Silicon-based composite material with stable structure, preparation method of silicon-based composite material and lithium ion battery

By using porous materials and silicon-based composite materials with a core-shell structure in lithium-ion battery anode materials, combined with the gradient distribution of magnesium silicate and lithium silicate and a carbon coating layer, the problem of silicon-based materials in lithium-ion batteries is solved. To solve the problems of low first efficiency and poor circulation, high cycle stability and improvement of first Coulombic efficiency have been achieved.

CN118738345APending Publication Date: 2024-10-01NORTHWESTERN POLYTECHNICAL UNIV
View PDF 0 Cites 0 Cited by

Patent Information

Application Number
CN202410953255.3
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Filing Date
2024-07-16
Publication Date
2024-10-01

Smart Images

  • Figure HDA0004947819540000011
    Figure HDA0004947819540000011
  • Figure HDA0004947819540000012
    Figure HDA0004947819540000012
  • Figure HDA0004947819540000013
    Figure HDA0004947819540000013
Patent Text Reader

Abstract

The invention provides a silicon-based composite material with a stable structure, a preparation method of the silicon-based composite material and a lithium ion battery. The silicon-based composite material comprises a porous material and a core-shell material distributed in the porous material, the core-shell material sequentially comprises an inner core, a pre-magnesium layer, a pre-lithium layer and a carbon coating layer from inside to outside, the inner core is a silicon-based material, the pre-magnesium layer sequentially comprises a magnesium silicate area and a magnesium silicate and lithium silicate mixing area from inside to outside, and the pre-lithium layer is lithium silicate; the lithium silicate in the mixing area is in gradient distribution with gradually increased concentration from inside to outside; the magnesium silicate is MgSiO3; the lithium silicate comprises Li2SiO3 and Li2Si2O5, and the lithium silicate comprises Li2SiO3 and According to the invention, the problems of low first effect, poor circulation and poor water resistance of the material caused by volume expansion and self stability of the material structure in the prior art are solved.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The invention belongs to the technical field of lithium ion battery materials, and in particular relates to a silicon-based composite material with a stable structure, a preparation method thereof, and a lithium ion battery. Background Art

[0002] China's new energy electric vehicle market is booming, which is driving power lithium-ion batteries towards high specific energy and high safety. As one of the important components of lithium-ion batteries, the performance of the negative electrode has an important impact on the overall indicators of the battery, requiring the materials used for the negative electrode to have characteristics such as high first efficiency and excellent cycle performance. Among them, silicon-based materials have attracted the attention of researchers around the world in recent years due to their abundant natural resources, extremely high theoretical specific capacity and suitable redox potential. However, some potential problems still restrict the commercial application of silicon-based materials, especially the capacity loss caused by irreversible lithium insertion products, poor conductivity and huge volume effect, which makes it estimated that the first efficiency, rate performance and cycle stability of the material cannot meet practical needs. Among them, the stability of the negative electrode active material silicon-based material itself is particularly important. Therefore, the slurry of the negative electrode material of lithium-ion batteries needs to have good stability, which is an important indicator to ensure the consistency of the battery during the battery production process.

[0003] The structural stability of silicon-based materials after modification is different to water, which will lead to many problems in the negative electrode aqueous slurry, such as poor material structural stability and water resistance, and the slurry will experience sedimentation, flocculation and other phenomena, which will have a great impact on subsequent coating and other processes. In order to solve the problems of first coulomb efficiency, cycle stability and slurry instability, existing literature has proposed many solutions, among which the technology of improving slurry stability from the perspective of material structural stability is an effective method.

