Semiconductor device and preparation method thereof
By designing a structure without a first barrier layer or a thin first barrier layer in a III nitride HEMT device, combined with a channel layer and a second channel layer with a height difference, turn-off at a low threshold voltage is achieved. Normally-off semiconductor devices solve the safety hazards of existing HEMT devices and improve the safety and voltage resistance of the devices.
Patent Information
- Application Number
- CN202310327779.7
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Filing Date
- 2023-03-29
- Publication Date
- 2024-10-01
AI Technical Summary
Existing Group III nitride high electron mobility transistor (HEMT) devices are difficult to manufacture in a normally-off type and pose safety risks because the device cannot be turned off without voltage applied to the gate, causing the load to withstand high voltage.
A semiconductor device structure is designed, including a channel layer, a second barrier layer and a gate electrode, in which there is no first barrier layer between the gate electrode and the channel layer, or the thickness of the first barrier layer is such that no external Two-dimensional electron gas is not formed under voltage. By forming a channel layer and a second channel layer with height differences, a self-aligned structure is achieved to ensure that the device does not form a two-dimensional electron gas when there is no external voltage, so that it can operate at low temperatures. threshold voltage.
A normally-off semiconductor device that can be turned off at a low threshold voltage is realized, which improves the safety and voltage resistance of the device, avoids the safety hazard of the load being subjected to high voltage when the gate is open, and improves the application reliability of the device. .
Smart Images

Figure CN118738110A_ABST
Abstract
Description
Technical Field
[0001] The present invention relates to the field of semiconductor technology, and in particular to a semiconductor device. Background Art
[0002] Group III nitride semiconductors are an important new type of semiconductor material, mainly including AlN, GaN, InN and compounds of these materials such as AlGaN, InGaN, AlInGaN, etc. Due to the advantages of direct bandgap, wide bandgap, high breakdown electric field strength, etc., Group III nitride semiconductors represented by GaN have broad application prospects in the fields of light-emitting devices, power electronics, and radio frequency devices. For example, GaN-based LED devices have become the main electrical devices that emit green and blue light, and have been widely used in lighting, backlighting, display screens, and other fields.
[0003] Another important device type of III-nitride semiconductors is the high electron mobility transistor (HEMT), which has great prospects in the field of power semiconductors. Due to the existence of spontaneous polarization and piezoelectric polarization effects, there is a strong polarization positive charge at the interface between GaN and AlGaN on the (0001) plane. The presence of these polarization positive charges will attract and lead to the generation of two-dimensional electron gas at the interface. These two-dimensional electron gases have a high carrier concentration and a high carrier mobility, and are the core components for making high electron mobility transistors (HEMTs).
[0004] For conventional HEMT structures, the two-dimensional electron gas conducts current between the source and drain, and the gate electrode controls the switching of the device. However, since 2DEG always exists in GaN and AlGaN, the current can only be turned off by applying a large negative voltage to the gate electrode. In other words, the threshold voltage of this device is negative. In the absence of voltage on the gate, the device cannot be turned off, that is, it is a normally-on device. In many applications, this will bring great safety hazards. Because in the event of failure such as gate disconnection or power failure, the load will be subjected to a very high voltage, which poses a serious safety hazard. Therefore, an important obstacle for HEMT in applications is the difficulty in manufacturing normally-off devices.
[0005] The main purpose of the present invention is to provide a structure and a manufacturing method of a normally-off device. This technology has the characteristics of self-alignment. Summary of the invention
[0006] In view of the technical problems existing in the prior art, the present invention proposes a semiconductor device, comprising: a channel layer; a second barrier layer, which is located on the channel layer, wherein a two-dimensional electron gas 2DEG is formed in the channel layer near the interface between the channel layer and the second barrier layer; a source electrode; a drain electrode; and a gate electrode, which is located above the channel layer; wherein there is no first barrier layer between the gate electrode and the channel layer, or the thickness of the first barrier layer between the gate electrode and the channel layer is such that a heterojunction between the channel layer and the first barrier layer does not form a two-dimensional electron gas 2DEG in the absence of an external voltage; wherein the channel layer includes a first channel layer at least partially located below the gate electrode and a second channel layer below the second barrier layer.
