Positive electrode lithium supplementing material Li2NiO2, and preparation method and application of positive electrode lithium supplementing material Li2NiO2
Lithium-nickel microspheres are generated through spray drying technology to achieve close contact between the lithium source and the nickel source, solving the problem of poor contact between the lithium source and the nickel source in the existing technology, and improving the sintering of the lithium-ion battery cathode lithium supplement material Li2NiO2 efficiency and battery energy density.
Patent Information
- Application Number
- CN202410721790.6
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Filing Date
- 2024-06-05
- Publication Date
- 2024-10-01
AI Technical Summary
In the existing technology, the contact effect between the lithium source and the nickel source is not good during the synthesis process of the lithium supplement material Li2NiO2 for the positive electrode of the lithium-ion battery, resulting in high energy consumption, complex process and low sintering efficiency, which cannot effectively improve the battery energy density.
Spray drying technology is used to form a slurry or solution of the lithium source and the nickel source in the dispersant. Microscopic pellets are generated in an inert atmosphere through a spray dryer. They are roasted once to increase the contact density of the lithium nickel precursor, and then dried at high temperature. Further roasting is performed to obtain high-purity Li2NiO2.
It simplifies the process flow, improves the contact effect and sintering efficiency of the lithium-nickel source, reduces energy consumption, has a wide range of applications, and improves the energy density of lithium-ion batteries.
Smart Images

Figure CN118738293A_ABST
Abstract
Description
Technical Field
[0001] The invention relates to a positive electrode lithium supplement material Li2NiO2, a preparation method of the positive electrode lithium supplement material Li2NiO2 and application thereof, and belongs to the technical field of lithium ion batteries. Background Art
[0002] In recent years, with the rapid development of new energy vehicles, portable electronic products, energy storage and other industries, higher requirements have been put forward for the various performances of lithium-ion batteries, especially in terms of battery energy density. During the formation process of lithium-ion batteries, the growth of SEI on the negative electrode surface consumes active lithium, resulting in battery energy loss. However, this can be compensated for by lithium replenishment technology to increase the energy density of the battery. Li2NiO2 is one of the currently commercialized positive electrode lithium replenishers, which has the characteristics of low lithium ion release voltage and good conductivity, and has broad application prospects. Unlike the positive electrode material LiNiO2, Li2NiO2 is calcined under an inert atmosphere, does not react with oxygen, and is a complete solid-phase reaction system, so the microscopic particle contact requirements of the lithium source and nickel source in the solid raw materials are extremely high.
[0003] In the existing technology, the contact between the lithium source and the nickel source is generally promoted by means of solvent ball milling, tablet pressing and mixing. Typical documents include the invention patent application with publication number CN110218078A, entitled "A lithium supplement material Li2NiO2 and a preparation method and application thereof". It not only has high energy consumption, but also has a long process flow. The contact effect between the lithium source and the nickel source is also average. The process is usually not enough to mix once. After sintering, it is necessary to repeatedly mix and roast again, so that the unreacted lithium source and the nickel source increase the contact probability during multiple densification processes. For example, the invention patent application with publication number CN108735526A, entitled "A preparation method of lithium supplement material LiNiO", and a lithium ion capacitor using the LiNiO, and the invention patent application with publication number CN115064698A, entitled "A positive electrode lithium supplement agent and a preparation method thereof" all have similar defects.
[0004] The synthesis of Li2NiO2 requires lithium and nickel sources, and the gas does not participate in the reaction, which is a pure solid-solid phase reaction. In order to increase the contact between the two, the existing technology has reduced the particle size of the two by ball milling, increased the tap density, and increased the contact of solid particles; there is also a method of tableting to reduce the microscopic distance between the two; but no matter which method is used, the effect of a single roasting is usually average, and repeated roasting and mixing are required to enhance the purity of the sintered product. Summary of the invention
[0005] The technical problem to be solved by the present invention is to provide a positive electrode lithium replenishing material Li2NiO2 with a simple process, good mixing effect, high sintering efficiency and a wide range of raw materials, a preparation method of the positive electrode lithium replenishing material Li2NiO2 and its application.