[0004] Chinese patent CN115663151B obtains a pre-magnesium silicon-oxygen composite material through pre-magnesium treatment, including a core and a first coating layer. The core includes SiO x , and 0<x<2. The first coating layer includes nano-silicon and silicon-oxygen magnesium compound, and the silicon-oxygen magnesium compound includes at least MgSiO 3 ,MgSiO 3It accounts for no less than 80% of the mass of the silicon-oxygen magnesium compound. Although the material of this structure effectively changes the cycle performance, the improvement of the first coulomb efficiency is not obvious, and there are also problems such as reduced capacity and unstable slurry. Chinese patent CN117747763A obtains a pre-lithiation silicon-based composite material through a pre-lithiation method. The material of this structure comprises pre-lithiation silicon-based composite particles with a core-shell structure. The core of the pre-lithiation silicon-based composite particles comprises a porous silicon matrix and a core lithium-containing component dispersed on the surface of the silicon matrix and in the pores; the outer surface of the core is sequentially coated with a first carbon layer and a second carbon layer from the inside to the outside, and the first carbon layer and the second carbon layer form an outer shell of the core-shell structure. Although the material of this structure solves the problems of slurry stability and water resistance to a certain extent, its first efficiency is not significantly improved, and the data of cycle stability is uneven. Chinese patent CN116799182A discloses a fluoride-modified coated pre-lithiation pre-magnesium silicon-oxygen composite negative electrode active material, whose chemical formula is Li x Mg y Si z O n / C@MgF 2 . The composite material is a core-shell structure, including an inner core of lithium magnesium silicate / carbon and an outer shell of a metal fluoride fast ion conductor. Although this material improves the first efficiency and improves the stability of the interface in the slurry to a certain extent, its cycle performance is poor. Chinese patent CN111342030B provides a multi-component composite high first efficiency lithium battery negative electrode material, including silicon compound particles and a conductive layer coated on the surface of the silicon compound particles, the negative electrode material also includes lithium silicate and magnesium silicate, which improves the first efficiency, but the cycle performance needs to be improved. Therefore, it is necessary to explore new solutions to solve the problems of stability and water resistance of silicon-based materials themselves. Summary of the invention

[0005] In order to overcome the problems of low initial efficiency, poor circulation, poor material water resistance and slurry coating caused by volume expansion and the stability of the material structure itself in the prior art, the present invention provides a structurally stable silicon-based composite material, a preparation method thereof and a lithium-ion battery.

[0006] The present invention is achieved through the following technical solutions:

[0007] The present invention provides a structurally stable silicon-based composite material, comprising a porous material and a core-shell material distributed in the porous material; the core-shell material comprises a core, a pre-magnesium layer, a pre-lithium layer and a carbon coating layer from the inside to the outside, the core is a silicon-based material, the pre-magnesium layer comprises a magnesium silicate region and a mixed region of magnesium silicate and lithium silicate from the inside to the outside, the pre-lithium layer is lithium silicate; wherein the lithium silicate in the mixed region is distributed in a gradient with a gradually increasing concentration from the inside to the outside; the magnesium silicate is MgSiO 3 ; The lithium silicate includes Li2 SiO 3 and Li 2 Si 2 O 5 .

[0008] Preferably, the chemical formula of the silicon-based material is SiO x , wherein 0<x<2; the porous material is a porous carbon material, a porous ceramic material or a porous nitride.

[0009] The present invention provides a method for preparing the structurally stable silicon-based composite material, comprising:

[0010] S1: mixing the silicon source and the magnesium source evenly, and performing heat treatment under vacuum conditions to obtain a precursor containing a pre-magnesium layer;

[0011] S2: pre-lithiating a precursor containing a pre-magnesium layer to obtain a silicon-based composite material containing a pre-lithium layer;

[0012] S3: performing carbon coating treatment on the silicon-based composite material containing the pre-lithium layer to obtain a silicon-based composite material containing a carbon coating layer;

[0013] S4: mixing the silicon-based composite material containing the carbon coating layer with the porous material, and performing heat treatment to obtain the silicon-based composite material with a stable structure.

[0014] Preferably, in S1, the magnesium source is metallic magnesium powder or magnesium salt, and the mass of the magnesium source accounts for 15% to 80% of the mass of the silicon source.