[0007] Particularly, the channel layer includes a first channel layer at least partially located under the gate electrode and a second channel layer under the second barrier layer.
[0008] Particularly, there is a height difference between the first channel layer and the second channel layer, and the height difference is no greater than 100 nm; or no greater than 80 nm, or no greater than 50 nm, or no greater than 30 nm.
[0009] Particularly, the height difference is greater than 5 nm, or greater than 10 nm, or greater than 15 nm, or 20 nm.
[0010] Particularly, the second channel layer is located on at least a portion of the first channel layer, and the second channel layer is unintentionally doped or N-type doped.
[0011] Particularly, a nitride epitaxial layer is included below the channel layer.
[0012] Particularly, the nitride epitaxial layer is a third barrier layer, and a two-dimensional hole gas 2DHG is formed in the channel layer near the interface between the nitride epitaxial layer and the channel layer.
[0013] Particularly, the nitride epitaxial layer includes a substrate below.
[0014] Particularly, a gate insulating layer is included between the gate electrode and the channel layer.
[0015] Particularly, the gate electrode and the gate insulating layer are aligned by self-alignment.
[0016] In particular, it further comprises one or more insulating separation layers, which are located on the side of the gate electrode.
[0017] Particularly, an insulating layer is included above the second barrier layer.
[0018] In particular, it further includes a body electrode, a third barrier layer is included below the channel layer, and the body electrode is electrically connected to a 2DHG formed by a heterojunction of the channel layer and the third barrier layer.
[0019] The present application further includes a method for preparing a semiconductor device, comprising: forming a first channel layer; forming a sacrificial layer above the first channel layer; patterning the sacrificial layer, wherein the first channel layer is partially removed when patterning the sacrificial layer; forming a second channel layer and a second barrier layer located above the second channel layer, wherein a two-dimensional electron gas 2DEG is formed in the second channel layer near an interface between the second channel layer and the second barrier; removing the sacrificial layer and forming a gate electrode above the first channel layer, wherein there is no first barrier layer between the gate electrode and the channel layer; and forming a source electrode and a drain electrode located on both sides of the gate electrode.
[0020] Particularly, the method further comprises forming a gate insulating layer on the first channel layer; wherein the gate insulating layer is patterned when the sacrificial layer is patterned.
[0021] In particular, the first channel layer is not removed when the sacrificial layer is patterned.
[0022] Particularly, the method further comprises: forming a second channel layer on the first channel layer, wherein the second channel layer is unintentionally doped or N-type doped.
[0023] In particular, the method further comprises: forming a nitride epitaxial layer on the substrate, wherein the first channel layer is on the nitride epitaxial layer.
[0024] In particular, the nitride epitaxial layer includes a third barrier layer, and the first channel layer is formed on the third barrier layer.
[0025] In particular, the method further includes: forming a body electrode electrically connected to a 2DHG formed by a heterojunction of the first channel layer and the third barrier layer.
[0026] Particularly, the method further comprises: forming a first insulating layer on the patterned sacrificial layer, wherein the first insulating layer is at least located on a side wall of the sacrificial layer.
[0027] Particularly, the method further comprises: forming a second insulating layer after forming the second channel layer and the second barrier layer; and planarizing the second insulating layer and exposing the sacrificial layer.
[0028] Particularly, the gate electrode occupies the position of the sacrificial layer, thereby achieving self-alignment with the first barrier layer.
[0029] The present application further provides a method for preparing a semiconductor device, comprising: forming a first channel layer; forming a first barrier layer on the first channel layer, wherein the thickness of the first barrier layer is such that a two-dimensional electron gas 2DEG is not formed at a heterojunction between the first channel layer and the first barrier type in the absence of an external voltage; forming a sacrificial layer above the first barrier layer; patterning the sacrificial layer; forming a second barrier layer, wherein a two-dimensional electron gas 2DEG is formed in the channel layer near an interface between the channel layer and the second barrier; removing the sacrificial layer and forming a gate electrode above the channel layer; and forming a source electrode and a drain electrode.
