The method for preparing a low-void all-intermetallic compound solder joint according to claim 1, characterized in that: In step 3), the In solder layer is deposited by magnetron sputtering technology, and the magnetron sputtering process parameters are: sputtering power 100-300W, sputtering pressure 1.1-4.5Pa, sputtering gas flow 20-50sccm, and sputtering time 0.5-5h.

10. The method for preparing a low-void all-intermetallic compound solder joint according to claim 1, characterized in that: In step 4), the solid-liquid interdiffusion bonding process parameters are: bonding temperature 150-250°C, bonding time 0.5-3h, vacuum degree 2.0×10 -3 ~5.0×10 -5 Pa.