[0015] Preferably, in S1, the heat treatment temperature is 1000°C to 1400°C, and the insulation time is 1h to 5h.

[0016] Preferably, S2 is specifically: mixing a lithium source, a pre-lithium reagent and an organic solvent to obtain a precursor solution; mixing a precursor containing a pre-magnesium layer with the precursor solution and then performing a sealing reaction, and drying the obtained solid and then calcining it to obtain a silicon-based composite material containing a pre-lithium layer.

[0017] Preferably, the calcination temperature is 500° C. to 1000° C., and the calcination time is 2 h to 12 h.

[0018] Preferably, the lithium source is one of lithium powder, lithium sheet, lithium foil, lithium block, lithium hydride and lithium hydroxide; the pre-lithium reagent is one of naphthalene, 1-methylnaphthalene, 3,3'-dimethylbiphenyl, 4,4'-dimethylbiphenyl and 3,3',4,4'-tetramethylbiphenyl.

[0019] Preferably, in S4, the heat treatment temperature is 650°C to 950°C, and the insulation time is 3h to 10h.

[0020] The present invention provides a lithium ion battery, comprising the structurally stable silicon-based composite material according to any one of claims 1 to 2 as a negative electrode material.

[0021] Compared with the prior art, the present invention has the following beneficial effects:

[0022] The silicon-based composite material of the present invention comprises a porous material and a core-shell material distributed in the porous material; the core-shell material comprises a core, a pre-magnesium layer, a pre-lithium layer and a carbon coating layer in sequence from the inside to the outside, the pre-magnesium layer comprises a magnesium silicate region and a mixed region of magnesium silicate and lithium silicate in sequence from the inside to the outside, and the pre-lithium layer is lithium silicate. 3 The existence of phases and the Li 2 Si 2 O 5 The existence of the phase can ensure that the structure has a certain stability, and Li 2 Si 2 O 5 It has good water resistance and can improve the stability of silicon-based composite material slurry, thereby improving the cycle stability of the material. 3 and Li 2 SiO 3 The presence of phases can improve the first cycle efficiency. The presence of two lithium silicates in the mixed zone, due to the difference in particle size, the relatively small particle size of magnesium silicate makes it easier to fill the gaps generated by the delithiation process. The presence of carbon coating and porous materials gives the material a good tolerance to volume expansion and prevents particle pulverization caused by expansion. In addition, porous materials have certain mechanical strength and toughness, which can resist the stress during charging and discharging, effectively maintain the structural stability of the negative electrode material, and achieve rapid lithium ion transmission.

[0023] The preparation method of the silicon-based composite material of the present invention sequentially performs pre-magnesium, pre-lithium, carbon coating, and composite porous material to obtain a core-shell material loaded on the porous material; the core-shell material sequentially includes a core, a pre-magnesium layer, a pre-lithium layer, and a carbon coating layer from the inside to the outside, the pre-magnesium layer sequentially includes a magnesium silicate region and a mixed region of magnesium silicate and lithium silicate from the inside to the outside, and the pre-lithium layer is lithium silicate. The silicon-based composite material of the structure obtained by the method of the present invention has the characteristics of good water resistance, high first efficiency, and good cycle stability. BRIEF DESCRIPTION OF THE DRAWINGS

[0024] In order to more clearly illustrate the embodiments of the present invention or the technical solutions in the prior art, the drawings required for use in the embodiments or the description of the prior art will be briefly introduced below. Obviously, the drawings described below are some embodiments of the present invention. For ordinary technicians in this field, other drawings can be obtained based on these drawings without paying creative work.