[0030] Particularly, the method further comprises forming a gate insulating layer on the first channel layer; wherein the gate insulating layer is patterned when the sacrificial layer is patterned.
[0031] In particular, when patterning the sacrificial layer, the first barrier layer and a portion of the first channel layer are removed.
[0032] Particularly, the method further comprises: forming a second channel layer on the first channel layer, wherein the second channel layer is unintentionally doped or N-type doped.
[0033] Particularly, when the sacrificial layer is patterned, the first barrier layer is not removed; and the second barrier layer is directly formed on the first barrier layer.
[0034] Particularly, the method further comprises: forming a first insulating layer on the patterned sacrificial layer, wherein the first insulating layer is at least located on a side wall of the sacrificial layer.
[0035] Particularly, the method further comprises: forming a second insulating layer after forming the second channel layer and the second barrier layer; and planarizing the second insulating layer and exposing the sacrificial layer.
[0036] In particular, according to the method of claim 21, the gate electrode occupies the position of the sacrificial layer, thereby achieving self-alignment with the first barrier layer.
[0037] In particular, it further includes: forming a first barrier layer on the first channel layer, wherein the thickness of the first barrier layer is such that the heterojunction between the first channel layer and the first barrier layer does not form a two-dimensional electron gas 2DEG when no external voltage is applied; wherein, when patterning the sacrificial layer, the first barrier layer is patterned. BRIEF DESCRIPTION OF THE DRAWINGS
[0038] The preferred embodiments of the present invention will be further described in detail below with reference to the accompanying drawings, wherein:
[0039] Figure 1AA schematic diagram of a semiconductor device structure according to an embodiment of the present invention;
[0040] Figure 1B A schematic diagram of a semiconductor device structure according to an embodiment of the present invention;
[0041] Figure 2A-2V is a flow chart of a method for preparing a semiconductor device according to an embodiment of the present invention;
[0042] Figure 3 A schematic diagram of a semiconductor device structure according to an embodiment of the present invention; DETAILED DESCRIPTION
[0043] In order to make the purpose, technical solution and advantages of the embodiments of the present invention clearer, the technical solution in the embodiments of the present invention will be clearly and completely described below in conjunction with the drawings in the embodiments of the present invention. Obviously, the described embodiments are part of the embodiments of the present invention, not all of the embodiments. Based on the embodiments of the present invention, all other embodiments obtained by ordinary technicians in this field without creative work are within the scope of protection of the present invention.
[0044] In the following detailed description, reference may be made to the various specification drawings that are part of the present application and are used to illustrate specific embodiments of the present application. In the accompanying drawings, similar reference numerals describe substantially similar components in different figures. The various specific embodiments of the present application are described below in sufficient detail so that a person of ordinary skill in the art with relevant knowledge and skills in the art can implement the technical solutions of the present application. It should be understood that other embodiments may also be used or structural, logical or electrical changes may be made to the embodiments of the present application.
[0045] Figure 1A A schematic diagram of a semiconductor device structure according to an embodiment of the present invention. As shown in the figure, the semiconductor device includes: a substrate 101, on which a nitride epitaxial layer 102 is arranged. A channel layer 103 and a channel layer 104 are arranged on the nitride epitaxial layer 102. Among them, the channel layer 103 can be a first channel layer, and the channel layer 104 can be a second channel layer. In some embodiments, the channel layer 103 and the channel layer 104 can be a whole, and a groove is formed by etching technology. In some embodiments, the channel layer 103 has a boss structure 1031. A gate insulating layer 121, which is located on the boss structure 1031 of the channel layer 103. A gate electrode 115, which is located on the gate insulating layer 121. In some embodiments, the nitride epitaxial layer 102 is not necessary. In some embodiments, the gate insulating layer 121 is not necessary.
