Fluorine-containing compound solid electrolyte, preparation method thereof and battery

By designing a fluoride compound solid electrolyte structure with high ionic conductivity in an all-solid-state battery, the problem of low conductivity of existing fluoride electrolytes is solved, and battery performance with high energy density and long life is achieved.

CN118738535APending Publication Date: 2024-10-01NINGBO EASTERN INSTITUTE FOR ADVANCED STUDY
View PDF 0 Cites 0 Cited by

Patent Information

Application Number
CN202411018427.4
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Filing Date
2024-07-29
Publication Date
2024-10-01

AI Technical Summary

Technical Problem

The ionic conductivity of existing fluoride electrolytes is low, which makes it difficult to meet the application requirements of all-solid-state batteries, limiting the improvement of battery energy density and voltage.

Method used

By designing the structure of the fluorine-containing compound solid electrolyte is (AX)aMBy, where A is Li, Na, K, Ag and Cu, M is Ti, Sn, Ta, Nb, Zr, Hf, Ga, Al and Fe, and B is F, Cl, Br and I,

Benefits of technology

It achieves a solid electrolyte with high ionic conductivity, supports all-solid-state batteries above 6V, is compatible with more high-energy-density cathode materials, and extends the service life of the battery.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN118738535A_ABST
    Figure CN118738535A_ABST
Patent Text Reader

Abstract

The invention relates to the technical field of battery materials, and provides a fluorine-containing compound solid electrolyte, the structural general formula is (AX) aMBy, A is at least one of Li, Na, K, Ag and Cu, M is at least one of Ti, Sn, Ta, Nb, Zr, Hf, Ga, Al and Fe, and 0.5 lt; a < lt >; 4; in addition, B is F, X is at least one of oxygen-containing anions and fluorine-containing anions, and y is 4 or 5; or, B is at least one of F, Cl, Br and I, X is BF4, and y is 3, 4 or 5. The solid electrolyte provided by the embodiment of the invention has relatively high ionic conductivity.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] This application belongs to the technical field of battery materials, and particularly relates to a fluoride-containing solid electrolyte, a preparation method thereof, and a battery. Background Art

[0002] In order to meet the needs of users for electronic products, further increase the energy density of batteries, reduce the charging times of devices such as power tools and mobile power supplies, and extend the service life of batteries. Increasing the charging voltage of the battery is one of the important ways to improve the energy density. However, increasing the charging voltage also means a challenge to the antioxidant and reduction ability of the electrolyte. Liquid electrolytes are limited by the oxidation limit of about 4.3 V of carbonate solvents, and electrolyte additives can only slightly improve the high-voltage resistance performance of the electrolyte. Fluoride solid electrolytes have a wide electrochemical stability window and are expected to be compatible with high-voltage cathodes and achieve all-solid-state batteries with higher energy density. However, the ionic conductivity of fluoride electrolytes is usually about 10 -8 S cm -1 or so, which is difficult to meet the actual application requirements. Therefore, there is no fluoride electrolyte suitable for all-solid-state battery systems so far. Developing fluoride solid electrolytes with high ionic conductivity has become an urgent problem to be solved. Summary of the Invention

[0003] The purpose of this application is to provide a fluoride-containing solid electrolyte, a preparation method thereof, and a battery, aiming to solve the problem of low ionic conductivity of fluoride electrolytes.

[0004] To achieve the above application purpose, the technical solutions adopted in this application are as follows:

[0005] In the first aspect, this application provides a fluoride-containing solid electrolyte with a structural general formula: (AX) a MB y , where: A is at least one of Li, Na, K, Ag, and Cu, M is at least one of Ti, Sn, Ta, Nb, Zr, Hf, Ga, Al, and Fe, and 0.5 < a < 4; in addition, it satisfies: B is F, X is at least one of an oxygen-containing anion and a fluorine-containing anion, and y is 4 or 5; or, B is at least one of F, Cl, Br, and I, X is BF4, and y is 3 or 4 or 5.

[0006] In the second aspect, this application provides a preparation method of a fluoride-containing solid electrolyte, including: under an anhydrous and oxygen-free inert atmosphere, subjecting AX powder and MB y powder to a solid-phase reaction by mechanical ball milling to obtain a fluoride-containing solid electrolyte (AX) a MB y .

[0007] In a third aspect, the present application provides a battery, comprising the above-mentioned fluorine-containing compound solid electrolyte or the fluorine-containing compound solid electrolyte obtained by the above-mentioned preparation method.

[0008] The present application forms an open framework structure by connecting X anions with transition metal-halogen ion polyhedra, establishing a cross-linked mesh skeleton and a three-dimensional channel running through it, so that A ions are filled in the vacancies therein. This design can realize the rapid conduction of A ions in a structure with a large free volume, and the solid electrolyte provided in the embodiment of the present application has a high ionic conductivity. Fluoride ions have high electronegativity (such as the oxidation potential limit of perfluorinated compound electrolytes is much higher than that of sulfide electrolytes and halide electrolytes). By adopting fluoride-containing electrolyte material development, all-solid-state batteries above 6V can be achieved, which are compatible with more high-energy-density positive electrode materials. BRIEF DESCRIPTION OF THE DRAWINGS

[0009] In order to more clearly illustrate the technical solutions in the embodiments of the present application, the drawings required for use in the embodiments or the description of the prior art will be briefly introduced below. Obviously, the drawings described below are only some embodiments of the present application. For ordinary technicians in this field, other drawings can be obtained based on these drawings without paying any creative work.