[0006] In order to solve the above technical problems, the preparation method of the positive electrode lithium supplement material Li2NiO2 of the present invention comprises the following specific steps:
[0007] S1. Put the nickel source and the lithium source into a dispersant to dissolve into a solution or form a suspension, and the Li / Ni molar ratio ranges from 1.95 to 2.2;
[0008] S2, pumping the dispersed lithium-nickel mixed precursor into a spray dryer through a pump, spraying the balls under an inert atmosphere to obtain lithium-nickel mixed precursor microspheres;
[0009] S3, heating the prepared microspheres to 300-470°C under an inert atmosphere for 1-24 hours;
[0010] S4. Continue to raise the temperature to 540-800°C, continue calcining for 1-24 hours, crush, screen and remove iron from the sintered material after cooling to obtain the positive electrode lithium supplement material Li2NiO2.
[0011] The lithium source in step S1 includes lithium hydroxide, lithium hydroxide monohydrate, lithium carbonate, and lithium oxide.
[0012] The nickel source in step S1 includes, but is not limited to, nickelous oxide, nickelous hydroxide, nickelous carbonate, nickelous oxalate, nickelous nitrate, nickelous sulfate, and nickelous acetate.
[0013] The dispersant in step S1 is ethanol or water.
[0014] The spray drying temperature of the spray dryer in step S2 is 200-300° C., the inert atmosphere is selected from N2, Ar or He, wherein the oxygen impurity concentration in the gas is less than 10 ppm; and the nozzle operation frequency of the spray dryer is 10-40 Hz.
[0015] The preferred range of temperature in step S3 is 370-450° C., and the preferred range of calcination time is 4-12 hours.
[0016] The preferred range of temperature in step S4 is 590-700° C., and the preferred range of calcination time is 4-12 hours.
[0017] A lithium supplement material Li2NiO2, characterized in that it is prepared by the preparation method described in any one of claims 1-7.
[0018] An application of lithium supplement material Li2NiO2, characterized in that: the lithium supplement material Li2NiO2 in claim 8 is used to prepare a lithium ion battery.
[0019] The advantages of the present invention are:
[0020] The mixed precursor of nickel source and lithium source is prepared by spray drying, and the process is simple, especially the wet mixing method of spray drying. The nickel source and lithium source are formed into closely contacted microscopic balls in the process of spraying balls, and the mixing effect is good. Each ball is an independent roasting unit. The lithium-nickel precursor mixed microspheres can be roasted once to obtain a high-purity Li2NiO2 product, and the sintering efficiency is improved. The range of applicable raw materials of nickel source and lithium source is also wide. BRIEF DESCRIPTION OF THE DRAWINGS
[0021] Figure 1 This is a SEM picture of the lithium nickel precursor after spray drying and mixing of the present invention;
[0022] Figure 2 This is an electrochemical performance evaluation diagram of the sample of Application Example 1 of the present invention after being prepared into a button-type battery. DETAILED DESCRIPTION
[0023] The positive electrode lithium supplement material Li2NiO2, the preparation method of the positive electrode lithium supplement material Li2NiO2 and the application thereof of the present invention are further described in detail below in conjunction with the accompanying drawings and specific embodiments.
[0024] Embodiment 1:
[0025] As for the preparation of positive electrode lithium supplement material Li2NiO2, after the inventors' hard work and attempts, we unexpectedly found that after dispersing lithium salt and nickel salt in a dispersant, whether it is a mixed solution or a suspension, after spray drying, microscopic small balls of lithium-nickel mixed materials can be obtained, and the mixing effect is good. Li2NiO2 with low nickel oxide residue can be obtained by direct roasting. If the lithium source used is lithium hydroxide or lithium hydroxide monohydrate, direct roasting at high temperature will form molten salt, causing Li to agglomerate and migrate, affecting the sintering result. Roasting at low temperature for a period of time can convert most of the raw materials below the melting point of the lithium salt, and the remaining lithium salt will not agglomerate and migrate when sintered at high temperature, and the purity of Li2NiO2 will be improved.