[0046] In some embodiments, a first barrier layer is included between the gate electrode 115 and the channel layer 103, wherein the first barrier layer is relatively thin, and the thickness of the first barrier layer between the gate electrode 115 and the channel layer 103 is such that, in the absence of an external voltage, the heterojunction between the channel layer 103 and the first barrier type does not form a two-dimensional electron gas 2DEG. In some embodiments, the first barrier layer is not included between the gate electrode 115 and the channel layer 103, and a two-dimensional electron gas 2DEG is not formed in the channel layer 103.
[0047] In some embodiments, the substrate may be removed by grinding, etching, etc. In some embodiments, the substrate 101 is not necessary.
[0048] The second channel layer 104 is located on the first channel layer 103 and in contact with the first channel layer 103 . The second channel layer 104 has two parts, which are respectively located on two sides of the boss structure 1031 of the first channel layer 103 .
[0049] The second barrier layer 108 is located on the second channel layer 104. The second barrier layer has two parts, which are respectively located on two parts of the second channel layer 104. The heterojunction between the second channel layer 104 and the second barrier layer 108 forms a two-dimensional electron gas 2DEG107.
[0050] The device further includes: a source electrode 111 and a drain electrode 113 . The source electrode 111 and the drain electrode 113 are electrically connected to the 2DEG 107 , respectively. A gate electrode 115 is located between the source electrode 111 and the drain electrode 113 , and is located above the boss structure 1031 of the first channel layer 103 .
[0051] Figure 1A In the structure shown, when the bias voltage applied to the gate 115 is lower than the threshold voltage, since there is no barrier layer (or a thin barrier layer) at the channel layer 103, 2DEG cannot be formed in the channel layer 103, no channel is formed, and carriers cannot pass through, so that the device is turned off. When a bias voltage higher than the threshold voltage is applied to the gate 115, a channel is formed in the channel layer 103, for example, at the boss structure 1031, connecting the 2DEG 107 on both sides, so that the carriers between the source electrode 111 and the drain electrode 113 can be smoothly transported, and the device can be turned on.
[0052] In some embodiments, there is a certain height difference between the first channel layer 103 and the second channel layer 104. In some embodiments, the height difference is not greater than 100 nm; or not greater than 80 nm, or not greater than 50 nm, or not greater than 30 nm. In some embodiments, the height difference is greater than 2 nm, or greater than 5 nm, or greater than 10 nm, or greater than 15 nm, or 20 nm.
[0053] According to one embodiment of the present invention, the material of the substrate 101 may be Si, SiC, intrinsic GaN or sapphire Al2O3, etc. In some embodiments, a Si substrate with lower cost and more mature process than other materials is selected as an example to illustrate the technical solution of the present invention. Those skilled in the art should understand that the substrate material of the present invention is not limited thereto.
[0054] In some embodiments, the nitride epitaxial layer 102 may be one or more of AlN, GaN, AlGaN, InGaN, AlInN and AlGaInN. The nitride epitaxial layer 102 may reduce the difference in lattice constant and thermal expansion coefficient between the substrate 101 and the upper channel layer 103, the channel layer 104, etc., avoid cracking of the nitride epitaxial layer, and improve device stability.
[0055] In some embodiments, a gate insulating layer 121 is included between the gate electrode 115 and the first channel layer 103. The gate insulating layer 121 may be made of any insulating material, such as SiN or SiO2. The gate insulating layer 121 may improve the voltage resistance of the gate electrode 115 and the entire device.
[0056] According to one embodiment of the present invention, the material of the channel layer 103 and the channel layer 104 may be GaN. According to one embodiment of the present invention, the material of the barrier layer 108 may be AlGaN. Those skilled in the art should understand that the back barrier layer, the channel layer and the barrier layer of the present invention are not limited thereto, and the bandgap width requirements between the three layers are met to form a corresponding 2DEG or 2DHG.