[0025] Figure 1 Schematic diagram of the structure of the silicon-based composite material with stable structure of the present invention;

[0026] Figure 2 is the XRD diagram of Example 1 of the present invention;

[0027] Figure 3 This is the XRD diagram of Comparative Example 2 of the present invention. DETAILED DESCRIPTION

[0028] The following describes the embodiments of the present invention through specific examples, and those skilled in the art can easily understand other advantages and effects of the present invention from the contents disclosed in this specification. The present invention can also be implemented or applied through other different specific embodiments, and the details in this specification can also be modified or changed in various ways based on different viewpoints and applications without departing from the spirit of the present invention.

[0029] It should be noted that the process equipment or devices not specifically specified in the following embodiments are all conventional equipment or devices in the art.

[0030] It should be noted that the terms "include" and "have" and any variations thereof are intended to cover non-exclusive inclusions. For example, a process, method, system, product or device that includes a series of steps or units is not necessarily limited to those steps or units clearly listed, but may include other steps or units that are not clearly listed or inherent to these processes, methods, products or devices. Moreover, unless otherwise specified, the numbering of each method step is only a convenient tool for identifying each method step, and is not intended to limit the order of arrangement of each method step or to define the scope of the present invention. Changes or adjustments in their relative relationships should also be regarded as the scope of the present invention without substantially changing the technical content.

[0031] like Figure 1 The structurally stable silicon-based composite material provided by the present invention is shown,

[0032] The invention comprises a porous material and a core-shell material distributed in the porous material; the core-shell material comprises a core, a pre-magnesium layer, a pre-lithium layer and a carbon coating layer from the inside to the outside, the core is a silicon-based material, the pre-magnesium layer comprises a magnesium silicate region and a mixed region of magnesium silicate and lithium silicate from the inside to the outside, and the pre-lithium layer is lithium silicate; wherein the lithium silicate in the mixed region is distributed in a gradient with a gradually increasing concentration from the inside to the outside; the magnesium silicate is MgSiO 3 ; The lithium silicate includes Li 2 SiO 3 and Li 2 Si 2 O 5 .

[0033] In a specific embodiment of the present invention, the chemical formula of the silicon-based material is SiO x , where the value range of x is 0 < x < 2, preferably 0 < x ≤ 1.5.

[0034] In a specific embodiment of the present invention, the thickness of the carbon coating layer is 100 nm to 250 nm.

[0035] In a specific embodiment of the present invention, the porous material is a porous carbon material, a porous ceramic material or a porous nitride, and the pore size range is 0.5 μm to 100 μm.

[0036] The preparation method of the silicon-based composite material with stable structure according to the present invention includes the following steps:

[0037] S1: Mix a certain amount of silicon source and magnesium source evenly, add them into a vacuum reaction chamber for heat treatment, after heat preservation, cooling, grinding and sieving, a precursor containing a pre-magnesium layer is obtained;

[0038] S2: Pre-lithiate the precursor containing the pre-magnesium layer in S1 to obtain a silicon-based composite material containing a pre-lithium layer;

[0039] S3: Perform carbon coating treatment on the silicon-based composite material containing the pre-lithium layer in S2 to obtain a silicon-based composite material containing a carbon coating layer;

[0040] S4: Uniformly disperse the silicon-based composite material containing the carbon coating layer in S3 in a porous material, perform high-temperature heat treatment, and after discharging, perform crushing and sieving to obtain the silicon-based composite material with stable structure.

[0041] In a specific embodiment of the present invention, the silicon source is SiO x , where 0 < x < 2, preferably 0 < x ≤ 1.5.

[0042] In a specific embodiment of the present invention, the magnesium source is metallic magnesium powder or magnesium salt, and the mass of the magnesium source accounts for 15% to 80% of the mass of the silicon source.

[0043] In a specific embodiment of the present invention, the heat treatment temperature in S1 is 1000 °C to 1400 °C, and the heat preservation time is 1 h to 5 h.

[0044] In a specific embodiment of the present invention, the cooling temperature in S1 is room temperature, the grinding is mechanical grinding, and the particle size range obtained by sieving is 0.1 μm to 30 μm.