[0010] Figure 1 This is the electrochemical impedance spectrum of (Li3PO4)TiF4 synthesized in Example 1.

[0011] Figure 2 The X-ray diffraction spectra of (LiBF4)2TaCl5, (LiBF4)3TaCl5, and (LiBF4)TaCl5 halogen-boron-fluorine compound solid electrolytes synthesized in Examples 6 to 8 are shown in Figure 1. In the figure, the horizontal axis represents the diffraction angle (2Theta), in degrees (°); the vertical axis represents the diffraction intensity.

[0012] Figure 3 This is the X-ray diffraction spectrum of the (Li3PO4)TiF4 solid electrolyte synthesized in Example 1. In the figure, the abscissa represents the diffraction angle (2Theta), the unit is degree (°); the ordinate represents the diffraction intensity.

[0013] Figure 4 The linear scanning curves of the solid electrolyte (LiBF4)2TaCl5 provided in Example 6 of the present invention and the solid electrolyte Li2ZrCl6 provided in Comparative Example 3 are shown in Table 1. The horizontal axis represents voltage in volts (V); the vertical axis represents current density in milliamperes per gram (mA g -1 ).

[0014] Figure 5The linear scanning curves of the (Li3PO4)TiF4 solid electrolyte synthesized in Example 1 of the present invention and the solid electrolyte Li2ZrCl6 provided in Comparative Example 3. The horizontal axis represents voltage in volts (V); the vertical axis represents current density in milliamperes per gram (mA g -1 ).

[0015] Figure 6 The charge and discharge curve of the all-solid-state lithium battery assembled in Example 8 of the present invention at a rate of 0.3C for the first three weeks. In the figure, the horizontal axis represents the specific capacity in milliampere hours per gram (mAh g -1 ); the ordinate represents the relative Li + / Li voltage, the unit is volt (V).

[0016] Figure 7 The charge and discharge curve of the all-solid-state lithium battery assembled in Example 9 of the present invention at a rate of 0.3C for the first three weeks. In the figure, the horizontal axis represents the specific capacity in milliampere hours per gram (mAh g -1 ); the ordinate represents the relative Li + / Li voltage, the unit is volt (V). DETAILED DESCRIPTION

[0017] In order to make the technical problems, technical solutions and beneficial effects to be solved by the present application more clearly understood, the present application is further described in detail below in conjunction with the embodiments. It should be understood that the specific embodiments described herein are only used to explain the present application and are not used to limit the present application.

[0018] In this application, the term "and / or" describes the association relationship of associated objects, indicating that there may be three relationships. For example, A and / or B can mean: A exists alone, A and B exist at the same time, and B exists alone. A and B can be singular or plural. The character " / " generally indicates that the associated objects are in an "or" relationship.

[0019] In this application, "at least one" means one or more, and "plurality" means two or more. "At least one of the following" or similar expressions refers to any combination of these items, including any combination of single items or plural items. For example, "at least one of a, b, or c", or "at least one of a, b, and c" can all mean: a, b, c, ab (i.e., a and b), ac, bc, or abc, where a, b, c can be single or multiple, respectively.

[0020] It should be understood that in various embodiments of the present application, the magnitudes of the serial numbers of the above processes do not imply the order of execution. Some or all of the steps may be executed in parallel or sequentially. The execution order of each process should be determined by its function and internal logic, and should not constitute any limitation to the implementation process of the embodiments of the present application.

[0021] The terms used in the embodiments of the present application are only for the purpose of describing specific embodiments, and are not intended to limit the present application. The singular forms of "a", "the", and "said" used in the embodiments of the present application and the appended claims are also intended to include the plural forms, unless the context clearly indicates otherwise.

[0022] The weights of the relevant components mentioned in the specification of the embodiments of the present application may not only refer to the specific contents of each component, but also represent the proportional relationship of the weights between the components. Therefore, as long as the contents of the relevant components in the specification of the embodiments of the present application are enlarged or reduced in proportion, they are within the scope disclosed in the specification of the embodiments of the present application. Specifically, the mass described in the specification of the embodiments of the present application may be mass units well-known in the chemical industry such as μg, mg, g, kg, etc.

[0023] In a first aspect of the embodiments of the present application, a fluorine-containing compound solid electrolyte is provided, and the structural general formula is: (AX) a MB y , where: A is at least one of Li, Na, K, Ag, and Cu, M is at least one of Ti, Sn, Ta, Nb, Zr, Hf, Ga, Al, and Fe, and 0.5 < a < 4; in addition, it satisfies:

[0024] B is F, X is at least one of an oxygen-containing anion and a fluorine-containing anion, and y is 4 or 5; or, B is at least one of F, Cl, Br, and I, X is BF4, and y is 3 or 4 or 5.