[0026] The preparation method of the positive electrode lithium supplement material Li2NiO2 of the present invention comprises the following specific steps:
[0027] S1, putting the nickel source and the lithium source into a dispersant to dissolve into a solution or form a suspension, the Li / Ni molar ratio range is 1.95-2.2, wherein the lithium source can be lithium hydroxide, lithium hydroxide monohydrate, lithium carbonate, lithium oxide, etc., the nickel source includes but is not limited to nickelous oxide, nickelous hydroxide, nickelous carbonate, nickelous oxalate, nickelous nitrate, nickelous sulfate, nickelous acetate, etc., and the dispersant can be ethanol or water, preferably water;
[0028] S2. The dispersed lithium-nickel mixed precursor is pumped into the feed port of a spray dryer, and sprayed under an inert atmosphere to obtain lithium-nickel mixed precursor microspheres; wherein the spray drying temperature of the spray dryer is 200-300°C, and the inert atmosphere is selected from N2, Ar or He, wherein the oxygen impurity concentration is less than 10ppm (oxygen is a gas impurity, and the oxygen impurity concentration in nitrogen, argon and helium cannot be too high); the nozzle operation frequency of the spray dryer is 10-40Hz.
[0029] S3. The prepared microspheres are heated to 300-470° C. under an inert atmosphere and kept warm for 1-24 hours. The preferred temperature range is 370-450° C. and the preferred calcination time range is 4-12 hours.
[0030] S4, continue to heat up to 540 ~ 800 ℃, continue to roast for 1 ~ 24h, and crush, screen and remove iron from the sintered material after cooling to room temperature to obtain the positive electrode lithium supplement material Li2NiO 2, The preferred temperature range is 590-700° C., and the preferred calcination time range is 4-12 hours.
[0031] Wherein, step S1 and step S2 are methods for preparing a precursor by mixing a lithium source and a nickel source, and step S3 and step S4 are methods for applying the precursor to LNO sintering; Example 2:
[0032] The lithium supplement material Li2NiO2 of this embodiment is prepared by the preparation method of the first embodiment.
[0033] Embodiment three:
[0034] The lithium supplement material Li2NiO2 obtained in the above example is used to prepare a lithium ion battery.
[0035] The effects of the present invention are verified below in combination with application examples and comparative examples:
[0036] Application Example 1:
[0037] Dissolve lithium hydroxide in water to prepare a 12wt% solution, weigh nickelous oxide solid according to the Li / Ni molar ratio of 2, add it into the solution and beat it into a suspension, use a peristaltic pump to pump it into the nozzle inlet of the spray drying equipment, and use nitrogen as the blast atmosphere for spray drying, the temperature is 250℃, the nozzle frequency is 30Hz, and the mixed and dried precursor beads are obtained at the bottom of the spray dryer. The mixed precursor microspheres are placed in an alumina crucible, baked in a nitrogen atmosphere at 450℃ for 2h, then heated to 650℃ and baked for 4h. The solid after cooling is crushed, screened, and iron removed to obtain the positive electrode lithium supplement material Li2NiO2. Application Example 2:
[0038] Lithium hydroxide is dissolved in water to form a 10wt% solution. Nickelous nitrate solid is weighed according to the Li / Ni molar ratio of 2, and dissolved in the solution to obtain a mixed solution. The mixed solution is pumped into the nozzle inlet of the spray drying equipment using a metering pump. The spray drying blast atmosphere uses nitrogen, the temperature is 300°C, and the nozzle frequency is 10Hz. The mixed and dried precursor microspheres are obtained at the bottom of the spray dryer. The mixed precursor microspheres are placed in an alumina crucible and roasted in a nitrogen atmosphere at 420°C for 8h, then heated to 700°C and roasted for 6h. The solid after cooling is crushed, screened, and iron removed to obtain the positive electrode lithium supplement material Li2NiO2.
[0039] Application Example 3:
[0040] Lithium oxide was dissolved in ethanol to prepare a 2wt% solution. Nickel hydroxide solid was weighed according to a Li / Ni molar ratio of 2.2, and then added to the solution to form a suspension. A peristaltic pump was used to pump the suspension into the nozzle inlet of the spray drying equipment. The spray drying blast atmosphere used nitrogen, the temperature was 300°C, and the nozzle frequency was 30Hz. The mixed and dried precursor microspheres were obtained at the bottom of the spray dryer. The mixed precursor microspheres were placed in an alumina crucible and calcined in a nitrogen atmosphere at 450°C for 12h, then heated to 800°C and calcined for 12h. The solid after cooling was crushed, screened, and iron removed to obtain the positive electrode lithium supplement material Li2NiO2.