[0057] In some embodiments, the channel layer 104 is unintentionally doped or N-type doped.
[0058] In some embodiments, the gate electrode 115 is aligned with the channel layer 103 by self-alignment. In the semiconductor device of the present invention, the gate electrode 115 may be covered with a sacrificial layer first, and then the sacrificial layer is removed, so that a groove-like structure is formed between the channel layer 103 and the second barrier layer 108, and then the gate electrode 115 is formed. The process of forming the gate electrode 115 is subject to certain restrictions, so that the gate electrode 115 is located just above the channel layer 103.
[0059] Figure 1B A schematic diagram of a semiconductor device structure according to an embodiment of the present invention is shown in the figure. Figure 1B and Figure 1AThe structure of the first barrier layer 105 is similar and will not be described again. A first barrier layer 105 is included between the gate insulating layer 121 and the channel layer 103. The first barrier layer 105 is thin, and a 2DEG cannot be formed in the channel layer 103, and no channel is formed, so that carriers cannot pass through, and the device is turned off. In some embodiments, the lowest position of the first barrier layer 105 is lower than the highest position of the second channel layer 104.
[0060] In some embodiments, the semiconductor device further includes one or more insulating separation layers 122, which are located on the side of the gate electrode 115. The presence of the insulating separation layer 122 increases the distance from the side wall of the gate electrode 115 to the 2DEG107, which is conducive to reducing the electric field nearby and reducing the gate current. In some embodiments, the thickness of the insulating separation layer 122 is preferably less than 100nm. In some embodiments, it can further include a second insulating layer 123 extending from the side wall of the gate electrode 115 to both sides and located above the second barrier layer 108, which further increases the distance from the side wall of the gate electrode 115 to the 2DEG107, which is conducive to reducing the electric field nearby and reducing the gate current.
[0061] In some embodiments, the width of the gate electrode 115 may be greater than the width of the original sacrificial layer. Here, the portion of the gate electrode 115 located above the 2DEG 107 constitutes a field plate, which is beneficial to further reduce the electric field peak and improve the electric field distribution.
[0062] Figure 1B In the structure shown, when the bias voltage applied to the gate 115 is lower than the threshold voltage, since the thickness of the first barrier layer 105 is relatively thin, no channel is formed in the channel layer 103, and carriers cannot pass through, so that the device is turned off. When a bias voltage higher than the threshold voltage is applied to the gate 115, a channel is formed in the channel layer 103, for example, at the boss structure 1031, connecting the 2DEG 107 on both sides, so that the carriers between the source electrode 111 and the drain electrode 113 can be smoothly transported, and the device can be turned on.
[0063] The present invention proposes a normally-off semiconductor device. Part of the channel layer 103 structure does not form 2DEG to achieve the normally-off state of the device. The normally-off semiconductor device of the present invention has a simple structure, good conductivity, and high carrier mobility. In addition, multiple insulating layers can be included near the gate to further improve the voltage resistance of the device.
[0064] The invention also provides a method for preparing a semiconductor device. Figure 2A-2V This is a flow chart of a method for preparing a semiconductor device according to an embodiment of the present invention. As shown in the figure, the method includes:
[0065] Figure 2A-2V This is a flow chart of preparing a semiconductor device according to an embodiment of the present invention, as shown in the figure.
[0066] In step 11, a substrate 201 is provided. Figure 2A In this embodiment, a device fabricated on a Si substrate is taken as an example. As those skilled in the art will appreciate, other substrates such as intrinsic GaN, Al2O3 (sapphire), SiC, etc., can also realize similar structures.
[0067] In step 22, a nitride epitaxial layer 202 is formed on the substrate 201, such as Figure 2B In some embodiments, the material of the nitride epitaxial layer 202 may be one or more of AlN, GaN, AlGaN, InGaN, AlInN and AlGaInN.
[0068] In step 23, a first channel layer 203 is formed on the nitride epitaxial layer 202, such as Figure 2C shown.