[0025] The fluorine-containing solid electrolytes provided by the embodiments of the present application mainly include two types:

[0026] The first type is: the structural general formula is: (AX) a MF y , where: A is at least one of Li, Na, K, Ag, and Cu, M is at least one of Ti, Sn, Ta, Nb, Zr, Hf, Ga, Al, and Fe, X is at least one of an oxygen-containing anion and a fluorine-containing anion; 0.5 < a < 4, and y is 4 or 5. It can be named a perfluorinated compound solid electrolyte.

[0027] The second type is: the structural general formula is: (ABF4) a MB y, where: A is at least one of Li, Na, K, Ag, and Cu; M is at least one of Ti, Sn, Ta, Nb, Zr, Hf, Ga, Al, and Fe; B is at least one of F, Cl, Br, and I; 0.5 < a < 4; y is 3 or 4 or 5. It can be named a halogen-boron fluoride solid electrolyte. In the formula, "B" in "BF4" represents boron element, and "B" in "MB y " represents at least one of F, Cl, Br, and I.

[0028] Wherein, X is at least one of an oxygen-containing anion and a fluorine-containing anion, which can be one or more of the oxygen-containing anions, or one or more of the fluorine-containing anion groups, or a combination of one or more of the oxygen-containing anions and one or more of the fluorine-containing anions.

[0029] In the embodiments of the present application, the X anion, MB y is a transition metal-halide ion polyhedron.

[0030] In the embodiments of the present application, an open framework structure is formed by connecting the X anion with the transition metal-halide ion polyhedron, establishing a crosslinked network skeleton and a through three-dimensional channel, so that the A ions are filled in the vacancies therein. This design can enable the rapid conduction of A ions in a structure with a large free volume, and the solid electrolyte provided by the embodiments of the present application has a high ionic conductivity.

[0031] Fluoride ions have a high electronegativity (for example, the oxidation potential limit of perfluorinated compound electrolytes is much higher than that of sulfide electrolytes and halide electrolytes). By using fluoride electrolyte materials for development, all-solid-state batteries with a voltage above 6V can be realized, which are compatible with more high-energy density cathode materials.

[0032] In some embodiments, the structural general formula is: (AX) a MB y , where: A is Li; M is at least one of Zr, Hf, Ta, Nb, Al, Fe, and Ga; B is at least one of F, Cl, Br, and I; X is BF4; y is 3 or 4 or; 0.5 < a < 4.

[0033] In the embodiments of the present application, the structural general formula is: (AX) a MF y can be named a perfluorinated compound solid electrolyte.

[0034] In some embodiments, the structural general formula is: (AX) a MB y, wherein: A is at least one of Li, Na, K, Ag and Cu; M is at least one of Ti, Sn, Ta, Nb, Zr, Hf and Ga; B is F, X is at least one of an oxygen-containing anion and a fluorine-containing anion; y is 4 or 5; 0.5 <a<4。

[0035] In the embodiment of the present application, the general structural formula is: (AX) a MB y , which can be named as halogen-boron-fluorine compound solid electrolyte.

[0036] In some embodiments, the oxygen-containing anions include at least one of O, O2, CO3, PO4, SO4, SiO3, NO3, MoO3, WO3, B4O7 and P2O7; and / or, the fluorine-containing anions include at least one of BF4, PF6 and AsF6.

[0037] In some embodiments, X anions in the fluorine-containing compound solid electrolyte are polyhedronically connected with transition metal-halogen ions to form an open framework structure, and A ions are filled in the vacancies of the open framework.

[0038] For the first type of fluorinated solid electrolyte ((AX) a MF y ), the material system consists of X anions and fluorinated transition metal polyhedrons (MF y ) are connected to form an open framework structure, and A ions are filled in the vacancies of the open framework to obtain a specific glass-ceramic phase, achieving rapid ion conduction, and the ion conduction is greater than 0.1mS / cm at 60°C. The glass phase and glass-ceramic interface are the main ways for rapid ion conduction in this specific glass-ceramic phase structure.

[0039] For the second type of fluorinated solid electrolyte (ABF4) a MB y ), the material system is composed of BF4 tetrahedron and transition metal-halogen ion polyhedron MB y ) are connected to form an open framework structure, and halogen ions (such as Li) are filled in the vacancies of the open framework to obtain a specific glass-ceramic phase, achieving rapid ion conduction, and the room temperature ion conduction is greater than 0.1mS / cm. The glass phase and glass-ceramic interface are the main ways for rapid ion conduction in this specific glass-ceramic phase structure.

[0040] In some embodiments, auxiliary additives are further included, and the weight of the auxiliary additives is 0<w%≤20%.