[0045] In a specific embodiment of the present invention, the pre-lithiation treatment described in S2 is liquid phase pre-lithiation, and the steps are: mixing a lithium source, a pre-lithiation reagent and an organic solvent to obtain a precursor solution; mixing a precursor containing a pre-magnesium layer therewith, conducting a sealed reaction, separating, filtering, drying and then transferring to a tubular furnace for calcination, wherein the calcination temperature is 500°C to 1000°C, preferably 650°C to 850°C, and the calcination time is 2h to 12h, preferably 4h to 8h.

[0046] In a specific embodiment of the present invention, the lithium element in the lithium source accounts for 1.5% to 28% of the mass of the silicon-based composite material containing the carbon coating layer, preferably 6 to 15%; the molar ratio of the lithium source to the pre-lithium reagent is (1 to 30):1, preferably (5 to 20):1.

[0047] In a specific embodiment of the present invention, the lithium source comprises one of lithium powder, lithium sheet, lithium foil, lithium block, lithium hydride and lithium hydroxide. The pre-lithium reagent is one of aromatic compounds and their derivatives, preferably one of naphthalene, 1-methylnaphthalene, 3,3'-dimethylbiphenyl, 4,4'-dimethylbiphenyl and 3,3',4,4'-tetramethylbiphenyl. The organic solvent is an ether organic solvent.

[0048] In a specific embodiment of the present invention, the carbon coating described in S3 is conventional carbon coating, including one of gas phase, solid phase and liquid phase coating.

[0049] In a specific embodiment of the present invention, the mixing method described in S4 includes liquid phase mixing or solid phase mixing; wherein the solvent in the liquid phase mixing is isopropanol or ethanol, and the solid phase mixing is ball milling, and the ball milling time is 2h to 15h, preferably 4h to 10h; the high temperature treatment temperature is 650°C to 950°C, and the insulation time is 3h to 10h.

[0050] The structurally stable silicon-based composite material of the present invention can be used as a negative electrode material to assemble a lithium-ion battery, and the lithium-ion battery assembled with the silicon-based composite material as the negative electrode material has both excellent first coulombic efficiency and high cycle stability.

[0051] Example 1

[0052] (1) SiO x The powder and the metal magnesium powder are mixed evenly in a mass ratio of 5:2 and added into a vacuum furnace, heated to 1100°C, and kept warm for 1 hour. After the steam is condensed, a precursor containing a pre-magnesium layer is obtained. Then, the precursor particles containing a pre-magnesium layer with a particle size of 1 to 5 μm are obtained after grinding and sieving.

[0053] (2) In a glove box, weigh 0.416 g of 1-methylnaphthalene and 0.203 g of lithium flakes and dissolve them in 35 ml of tetrahydrofuran, stir mechanically, then weigh 7.00 g of the precursor particles containing the pre-magnesium layer in step (1) and add them to the above solution and continue stirring, then cover the bottle mouth and seal it with tape. After heating the reaction system in an oil bath for 5 h, transfer it to a glove box and let it settle for 0.5 h. After multiple washings and vacuum drying, transfer it to a tube furnace and calcine it in an Ar gas atmosphere at a calcination temperature of 700 ° C, a heating rate of 5 ° C / min, and keep it warm for 4 h to obtain a silicon-based composite material containing a pre-lithium layer;

[0054] (3) placing the silicon-based composite material containing the pre-lithium layer in step (2) in a tubular furnace, heating it to 850° C. under an argon atmosphere, introducing argon and methane gas at a volume ratio of 1:1 for gas phase coating, keeping the temperature for 1.5 hours, turning off the organic gas source, cooling it to room temperature and discharging it to obtain a silicon-based composite material containing a carbon coating layer.

[0055] (4) The silicon-based composite material containing the carbon coating layer in step (3) and the porous carbon are uniformly dispersed in isopropanol, and the resulting mixed solution is placed in a high-temperature furnace, heated to 700° C., and kept warm for 4 hours. After the material is discharged, it is crushed and sieved to obtain a silicon-based composite material with a stable structure.

