Composite solid electrolyte membrane for lithium battery and preparation method of composite solid electrolyte membrane

By using a composite solid electrolyte membrane composed of polyvinylidene fluoride, lithium salts, polyimidazolium salts and modified mesoporous molecular sieves in lithium-ion batteries, the safety and stability problems of traditional liquid electrolytes are solved, and the ionic conductivity of the battery is improved. and flexibility, extending battery life.

CN118738544AActive Publication Date: 2024-10-01JIANGXI JIANDAYUANHONG NEW ENERGY TECH CO LTD

Patent Information

Application Number
CN202411104378.6
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Filing Date
2024-08-13
Publication Date
2024-10-01
Estimated Expiration
2044-08-13

AI Technical Summary

Technical Problem

Traditional lithium-ion batteries using liquid electrolytes have safety hazards and stability issues, and are sensitive to temperature and pressure, affecting battery performance and life.

Method used

A composite solid electrolyte membrane composed of polyvinylidene fluoride, lithium salt, polyimidazole salt and modified mesoporous molecular sieve is used to synthesize polyimidazolium salts with different numbers of carbon atoms in the main chain through Debus-Radziszewski reaction, and is treated with ultrasonic treatment and packaging Coating technology improves dispersion and forms a network structure to improve conductivity and flexibility.

Benefits of technology

It significantly improves the ionic conductivity and flexibility of the electrolyte membrane, enhances the mechanical strength and cycle stability of the battery, solves the safety and stability problems of traditional electrolytes, and extends the service life of the battery.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure BDA0004990304680000031
    Figure BDA0004990304680000031
Patent Text Reader

Abstract

The invention belongs to the technical field of lithium ion batteries, and particularly relates to a composite solid electrolyte membrane for a lithium battery and a preparation method of the composite solid electrolyte membrane. The polyimidazole salt and the modified mesoporous molecular sieve are used as additives of the solid electrolyte membrane. The used polyimidazole salt is synthesized by adopting Debus-Radziszewski reaction, the main chain of the polyimidazole salt is provided with alkyl chains with different carbon atom numbers, and the ionic conductivity and the flexibility of the electrolyte membrane can be effectively enhanced by adopting a proper carbon chain length. The modified mesoporous molecular sieve has an orderly-arranged pore channel structure, a large specific surface area and good dispersity, the mechanical strength of the solid polymer electrolyte can be enhanced, and the ionic conductivity and cycling stability of a lithium ion battery are improved. And the ionic conductivity and the flexibility of the electrolyte membrane are greatly improved through the synergism of the two.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The present invention belongs to the technical field of lithium ion batteries, and specifically relates to a composite solid electrolyte membrane for lithium batteries and a preparation method thereof. Background Art

[0002] Lithium battery is an important rechargeable battery technology, widely used in electric vehicles, portable devices and energy storage systems. Traditional lithium-ion batteries use liquid electrolytes, but liquid electrolytes have a series of safety and stability issues, such as battery combustion, leakage and evaporation. Therefore, in recent years, researchers have been committed to developing safer, more stable and better performing electrolyte materials, among which composite solid electrolyte membranes have attracted much attention as a potential alternative.

[0003] Traditional liquid electrolytes, such as organic solvents and salt solutions, have safety risks such as flammability, high volatility, and easy generation of gas at high temperatures. In addition, liquid electrolytes are sensitive to temperature and external pressure, which may cause fluctuations and degradation of battery performance.

[0004] The composite solid electrolyte membrane is composed of a polymer matrix and ceramic particles, and has excellent ionic conductivity and chemical stability, which can effectively solve the problems of traditional liquid electrolytes. At the same time, the composite solid electrolyte can inhibit the formation of lithium dendrites and improve the cycle life of the battery.

[0005] The polymer matrix is ​​the main component of the composite solid electrolyte, and the common ones are polyethylene oxide (PEO), polyacrylonitrile (PAN), etc. These polymers have high molecular chain flexibility, which can provide sufficient mechanical strength and flexibility while maintaining high lithium ion conductivity. The introduction of ceramic particles, such as lithium oxide (Li2O), helps to improve the ion conductivity of the composite solid electrolyte. Ceramic particles form a network structure in the polymer matrix, which makes it easier for lithium ions to pass through, thereby improving the conductivity of the battery.

[0006] The technology for preparing composite solid electrolytes is constantly developing. Electrolyte membranes with a certain thickness and uniformity can be prepared by casting, solution impregnation, stretching and other methods. The influence of the control of temperature, humidity and pressure during the preparation process on the performance of the electrolyte membrane has gradually been studied in depth.

[0007] As one of the key components of lithium batteries, composite solid electrolyte membrane provides higher safety and stability for batteries and is expected to be widely used in electric vehicles, wearable devices, energy storage systems, etc. The continuous improvement of its performance will promote the development of lithium battery technology and achieve higher energy density, longer life, and safer and more reliable battery systems.

[0008] In general, composite solid electrolyte membranes have great potential in the field of lithium battery technology, and their research and development will provide strong support for the advancement of future energy storage technology. Summary of the invention

[0009] In view of the defects in the prior art, the present invention discloses a composite solid electrolyte membrane for a lithium battery and a preparation method thereof.

[0010] A composite solid electrolyte membrane for lithium batteries comprises the following components: a polymer matrix, a lithium salt, a polyimidazole salt, and a modified mesoporous molecular sieve.

[0011] Preferably, the composite solid electrolyte membrane for lithium battery is composed of the following components by mass: 90-110 parts of polymer matrix, 1-20 parts of lithium salt, 10-20 parts of polyimidazole salt, and 10-15 parts of modified mesoporous molecular sieve.