[0041] In order to further improve its electrochemical properties, specific additive components can be added to the glass phase and ceramic phase by means of composite, chemical, solid solution, and mixing; the additives can also include one or a combination of elements such as H, C, N, O, Si, P, S, Se, In, Ge, Sn, etc.; the additives can also include one or a combination of alkali metal elements, alkaline earth metal elements, transition metal elements, and rare earth elements.

[0042] The mass content w% of the additive is 0<w%≤20%.

[0043] The second aspect of the present invention provides a method for preparing a fluorine-containing solid electrolyte, comprising: mixing AX powder and MB in a stoichiometric ratio in an inert atmosphere without water or oxygen. y The powder undergoes solid phase reaction by mechanical ball milling to obtain a fluorine-containing compound solid electrolyte (AX) a MB y . ,

[0044] In some embodiments, the water-free and oxygen-free inert atmosphere is N2 or Ar gas.

[0045] Furthermore, the inert atmosphere is Ar gas.

[0046] In some embodiments, during the mechanical ball milling process, the ball milling tank needs to be effectively cooled to prevent the tank temperature from being too high. Further, a circulating water cooling method is used.

[0047] In some embodiments, for the first type of fluorine-containing solid electrolyte ((AX) a MF y ), in an inert atmosphere without water or oxygen, AX powder and MF in a stoichiometric ratio were mixed. y The powder undergoes solid phase reaction by mechanical ball milling to obtain a perfluorinated compound solid electrolyte (AX) a MF y .

[0048] In some embodiments, for the second type of fluorine-containing solid electrolyte (ABF4) a MB y ), in an inert atmosphere without water or oxygen, the raw material ABF4 powder and MB in a stoichiometric ratio are mixed. y The powder undergoes solid-phase reaction through mechanical ball milling to obtain a halogen-boron-fluorine compound solid electrolyte (ABF4) a MB y .

[0049] In some embodiments, during the mechanical ball milling process, the control parameters satisfy at least one of the following (1) to (4):

[0050] (1) The diameter of the ball milling beads is 3 mm to 10 mm;

[0051] (2) The material-to-ball ratio is 60:1 to 20:1;

[0052] (3) Ball milling time is 1h to 30h;

[0053] (4) The ball mill speed is 400r / min~800r / min.

[0054] Furthermore, the ball milling beads have a diameter of 3 mm to 10 mm; in specific examples, the ball milling beads have a diameter of 3 mm, 4 mm, 5 mm, 6 mm, 6 mm, 7 mm, 8 mm, 9 mm, 10 mm, etc.

[0055] Furthermore, the material-to-ball ratio is 60:1-20:1; in specific examples, the material-to-ball ratio is 20:1, 25:1, 30:1, 35:1, 40:1, 45:1, 50:1, 55:1, 60:1, etc.

[0056] Furthermore, the ball milling time is 1 h to 30 h; in a specific example, the ball milling time is 1 h, 1.5 h, 2 h, 3 h, 5 h, 6 h, 8 h, 10 h, 12 h, 14 h, 18 h, 20 h, 22 h, 24 h, 26 h, 28 h, 30 h, etc.

[0057] Furthermore, the speed of the ball mill is 400 r / min to 800 r / min; in a specific example, the speed of the ball mill is 400 r / min, 450 r / min, 500 r / min, 550 r / min, 600 r / min, 650 r / min, 700 r / min, 750 r / min, 800 r / min, etc.

[0058] Furthermore, the diameter of the ball milling beads is 3 mm, and the material-to-ball ratio is 30:1.

[0059] Furthermore, the ball milling time is 6 h, and the ball mill speed is 500 r / min.

[0060] In some embodiments, before the mechanical ball milling process, a premixing process is further included, wherein the premixing process comprises: mixing AX powder and MB powder in a stoichiometric ratio in an inert atmosphere without water or oxygen. y The powders are pre-mixed to obtain pre-mixed powders; the pre-mixed powders are then subjected to mechanical ball milling to synthesize a fluorine-containing compound solid electrolyte (AX) a MB y .

[0061] Furthermore, the water-free and oxygen-free inert atmosphere is N2 or Ar gas; further, Ar gas is used.

[0062] Furthermore, the premixing can be carried out by hand grinding in a mortar, mixing in a mixer, or the like.

[0063] A third aspect of an embodiment of the present application provides a battery, comprising the above-mentioned fluorine-containing compound solid electrolyte or the fluorine-containing compound solid electrolyte obtained by the above-mentioned preparation method.

[0064] In some embodiments, the battery is an all-solid-state battery.

[0065] Furthermore, the all-solid-state battery includes a positive electrode sheet, a negative electrode sheet, and a solid electrolyte sheet between the positive electrode sheet and the negative electrode sheet; the solid electrolyte sheet is obtained by cold pressing a solid electrolyte material; the solid electrolyte material contains the above-mentioned fluorine-containing compound solid electrolyte or the fluorine-containing compound solid electrolyte prepared by the above-mentioned preparation method.

[0066] Furthermore, the positive electrode sheet is obtained by cold pressing or coating the positive electrode active material and the positive electrode filler.