[0069] In step 24, if Figure 2D As shown, a gate insulating layer 221 is formed on the first channel layer 203. The gate insulating layer 221 is formed on the first channel layer 203 by epitaxial growth.
[0070] In step 25, a sacrificial layer 241 is formed on the gate insulating layer 221. Figure 2E The sacrificial layer 241 may be made of a material that can be selectively etched with the gate insulating layer 221, such as silicon oxide.
[0071] In step 26, the sacrificial layer 241 is patterned, such as Figure 2F In some embodiments, the sacrificial layer 241 may be covered with a photoresist 242 and the sacrificial layer 241 may be selectively etched by photolithography.
[0072] In step 27, the gate insulating layer 221 and a portion of the first channel layer 203 are etched. Figure 2G As shown. The gate insulating layer 221 and a portion of the first channel layer 203 are etched to form a structure as shown, wherein the first channel layer 203 includes a high platform structure. In some embodiments, the first channel layer 203 may not be removed. For example, the height of the gate insulating layer 221 may be appropriately increased to form a similar structure, which also has the advantages described in the present application.
[0073] In step 28, a second channel layer is formed, such as Figure 2H As shown, on the channel layer 203, channel layers 204 are formed on both sides of the high platform structure. The second channel layer is unintentionally doped or N-type doped.
[0074] In step 29, a second barrier layer is formed, such as Fig.2IA second barrier layer 208 is formed on the second channel layer 204 by epitaxial growth.
[0075] Fundamentally, the most critical thing is to form a channel. The channel is generated at the interface of a nitride semiconductor with a narrower bandgap width / a nitride semiconductor with a wider bandgap width, and is located in the channel layer with a lower bandgap width and close to the interface of the channel layer / barrier layer, forming a 2DEG.
[0076] In step 30, the sacrificial layer is removed, such as Figure 2J The sacrificial layer 241 is removed by selective etching.
[0077] In step 31, electrodes are formed on the barrier layer. In some embodiments, a source electrode, a drain electrode, a gate electrode, and a body electrode are formed on the gate insulating layer or the second barrier layer to form a similar Figure 1A The structure shown in FIG. The source electrode and the drain electrode are electrically connected to the 2DEG 207 respectively, and the gate electrode is located between the source electrode and the drain electrode and above the gate insulating layer. In some embodiments, the body electrode is not necessary. The arrangement of the electrodes in the present application is not limited thereto.
[0078] In some embodiments, the method further comprises after step 23:
[0079] In step 32, a first barrier layer 205, a gate insulating layer 233 and a sacrificial layer 241 are formed on the first channel layer 203. Figure 2K A gate insulating layer 233 and a sacrificial layer 241 are formed on the first barrier layer 205 in sequence.
[0080] In step 33, the sacrificial layer 241 is patterned, such as Figure 2L In some embodiments, the sacrificial layer 241 may be covered with a photoresist 242 and the sacrificial layer 241 may be selectively etched by photolithography.
[0081] In step 34, an insulating separation layer 232 is formed, such as Figure 2M In some embodiments, in addition to forming the insulating separation layer 232 on the sidewall of the sacrificial layer 241 , the insulating separation layer 232 may also be formed at other places.
[0082] In step 35, the insulating spacer layer, the gate insulating layer, the first barrier layer and a portion of the channel layer are etched. Figure 2N As shown, the sacrificial layer is used as a mask and anisotropic etching is performed to remove a portion of the insulating separation layer 232, the gate insulating layer 233, the first barrier layer 205 and a portion of the channel layer 203. A portion of the insulating separation layer 222 is retained, wherein the channel layer 203 includes a high platform structure.
[0083] In step 36, a second channel layer and a second barrier layer are formed, such as Fig.2OAs shown, on the first channel layer 203, a second channel layer 204 is formed on both sides of the high-mountain structure. On the second channel layer 204, a second barrier layer 208 is formed by epitaxial growth.