[0056] Figure 2 is the XRD diffraction pattern of the silicon-based composite material with a stable structure obtained in Example 1. It can be seen that Li 2 SiO 3 At 2θ of about 24.6° and 37.5°, Li 2 Si 2 O 5 MgSiO appears at about 30.7°, 35.6°, 43.2° and 65.5° 2θ. 3 The peaks indicate that lithium-containing silicate and magnesium-containing silicate materials were successfully synthesized after pre-lithiation and pre-magnesiation treatments.

[0057] Example 2

[0058] The method of Example 1 is followed except that: the SiO x The powder and the metal magnesium powder are evenly mixed in a mass ratio of 8:5, and the other steps are the same as those in Example 1 to obtain a silicon-based composite material with a stable structure.

[0059] Example 3

[0060] The method of Example 1 is followed except that the magnesium source in step (1) is replaced with magnesium carbonate, SiO xThe powder and magnesium carbonate were uniformly mixed in a mass ratio of 13:10, the heating temperature was changed to 1000° C., the insulation time was changed to 2 h, and the other steps were the same as in Example 1 to obtain a silicon-based composite material with a stable structure.

[0061] Example 4

[0062] The method of Example 1 is followed, except that in step (2), 0.74 g of naphthalene and 0.406 g of lithium flakes are weighed in a glove box and dissolved in 35 ml of tetrahydrofuran. The other steps are the same as those of Example 1 to obtain a structurally stable silicon-based composite material.

[0063] Example 5

[0064] The method of Example 1 is followed, except that the lithium source in step (2) is changed to lithium powder, the calcination temperature is changed to 750° C., and the other steps are the same as those of Example 1, to obtain a silicon-based composite material with a stable structure.

[0065] Example 6

[0066] The method of Example 1 is followed, except that step (3) is changed to: the silicon-based composite material containing the pre-lithium layer described in step (2) and asphalt are dissolved in isopropanol in a mass ratio of 12:3, stirred for 3.5 hours to form a uniform slurry, and then placed in a tubular furnace after drying, heated to 800°C in argon, and kept warm for 2 hours. The other steps are the same as in Example 1, to obtain a silicon-based composite material with a stable structure.

[0067] Example 7

[0068] The method of Example 1 is followed, except that the porous carbon in step (4) is replaced by porous silicon nitride, the heat treatment temperature is changed to 800° C., and the other steps are the same as those of Example 1, to obtain a silicon-based composite material with a stable structure.

[0069] Example 8

[0070] The method of Example 1 is followed, except that step (4) is changed to: placing the silicon-based composite material containing a carbon coating layer in step (3) and porous carbon in a ball mill, and mixing them by ball milling for 5 hours in an argon atmosphere to disperse the material in step (3) in the pores of the porous carbon to obtain a precursor material; then placing it in a tubular furnace, heating it to 650°C in an argon atmosphere, and keeping it warm for 5 hours to perform high-temperature heat treatment to obtain a silicon-based composite material with a stable structure.

[0071] Comparative Example 1

[0072] The method of Example 1 is followed, except that the pre-lithiation in step (2) is not performed, and the other steps are the same as those of Example 1, to obtain a silicon-based composite material without a pre-lithiation layer.

[0073] Comparative Example 2

[0074] The method of Example 1 is followed, except that the pre-magnesium treatment in step (1) is not performed, and the other steps are the same as those of Example 1, to obtain a silicon-based composite material without a pre-magnesium layer.

[0075] Figure 3 This is the XRD diffraction pattern of the material prepared in Example 2. It can be seen that Li 2 SiO 3 At 2θ of about 24.6° and 37.4°, Li 2 Si 2 O 5 peak, indicating that lithium silicate-containing materials were synthesized by pre-lithiation treatment.