[0067] The positive electrode active material includes but is not limited to at least one of cobalt aluminum oxide, lithium iron phosphate, lithium-rich lithium manganese oxide, lithiated layered oxides and lithiated layered sulfides. The positive electrode filler is at least one of an ion conductor, a conductive agent and a binder; the ion conductor and the solid electrolyte between the positive and negative electrodes of the battery are of the same material; the conductive agent may include at least one of graphite, carbon black, acetylene black, Ketjen black and carbon fiber; the binder may include at least one of styrene-butadiene rubber, polytetrafluoroethylene, polyvinylidene fluoride and polyethylene. Cold pressing or coating methods are common methods for preparing positive electrode sheets in the art.

[0068] Furthermore, the negative electrode sheet is obtained by cold pressing or coating the negative electrode active material and the negative electrode filler.

[0069] The negative electrode active material refers to the material that can store and release A + Ionic materials include but are not limited to metal materials, graphite, silicon, etc.; metal materials can be single metals or alloys; when metal materials are used as negative electrode active materials, negative electrode fillers can be omitted. Negative electrode fillers are at least one of ion conductors, conductive agents, and adhesives; the ion conductors and the solid electrolytes between the positive and negative electrodes of the battery are of the same material; conductive agents may include at least one of graphite, carbon black, acetylene black, Ketjen black, and carbon fiber; adhesives may include, for example, at least one of styrene-butadiene rubber, polytetrafluoroethylene, polyvinylidene fluoride, and polyethylene. Cold pressing or coating methods are common methods for preparing negative electrode sheets in this field.

[0070] The following describes the invention in conjunction with specific embodiments.

[0071] Example 1

[0072] This embodiment provides a perfluorinated compound solid electrolyte (Li3PO4)TiF4, and the specific preparation method is as follows:

[0073] In an anhydrous and oxygen-free argon atmosphere glove box, Li3PO4 and TiF4 were mixed at a molar ratio of 1:1 and hand-ground using an agate mortar for 10 min to fully pre-mix.

[0074] The premixed powder (about 1 g) was transferred to a 75 mL ball mill, and 40 g of grinding beads with a diameter of 3 mm were added accordingly. The ball mill was then evacuated and sealed. The ball mill was milled on a planetary ball mill at a speed of 600 r / min for 6 h. After the ball milling was completed, the ball mill was transferred to a glove box and opened to take out the powder in the jar, which was the synthesized (Li3PO4)TiF4 perfluorinated compound solid electrolyte.

[0075] Example 2

[0076] This embodiment provides a perfluorinated compound solid electrolyte (Li3PO4) SnF4, and the specific preparation method is the same as that of Example 1, except that:

[0077] The raw material TiF4 was replaced by SnF4.

[0078] Example 3

[0079] This embodiment provides a perfluorinated compound solid electrolyte (Li2CO3)TiF4, and the specific preparation method is the same as that of Example 1, except that:

[0080] The raw material Li3PO4 was replaced by Li2CO3.

[0081] Example 4

[0082] This embodiment provides a perfluorinated compound solid electrolyte (LiBF4)2TiF4, and the specific preparation method is the same as that of Example 1, except that:

[0083] The raw material Li3PO4 is replaced by LiBF4, and the corresponding raw material substance ratio is changed from 1:1 to 2:1.

[0084] Example 5

[0085] This embodiment provides a perfluorinated compound solid electrolyte (Li3PO4)(SiF4) 0.2 TiF4, the specific preparation method is the same as that in Example 1, except that:

[0086] The raw material SiF4 was added, and the ratio of the raw material substances was replaced with Li3PO4:SiF4:TiF4=1:0.2:1.

[0087] Example 6

[0088] This embodiment provides a halogen-boron-fluorine compound solid electrolyte (LiBF4)2TaCl5, and the specific preparation method is as follows:

[0089] In an argon atmosphere glove box without water or oxygen, LiBF4 and TaCl5 were mixed at a molar ratio of 2:1 and hand-ground using an agate mortar for 10 min to fully pre-mix.

[0090] The pre-mixed powder (about 1g) was transferred to a 75mL ball mill, and 40g of grinding beads with a diameter of 3mm were added accordingly. The ball mill was then evacuated and sealed. The ball mill was milled on a planetary ball mill at a speed of 600 rpm for 10 hours. After the ball milling was completed, the ball mill was transferred to a glove box and opened to take out the powder in the jar, which was the synthesized (LiBF4)2TaCl5 halogen-boron-fluorine compound solid electrolyte.

[0091] Example 7

[0092] This embodiment provides a halogen-boron-fluorine compound solid electrolyte (LiBF4)3TaCl5, and the specific preparation method is the same as that of Example 1, except that:

[0093] The molar ratio of the raw materials LiBF4 and TaCl5 was changed from 2:1 to 3:1.

[0094] Example 8

[0095] This embodiment provides a halogen-boron-fluorine compound solid electrolyte (LiBF4)TaCl5, and the specific preparation method is the same as that of Example 1, except that:

[0096] The molar ratio of the raw materials LiBF4 and TaCl5 was changed from 2:1 to 1:1.