[0084] In step 37, an insulating layer 223 is formed, such as Figure 2P An insulating layer 223 is formed on the second barrier layer and the sacrificial layer.
[0085] In step 38, the insulating layer is etched, such as Figure 2Q The second insulating layer 223 is planarized by etching or other processes to form insulating layers 224 located on both sides of the insulating separation layer 222 and expose the sacrificial layer 241 .
[0086] In step 39, the sacrificial layer is removed, such as Figure 2R The sacrificial layer 241 is removed by selective etching.
[0087] Subsequently, the corresponding electrodes can be formed as described above to form a similar Figure 1B Device with the structure shown.
[0088] In some embodiments, during the etching process, the channel layer 203 may not be etched, but the channel layer 203 may be completely retained. Figure 2S shown.
[0089] Then, a second channel layer 204 and a second barrier layer 208 are formed. Figure 2T shown.
[0090] Similarly, for Figure 1B It is also possible not to etch the channel layer 203, but to completely retain the channel layer 203, such as Figure 2U shown.
[0091] Then, a second channel layer 204 and a second barrier layer 208 are formed. Figure 2V shown.
[0092] In some embodiments, a first barrier layer may be further formed on the first channel layer, wherein the thickness of the first barrier layer is such that the heterojunction between the first channel layer and the first barrier layer does not form a two-dimensional electron gas 2DEG when no external voltage is applied. When the sacrificial layer is patterned, the first barrier layer is patterned.
[0093] Figure 3 A schematic diagram of a semiconductor device structure according to an embodiment of the present invention. Part of the structure is similar to Figure 1A The structure shown is similar and will not be described again here. Figure 3In the structure, a third barrier layer 106 is formed on the substrate, and the material of the third barrier layer 106 can be similar to that of the first barrier layer and the second barrier layer. The third barrier layer 106 has a larger bandgap than the channel layer 103, and even a 2DHG 109 can be formed at the interface between the two.
[0094] The body electrode 117 is located on a side close to the source electrode 111. According to one embodiment of the present invention, the body electrode 117 is electrically connected to the heterojunction formed by the channel layer 103 and the nitride epitaxial layer 102. According to one embodiment of the present invention, the arrangement of the electrodes is not limited to that shown in the figure, as long as the above relationship is satisfied. According to one embodiment of the present invention, the body electrode 117 has the same potential as the source electrode 111. In some embodiments, the body electrode 117 is close to the source electrode 111 and electrically connected to the source electrode 111.
[0095] In some embodiments, the body electrode can be electrically connected to the 2DHG. In some embodiments, the body electrode is electrically connected to the source electrode. The present application electrically connects the floating 2DHG. In some embodiments, the body electrode and the source electrode are connected together or at the same potential. By electrically connecting the 2DHG, the floating problem of the 2DHG potential is avoided. At the same time, when the device is turned off, since the 2DHG will also respond to the electric field and be depleted, it complements the depleted 2DEG. The electric field distribution can be significantly improved, the excessive concentration of the electric field can be avoided, and the voltage resistance of the device can be effectively improved.
[0096] In some embodiments, a low-doping layer may be formed between the channel layer and the third barrier layer, and the layer may reduce the scattering caused by doping ions on the 2DHG.
[0097] The above embodiments are only used to illustrate the present invention, but not to limit the present invention. Ordinary technicians in the relevant technical field can make various changes and modifications without departing from the scope of the present invention. Therefore, all equivalent technical solutions should also fall within the scope of the present invention.
Claims
1. A semiconductor device, comprising: Channel layer; A second barrier layer, which is located on the channel layer, wherein a two-dimensional electron gas 2DEG is formed in the channel layer near the interface between the channel layer and the second barrier layer; source electrode; Drain electrode; as well as a gate electrode located above the channel layer; There is no first barrier layer between the gate electrode and the channel layer, or the thickness of the first barrier layer between the gate electrode and the channel layer is such that a two-dimensional electron gas 2DEG is not formed at the heterojunction between the channel layer and the first barrier layer in the absence of an external voltage; The channel layer includes a first channel layer at least partially located under the gate electrode and a second channel layer under the second barrier layer.