[0076] Comparative Example 3

[0077] The method of Example 1 is followed, except that the carbon coating treatment in step (3) is not performed, and the other steps are the same as those of Example 1, to obtain a silicon-based composite material without carbon coating.

[0078] Comparative Example 4

[0079] The method of Example 1 is followed, except that the mixing treatment with porous carbon in step (4) is not performed, and the other steps are the same as those of Example 1, to obtain a silicon-based composite material without an external porous layer.

[0080] Comparative Example 5

[0081] The method of Example 1 is followed, except that the pre-magnesium and pre-lithium treatments in steps (1) and (2) are not performed, and the other steps are the same as those of Example 1, to obtain a silicate-free silicon-based composite material.

[0082] The composite materials obtained in the above-mentioned embodiments and comparative examples were used as negative electrode active materials to assemble button-type batteries.

[0083] Preparation and testing of button half-cells: The silicon-based composite material, SP, and adhesive are weighed in a mass ratio of 80%: 10%: 10%, and the slurry is prepared with a beater, followed by coating, drying, and cutting, and assembled into button half-cells in a glove box. Finally, the test was carried out using a blue electric device, with a discharge cut-off voltage of 0.005V and a charge cut-off voltage of 1.5V. The discharge was carried out at a constant current of 0.1C, 0.05C, and 0.02C to 0.005V, and then charged at a constant current of 0.1C to 1.5V. The above charge and discharge were repeated for two cycles, and the discharge tests after the third cycle were all carried out at a current density of 0.1C. The changes in the first coulomb efficiency and the retention rate after 100 and 200 cycles were measured respectively.

[0084] The battery performance data of the above examples and comparative examples are shown in Table 1 below:

[0085] Table 1 Battery performance data

[0086] Sample performance First coulombic efficiency % 100 cycles capacity retention rate % 200 cycles capacity retention rate % Example 1 91.85 95.3 93.4 Example 2 91.76 93.4 92.7 Example 3 90.12 91.9 90.2 Example 4 92.29 94.5 93.1 Example 5 92.10 94.9 93.3 Example 6 91.70 93.1 90.5 Example 7 89.96 92.8 91.1 Example 8 91.03 92.2 90.8 Comparative Example 1 84.16 93.5 88.3 Comparative Example 2 87.03 92.2 85.9 Comparative Example 3 90.31 93.5 89.6 Comparative Example 4 89.49 91.4 86.7 Comparative Example 5 76.31 88.4 63.2

[0087] As shown in Table 1, the silicon-based composite materials prepared in Examples 1 to 8 of the present invention have a first coulombic efficiency of more than 89%, a 100-cycle capacity retention rate of more than 91%, and a 200-cycle capacity retention rate of more than 90%. It can be seen that the silicon-based composite materials prepared by the present invention have high first coulombic efficiency and cycle stability.

[0088] Comparing Comparative Example 1 without pre-lithiation with Example 1, it can be seen that the first coulombic efficiency and cycle stability of the silicon-based composite material in Comparative Example 1 are lower than those in Example 1. This is because Li 2 Si 2 O 5 It has good water resistance and can improve the stability of silicon-based composite material slurry. 2 SiO 3 The presence of phase can improve the first cycle efficiency.

[0089] Comparing the comparative example 2 without pre-magnesium treatment with the example 1, it can be seen that the first coulombic efficiency and cycle stability of the silicon-based composite material in the comparative example 2 are lower than those in the example 1, especially the cycle stability is significantly reduced. This is because the MgSiO 3 The existence of the phase can ensure that the structure has a certain stability and can also improve the first cycle efficiency.

[0090] Comparing the comparative example 3 without carbon coating with the example 1, it can be seen that the first coulombic efficiency and cycle stability of the silicon-based composite material in the comparative example 3 are lower than those in the example 1. The results show that the presence of the carbon coating makes the material have better stability.