[0097] Example 9

[0098] This embodiment provides a halogen-boron-fluorine compound solid electrolyte (LiBF4)2ZrCl4, and the specific preparation method is the same as that of Example 1, except that:

[0099] The raw material TaCl5 was replaced by ZrCl4, and the ball milling time was changed from 10 h to 20 h.

[0100] Example 10

[0101] This embodiment provides a halogen-boron-fluorine compound solid electrolyte (Li2O) 0.2 (LiBF4)2TaCl5, the specific preparation method is the same as that in Example 1, except that:

[0102] Add additive Li2O to the raw material, and the molar ratio of the raw materials is Li2O:LiBF4:TaCl5=0.2:2:1.

[0103] Embodiment 11

[0104] This embodiment provides an all-solid-state lithium battery, which is assembled using the perfluorinated compound solid electrolyte (Li3PO4) TiF4 provided in Example 1. The specific assembly process is as follows:

[0105] Step 1: Weigh the commercially available lithium-rich cathode Li 1.14 Ni 0.29 Mn 0.57 O2 (as positive electrode active material), (Li3PO4)TiF4 (as ion conductor) and VGCF (vapor-grown carbon fiber, as electronic conductor) with a mass ratio of 65:30:5 were manually ground in a mortar for 10 min until uniformly mixed to form a composite positive electrode.

[0106] Step 2: Weigh 50 mg of the perfluorinated solid electrolyte (Li3PO4)TiF4 powder synthesized in Example 1, and cold press it into a solid electrolyte sheet with a diameter of 10 mm at a pressure of 100 MPa for 2 min. Weigh 50 mg of Li6PS5Cl as a barrier layer between the perfluorinated solid electrolyte (Li3PO4)TiF4 and the LiIn negative electrode, and evenly spread it on the (Li3PO4) 4) One side surface of the TiF4 solid electrolyte sheet was cold pressed at a pressure of 100 MPa and maintained at this pressure for 2 minutes.

[0107] Step 3: Weigh 10 mg of the composite positive electrode prepared in step 1, evenly spread it on the other side of the (Li3PO4)TiF4 solid electrolyte sheet prepared in step 2, and cold press it at a pressure of 350 MPa for 2 minutes.

[0108] Step 4: Use a commercially available indium sheet (10 mm in diameter and 200 μm in thickness) as the negative electrode active material and stick it on the other side of the Li6PS5Cl barrier layer prepared in step 2 to form a four-layer structure of "positive electrode sheet - solid electrolyte sheet - barrier layer - negative electrode sheet". Apply a pressure of 100 MPa to the whole structure, and complete the assembly to obtain an all-solid-state lithium battery.

[0109] The above steps 1 to 4 are all carried out in a glove box with an anhydrous and oxygen-free argon atmosphere.

[0110] Example 12

[0111] This embodiment provides an all-solid-state lithium battery, which is assembled using the halogen-boron-fluorine compound solid electrolyte (LiBF4)2TaCl5 provided in Example 1. The specific assembly process is as follows:

[0112] Step 1: Weigh the commercially available lithium-rich cathode Li 1.14 Ni 0.29Mn 0.57 O2 (as positive electrode active material), (LiBF4)2TaCl5 (as ion conductor) and VGCF (vapor-grown carbon fiber, as electronic conductor) with a mass ratio of 65:30:5 were manually ground in a mortar for 10 min until uniformly mixed to form a composite positive electrode.

[0113] Step 2: Weigh 50 mg of the halogen-boron-fluoride solid electrolyte (LiBF4)2TaCl5 powder synthesized in Example 1, cold press it into a solid electrolyte sheet with a diameter of 10 mm, and keep the pressure at 100 MPa for 2 min. Weigh 50 mg of Li6PS5Cl as a barrier layer between the halogen-boron-fluoride solid electrolyte (LiBF4)2TaCl5 and the LiIn negative electrode, evenly spread it on one side of the (LiBF4)2TaCl5 solid electrolyte sheet, cold press it at a pressure of 100 MPa, and keep the pressure for 2 min.

[0114] Step 3: Weigh 10 mg of the composite positive electrode prepared in step 1, evenly spread it on the other side of the (LiBF4)2TaCl5 solid electrolyte sheet prepared in step 2, and cold press it at a pressure of 350 MPa for 2 minutes.

[0115] Step 4: Use a commercially available indium sheet (10 mm in diameter and 200 μm in thickness) as the negative electrode active material and stick it on the other side of the Li6PS5Cl barrier layer prepared in step 2 to form a four-layer structure of "positive electrode sheet - solid electrolyte sheet - barrier layer - negative electrode sheet". Apply a pressure of 100 MPa to the whole structure, and complete the assembly to obtain an all-solid-state lithium battery.

[0116] The above steps 1 to 4 are all carried out in a glove box with an anhydrous and oxygen-free argon atmosphere.