[0041] Comparative Example 1:
[0042] Lithium hydroxide and nickelous oxide were mixed at a Li / Ni molar ratio of 2, ball-milled for 24 hours, then transferred into a crucible, calcined at 450°C for 8 hours under nitrogen protection, then heated to 800°C and calcined for 24 hours. The solid after cooling was crushed, screened, and iron removed to obtain the positive electrode lithium supplement material Li2NiO2.
[0043] The material quality data obtained from the above application examples 1-3 and the comparative example are summarized in the following table
[0044] Case Residual NiO Example 1 5.9 Example 2 6.3 Example 3 7.1 Comparative Example 1 19.1
[0045] From the above comparison, it can be seen that the method provided by the present invention is simple, and lithium-nickel mixed precursor pellets are prepared by spray drying, and high-purity Li2NiO2 can be obtained by direct calcination. Usually, the NiO residue can be less than 8%, and the first charging capacity can be greater than 400mAh / g.
[0046] Of course, the above description is not a limitation of the present invention, and the present invention is not limited to the above examples. Changes, modifications, additions or substitutions made by technicians in this technical field within the essential scope of the present invention should also fall within the protection scope of the present invention.
Claims
1. A method for preparing a positive electrode lithium supplement material Li2NiO2, characterized in that: The specific steps are as follows: S1. Put the nickel source and the lithium source into a dispersant to dissolve into a solution or form a suspension, and the Li / Ni molar ratio ranges from 1.95 to 2.2; S2, pumping the dispersed lithium-nickel mixed precursor into a spray dryer through a pump, spraying the balls under an inert atmosphere to obtain lithium-nickel mixed precursor microspheres; S3, heating the prepared microspheres to 300-470°C under an inert atmosphere for 1-24 hours; S4. Continue to raise the temperature to 540-800°C, continue calcining for 1-24 hours, crush, screen and remove iron from the sintered material after cooling to obtain the positive electrode lithium supplement material Li2NiO2.
2. The method for preparing the positive electrode lithium supplement material Li2NiO2 according to claim 1, characterized in that: The lithium source in step S1 includes lithium hydroxide, lithium hydroxide monohydrate, lithium carbonate, and lithium oxide.
3. The method for preparing the positive electrode lithium supplement material Li2NiO2 according to claim 1, characterized in that: The nickel source in step S1 includes, but is not limited to, nickelous oxide, nickelous hydroxide, nickelous carbonate, nickelous oxalate, nickelous nitrate, nickelous sulfate, and nickelous acetate.
4. The method for preparing the positive electrode lithium supplement material Li2NiO2 according to claim 1, characterized in that: The dispersant in step S1 is ethanol or water.
5. The method for preparing the positive electrode lithium supplement material Li2NiO2 according to claim 1, characterized in that: The spray drying temperature of the spray dryer in step S2 is 200-300° C., the inert atmosphere is selected from N2, Ar or He, wherein the oxygen impurity concentration in the gas is less than 10 ppm; and the nozzle operation frequency of the spray dryer is 10-40 Hz.
6. The method for preparing the positive electrode lithium supplement material Li2NiO2 according to claim 1, characterized in that: The preferred range of temperature in step S3 is 370-450° C., and the preferred range of calcination time is 4-12 hours.
7. The method for preparing the positive electrode lithium supplement material Li2NiO2 according to claim 1, characterized in that: The preferred range of temperature in step S4 is 590-700° C., and the preferred range of calcination time is 4-12 hours.
8. A lithium supplement material Li2NiO2, characterized in that: The compound is prepared by the preparation method according to any one of claims 1 to 7.
9. An application of lithium supplement material Li2NiO2, characterized in that: The lithium supplement material Li2NiO2 in claim 8 is used to prepare lithium ion batteries.
Citation Information
Patent Citations
Method for preparing lithium-replenishing material Li2NiO2, and lithium ion capacitor using Li2NiO2
CN108735526A
Lithium-supplementing material Li2NiO2 as well as preparation method and application thereof
CN110218078A
Positive electrode lithium supplement agent and preparation method thereof
CN115064698A
Cited By
Positive lithium supplement agent, preparation method thereof and positive plate
CN122417892A