[0091] Comparing the comparative example 4 without composite porous carbon material with the example 1, it can be seen that the first coulombic efficiency and cycle stability of the comparative example 4 are lower than those of the example 1, which indicates that the porous material can improve the structural stability of the material, thereby providing cycle stability.

[0092] Comparative Example 5 was neither pre-magnesiumized nor pre-lithiated. The first coulombic efficiency and cycle stability of the obtained material were significantly lower than those of Example 1, and lower than those of Comparative Examples 1 and 2. This also shows that both pre-magnesiumized and pre-lithiated treatments can improve the first coulombic efficiency and cycle stability of the material.

Claims

1. A structurally stable silicon-based composite material, characterized in that: It comprises a porous material and a core-shell material distributed in the porous material; the core-shell material comprises an inner core, a pre-magnesium layer, a pre-lithium layer and a carbon coating layer from the inside to the outside, the inner core is a silicon-based material, the pre-magnesium layer comprises a magnesium silicate zone and a mixed zone of magnesium silicate and lithium silicate from the inside to the outside, and the pre-lithium layer is lithium silicate; wherein the lithium silicate in the mixed zone is distributed in a gradient with gradually increasing concentration from the inside to the outside; the magnesium silicate is MgSiO3; the lithium silicate comprises Li2SiO3 and Li2Si2O5.

2. The structurally stable silicon-based composite material according to claim 1, characterized in that: The chemical formula of the silicon-based material is SiO x , wherein 0<x<2; the porous material is a porous carbon material, a porous ceramic material or a porous nitride.

3. The method for preparing a structurally stable silicon-based composite material according to any one of claims 1 to 2, characterized in that: include: S1: mixing the silicon source and the magnesium source evenly, and performing heat treatment under vacuum conditions to obtain a precursor containing a pre-magnesium layer; S2: pre-lithiating a precursor containing a pre-magnesium layer to obtain a silicon-based composite material containing a pre-lithium layer; S3: performing carbon coating treatment on the silicon-based composite material containing the pre-lithium layer to obtain a silicon-based composite material containing a carbon coating layer; S4: mixing the silicon-based composite material containing the carbon coating layer with the porous material, and performing heat treatment to obtain the silicon-based composite material with a stable structure.

4. The method for preparing a structurally stable silicon-based composite material according to claim 3, characterized in that: In S1, the magnesium source is metal magnesium powder or magnesium salt, and the mass of the magnesium source accounts for 15% to 80% of the mass of the silicon source.

5. The method for preparing a structurally stable silicon-based composite material according to claim 3, characterized in that: In S1, the heat treatment temperature is 1000°C to 1400°C, and the holding time is 1h to 5h.

6. The method for preparing a structurally stable silicon-based composite material according to claim 3, characterized in that: S2 specifically comprises: mixing a lithium source, a pre-lithium reagent and an organic solvent to obtain a precursor solution; mixing a precursor containing a pre-magnesium layer with the precursor solution and then performing a sealing reaction, and drying and calcining the obtained solid to obtain a silicon-based composite material containing a pre-lithium layer.

7. The method for preparing a structurally stable silicon-based composite material according to claim 6, characterized in that: The calcination temperature is 500°C to 1000°C, and the calcination time is 2h to 12h.

8. The method for preparing a structurally stable silicon-based composite material according to claim 3, characterized in that: The lithium source is one of lithium powder, lithium sheet, lithium foil, lithium block, lithium hydride and lithium hydroxide; the pre-lithium reagent is one of naphthalene, 1-methylnaphthalene, 3,3'-dimethylbiphenyl, 4,4'-dimethylbiphenyl and 3,3',4,4'-tetramethylbiphenyl.

9. The method for preparing a structurally stable silicon-based composite material according to claim 3, characterized in that: In S4, the heat treatment temperature is 650°C to 950°C, and the insulation time is 3h to 10h.

10. A lithium ion battery, characterized in that: A structurally stable silicon-based composite material comprising any one of claims 1 to 2 as a negative electrode material.