[0117] Example 13

[0118] This embodiment provides an all-solid-state LiIn-LiCoO2 battery. The specific assembly process is the same as that of Embodiment 12, except that:

[0119] The positive electrode active material is Li 1.14 Ni 0.29 Mn 0.57 O2 was replaced by LiCoO2, the conductive agent was replaced by VGCF by carbon black, and the corresponding raw material mass ratio was changed from 65:30:5 to 70:30:1.

[0120] Comparative Example 1

[0121] This case provides a solid electrolyte, and the specific preparation method is as follows:

[0122] In an argon atmosphere glove box without water or oxygen, LiF and TaF5 were mixed at a molar ratio of 1:1 and hand-ground with an agate mortar for 10 min to fully mix.

[0123] The mixed powder (about 1g) was transferred to a 75mL ball mill, and 40g of 3mm diameter grinding beads were added accordingly. The ball mill was then evacuated and sealed. The ball mill was milled on a planetary ball mill at a speed of 600 rpm for 20h. After the ball milling was completed, the ball mill was transferred to a glove box and opened to take out the powder in the jar, which was the synthesized LiTaF6 halide solid electrolyte.

[0124] Comparative Example 2

[0125] This case provides a solid electrolyte, and the specific preparation method is as follows:

[0126] In an argon atmosphere glove box without water or oxygen, LiF and ZrCl4 were mixed at a molar ratio of 8:1 and hand-ground using an agate mortar for 10 min to fully pre-mix.

[0127] The pre-mixed powder (about 1g) was transferred to a 75mL ball mill, and 40g of 3mm diameter grinding beads were added accordingly. The ball mill was then evacuated and sealed. The ball mill was milled on a planetary ball mill at a speed of 600 rpm for 20h. After the ball milling was completed, the ball mill was transferred to a glove box and opened to take out the powder in the jar, which was the synthesized Li8F8ZrCl4 halide solid electrolyte.

[0128] Comparative Example 3

[0129] This case provides a solid electrolyte, and the specific preparation method is as follows:

[0130] In an argon atmosphere glove box without water or oxygen, LiCl and ZrCl4 were mixed at a molar ratio of 2:1 and hand-ground using an agate mortar for 10 min to fully pre-mix.

[0131] The pre-mixed powder (about 1g) was transferred to a 75mL ball mill, and 40g of 3mm diameter grinding beads were added accordingly. The ball mill was then evacuated and sealed. The ball mill was milled on a planetary ball mill at a speed of 600 rpm for 20h. After the ball milling was completed, the ball mill was transferred to a glove box and opened to take out the powder in the jar, which was the synthesized Li2ZrCl6 halide solid electrolyte.

[0132] 1. Characterization and Analysis

[0133] 1. Characterization and analysis of ionic conductivity

[0134] (1) Characterization methods

[0135] In a water-free and oxygen-free argon atmosphere glove box, the solid electrolyte powders prepared in Examples 1-4, Examples 6-10 and Comparative Examples 1-2 were filled into a cylindrical tabletting mold (with a diameter of 10 mm); and cold pressed at a pressure of 375 MPa for 2 min to obtain a solid electrolyte sheet with a thickness of 0.5 mm to 1.5 mm and a diameter of 10 mm; after gold plating on the upper and lower surfaces of the solid electrolyte sheet, two stainless steel blocking electrodes were used to clamp the upper and lower surfaces, and the electrochemical workstation was connected to test the electrochemical AC impedance spectrum at room temperature; room temperature Li was extracted from the measured electrochemical impedance spectrum. + Ionic conductivity.

[0136] (2) Characterization results

[0137] Table 1 shows the ionic conductivity of each solid electrolyte sample at 60 °C.

[0138] Figure 1 The electrochemical impedance spectroscopy of (Li3PO4)TiF4 synthesized in Example 1 at 60°C is shown.

[0139] Table 1 Ionic conductivity of each solid electrolyte sample

[0140]

[0141]

[0142] 2. Crystal structure characterization and analysis

[0143] (1) Characterization methods

[0144] The solid electrolytes prepared in Examples 6-8 were characterized using an X-ray diffractometer.

[0145] (2) Characterization results

[0146] like Figure 2 As shown, the crystal structures of (LiBF4)2TaCl5, (LiBF4)3TaCl5, (LiBF4)TaCl5 and (Li3PO4)TiF4 solid electrolytes synthesized in the examples are respectively characterized.

[0147] The results show that the diffraction peaks of the three halogen-boron-fluorine compound solid electrolytes provided in the examples can be calibrated as the residual raw material phase LiBF4, and the characteristic XRD peaks are located at 2theta = 14.1°, 20.0°, 24.9°, 26.4°, and 31.8°. This indicates that in addition to the raw material crystalline phase, there are a large number of amorphous phases in the above three halogen-boron-fluorine compound solid electrolytes, and the amorphous phases contain several elements such as Li, B, F, Ta, and Cl.

[0148] The XRD pattern of (Li3PO4)TiF4 is shown in Figure 3, no characteristic diffraction peak appears, and the (Li3PO4)TiF4 solid electrolyte is an amorphous phase.