2. The semiconductor device according to claim 2, wherein: there is a height difference between the first channel layer and the second channel layer, and the height difference is not greater than 100 nm; or not greater than 80 nm, or not greater than 50 nm, or not greater than 30 nm. 3 . The semiconductor device according to claim 2 , wherein the height difference is greater than 5 nm, or greater than 10 nm, or greater than 15 nm, or 20 nm. 4 . The semiconductor device according to claim 2 , wherein the second channel layer is located on at least a portion of the first channel layer, and the second channel layer is unintentionally doped or N-type doped. The semiconductor device according to claim 1 , wherein a nitride epitaxial layer is included below the channel layer. 6 . The semiconductor device according to claim 6 , wherein the nitride epitaxial layer is a third barrier layer, and a two-dimensional hole gas 2DHG is formed in the channel layer near an interface between the nitride epitaxial layer and the channel layer. The semiconductor device according to claim 6 , wherein a substrate is included below the nitride epitaxial layer. 8 . The semiconductor device according to claim 1 , wherein a gate insulating layer is included between the gate electrode and the channel layer. 9 . The semiconductor device according to claim 9 , wherein the gate electrode and the gate insulating layer are aligned by self-alignment. 10 . The semiconductor device according to claim 1 , further comprising one or more insulating spacer layers located on sides of the gate electrode. The semiconductor device according to claim 1 , wherein an insulating layer is disposed above the second barrier layer. 12 . The semiconductor device according to claim 7 , further comprising a body electrode electrically connected to a 2DHG formed by a heterojunction of the channel layer and the third barrier layer.
13. A method for preparing a semiconductor device, comprising: forming a first channel layer; forming a sacrificial layer over the first channel layer; patterning the sacrificial layer, wherein the first channel layer is partially removed when patterning the sacrificial layer; forming a second channel layer and a second barrier layer located above the second channel layer, wherein a two-dimensional electron gas 2DEG is formed in the second channel layer near an interface between the second channel layer and the second barrier layer; removing the sacrificial layer and forming a gate electrode over the first channel layer, wherein there is no first barrier layer between the gate electrode and the channel layer; and A source electrode and a drain electrode are formed on both sides of the gate electrode.
14. The method according to claim 13, further comprising forming a gate insulating layer on the first channel layer; wherein When the sacrificial layer is patterned, the gate insulating layer is patterned.
15. The method according to claim 13, wherein: When the sacrificial layer is patterned, the first channel layer is not removed. The method of claim 15 , wherein the second channel layer is unintentionally doped or N-type doped.
17. The method according to claim 13, further comprising: A nitride epitaxial layer is formed on a substrate, wherein the first channel layer is on the nitride epitaxial layer.
18. The method according to claim 17, wherein: The nitride epitaxial layer includes a third barrier layer, and the first channel layer is formed on the third barrier layer.
19. The method according to claim 18, further comprising: A body electrode is formed, which is electrically connected to the 2DHG formed by the heterojunction of the first channel layer and the third barrier layer.
20. The method of claim 13, further comprising: An insulating separation layer is formed on the patterned sacrificial layer, wherein the insulating separation layer is at least located on a sidewall of the sacrificial layer.
21. The method of claim 18, further comprising: After forming the second channel layer and the second barrier layer, forming an insulating layer; and planarizing the second insulating layer and exposing the sacrificial layer. 22 . The method according to claim 13 , wherein the gate electrode occupies a position of the sacrificial layer to achieve self-alignment with the first barrier layer.
23. The method of claim 13, further comprising: A first barrier layer is formed on the first channel layer, wherein the thickness of the first barrier layer is such that a two-dimensional electron gas 2DEG is not formed at the heterojunction between the first channel layer and the first barrier layer in the absence of an external voltage; wherein the first barrier layer is patterned when the sacrificial layer is patterned.