[0149] 3. Electrochemical window test

[0150] (1) Test method

[0151] At room temperature, the EC-lab electrochemical workstation was used to perform a linear scanning test on a battery configured as solid electrolyte + carbon black (mass ratio 5:5) | solid electrolyte | Li6PS5Cl | Li.

[0152] (2) Test results

[0153] Test results such as Figure 4 and Figure 5 As shown, (LiBF4)2TaCl5 still has no obvious oxidation peak above 6V. (Li3PO4)TiF4 also has no obvious oxidation peak above 6V.

[0154] 4. Constant current charge and discharge test

[0155] (1) Test method

[0156] At room temperature, the all-solid-state batteries provided in Examples 9-10 were subjected to constant current charge and discharge tests using a BlueDian battery testing system, with a voltage range of 2.5 V to 4.8 V (relative voltage of Li+ / Li) and a cycle rate of 0.3C.

[0157] (2) Test results

[0158] Test results such as Figure 6 and Figure 7 shown.

[0159] The all-solid-state battery provided in Example 9 has a reversible capacity of 177.2 mAh g at a rate of 0.3C. -1 The first-week efficiency and the second-week efficiency were 87.0% and 99.3% respectively.

[0160] The all-solid-state battery provided in Example 10 has a reversible capacity of 203.1 mAh g at a rate of 0.3C. -1 The efficiency in the first week and the second week were 91.5% and 99.2% respectively.

[0161] The above description is only a preferred embodiment of the present application and is not intended to limit the present application. Any modifications, equivalent substitutions and improvements made within the spirit and principles of the present application should be included in the protection scope of the present application.

Claims

1. A fluorine-containing compound solid electrolyte, characterized in that: The structural general formula is: (AX) a MB y , where: A is at least one of Li, Na, K, Ag, and Cu, M is at least one of Ti, Sn, Ta, Nb, Zr, Hf, Ga, Al, and Fe, 0.5 < a < 4; in addition, it satisfies: B is F, X is at least one of an oxygen-containing anion and a fluorine-containing anion, and y is 4 or 5; Alternatively, B is at least one of F, Cl, Br and I, X is BF4, and y is 3 or 4 or 5.

2. The fluorine-containing compound solid electrolyte according to claim 1, characterized in that The general structural formula is: (AX) a MB y ,in: A is Li; M is at least one of Zr, Hf, Ta, Nb, Al, Fe and Ga; B is at least one of F, Cl, Br and I; X is BF4; y is 3 or 4 or; 0.5<a<4。 3. The fluorine-containing compound solid electrolyte according to claim 1, characterized in that The general structural formula is: (AX) a MB y ,in: A is at least one of Li, Na, K, Ag and Cu; M is at least one of Ti, Sn, Ta, Nb, Zr, Hf and Ga; B is F, and X is at least one of an oxygen-containing anion and a fluorine-containing anion; y is 4 or 5; 0.5<a<4。 4. The fluorine-containing compound solid electrolyte according to claim 1, characterized in that The oxygen-containing anions include at least one of O, O2, CO3, PO4, SO4, SiO3, NO3, MoO3, WO3, B4O7 and P2O7; and / or the fluorine-containing anions include at least one of BF4, PF6 and AsF6.

5. The fluorine-containing compound solid electrolyte according to any one of claims 1 to 5, characterized in that In the fluorine-containing compound solid electrolyte, X anions are polyhedronically connected with transition metal-halogen ions to form an open framework structure, and A ions are filled in the vacancies of the open framework.

6. The fluorine-containing compound solid electrolyte according to any one of claims 1 to 5, characterized in that It also includes auxiliary additives, and the weight of the auxiliary additives is 0<w%≤20%.

7. A method for preparing a fluorine-containing compound solid electrolyte, characterized in that: include: In an inert atmosphere without water or oxygen, AX powder and MB in a stoichiometric ratio were mixed. y The powder undergoes solid phase reaction by mechanical ball milling to obtain a fluorine-containing compound solid electrolyte (AX) a MB y .

8. The method for preparing a fluorine-containing compound solid electrolyte according to claim 7, wherein: During the mechanical ball milling process, the control parameters satisfy at least one of the following (1) to (4): (1) The diameter of the ball milling beads is 3 mm to 10 mm; (2) The material-to-ball ratio is 60:1 to 20:1; (3) The ball milling time is 1h to 30h. (4) The ball mill speed is 400r / min~800r / min.

9. The method for preparing a fluorine-containing compound solid electrolyte according to claim 7, characterized in that: Before the mechanical ball milling process, a premixing process is also included, and the premixing process includes: In an inert atmosphere without water or oxygen, AX powder and MB in a stoichiometric ratio were mixed. y The powders are pre-mixed to obtain pre-mixed powders; The premixed powder is then subjected to mechanical ball milling to synthesize a fluorine-containing compound solid electrolyte (AX) a MB y .

10. A battery, characterized in that: It comprises the fluorine-containing compound solid electrolyte as described in any one of claims 1 to 6 or the fluorine-containing compound solid electrolyte obtained by the preparation method as described in any one of claims 7 to 9.