[0012] The polymer matrix is ​​a polymer electrolyte commonly used in the art, and can be selected from at least one of polyethylene oxide, polyacrylonitrile, polyvinylidene fluoride, polycarbonate, and polyacrylate; preferably, the present invention uses polyvinylidene fluoride as the polymer matrix.

[0013] Polyvinylidene fluoride has excellent chemical stability and can resist corrosion from many chemicals, which allows it to remain stable in the electrolyte membrane for a longer time and is not prone to chemical degradation; it is also a polar polymer with a high electrical susceptibility and dielectric constant, which helps to improve the ionic conductivity of the solid electrolyte membrane. Polyvinylidene fluoride also has good thermal stability and can maintain physical and electrical properties over a wide temperature range, suitable for a variety of working conditions. Polyvinylidene fluoride has good solubility in some solvents, which helps to regulate its structure and properties when preparing the film. However, although polyvinylidene fluoride is flexible, its crystallinity on the polymer chain may also lead to relatively poor processability. This may pose some challenges to the preparation and molding of the membrane. Relative to some other solid electrolyte materials, polyvinylidene fluoride may have lower ionic conductivity. This may be a disadvantage in some applications that require high ionic conductivity.

[0014] The lithium salt is at least one of lithium perchlorate, lithium hexafluorophosphate, lithium difluorooxalatoborate, lithium trifluoromethanesulfonate, lithium bis(trifluoromethanesulfonyl imide), lithium tetrafluoroborate, lithium dioxalatoborate, and lithium nitrate; preferably, the present invention uses lithium tetrafluoroborate as the lithium salt of the present invention, which has higher electrical conductivity and better chemical stability.

[0015] The polyimidazolium salt is a main chain alkylated polyimidazolium salt, and the main chain thereof is composed of imidazole groups and alkyl groups alternately.

[0016] The preparation method of the polyimidazole salt comprises the following steps:

[0017] 90-110 mmol of a diamine and 20-30 mL of water are mixed and placed in an ice water bath for cooling to obtain a mixed solution; 20-30 mL of a 37 wt% aqueous hydrochloric acid solution is added to the mixed solution to obtain an acidic diamine solution; a mixture of 8-9 g of formaldehyde and 14-15 g of glyoxal is added dropwise to the acidic diamine solution, and then refluxed at 75-85° C. for 4-5 hours, and the solvent and unreacted monomers are removed by rotary evaporation to obtain the polyimidazole salt.

[0018] The diamine is one of 1,4-diaminobutane, 1,6-diaminohexane, 1,8-diaminooctane, 1,10-diaminodecane and 1,12-diaminododecane; preferably, the diamine is 1,8-diaminooctane.

[0019] The present invention adopts Debus-Radziszewski reaction to synthesize polyimidazolate salts with different carbon atom number alkyl chains in the main chain, and the present invention finds that the length of carbon chain has a greater impact on the performance of polyimidazolate salts. The present invention adds polyimidazolate salts with different carbon chain lengths to the electrolyte membrane, and finds that longer carbon chains can better enhance the flexibility, high temperature resistance and corrosion resistance of the electrolyte membrane, but longer carbon chains are not conducive to ion conduction, which can reduce the ionic conductivity of the electrolyte membrane, and when the carbon chain is shorter, the addition of polyimidazolate salts reduces the toughness of the electrolyte membrane, showing more obvious brittleness, making the electrolyte membrane prone to cracking or fracture in actual use. This may affect the mechanical stability and life of the electrolyte membrane. Therefore, the present invention preferably uses 1,8-diaminooctane as a raw material to synthesize a polyimidazolate salt with eight carbon atoms in length, which has excellent flexibility, high temperature resistance and corrosion resistance, and is also less influential on the ionic conductivity of the electrolyte membrane.

[0020] The reaction process of synthesizing polyimidazole salt from 1,8-diaminooctane is as follows:

[0021]

[0022] The preparation method of the modified mesoporous molecular sieve comprises the following steps:

[0023] S1. Add mesoporous molecular sieve into 9-11 mmol / L Tris buffer solution, and disperse it evenly by ultrasonic treatment to obtain a mesoporous molecular sieve suspension;

[0024] S2: adding dopamine to the mesoporous molecular sieve suspension obtained in step S1 to obtain a precursor suspension, stirring at 40-50° C. for 6-8 hours, filtering, washing and drying to obtain a modified mesoporous molecular sieve.

[0025] The ultrasonic power is 600-800W and the frequency is 40-80kHz.

[0026] The concentration of dopamine in the precursor suspension is 10-30 mmol / L, and the mass volume ratio of the added amount of the mesoporous molecular sieve to the Tris buffer solution is 1 g: (5-20) L.

[0027] Since the mesoporous molecular sieve has an orderly arranged pore structure, a large specific surface area and a nanometer-level particle size, the surface voids formed during accumulation and its unique mesoporous channels are conducive to the entry and passage of ions. In addition, as an inorganic particle, the mesoporous molecular sieve can improve the mechanical properties of the polymer electrolyte membrane while improving the ionic conductivity. However, like most inorganic particles, its dispersibility in the polymer is poor. Therefore, the present invention adopts polydopamine coating to anchor the mesoporous molecular sieve in the polymer cross-linked network, thereby enhancing the mechanical strength of the solid polymer electrolyte, improving its dispersibility in the polymer matrix, being conducive to the suppression of lithium dendrites, and improving the ionic conductivity and cycle stability of the lithium ion battery.

[0028] A composite solid electrolyte membrane for a lithium battery and a preparation method thereof, comprising the following steps:

[0029] The polyvinylidene fluoride and acetone solution are mixed, and stirred at 50-60°C until the polyvinylidene fluoride is dissolved in the acetone to form a transparent sol. After 0.5-1h, lithium salt, polyimidazole salt, and modified mesoporous molecular sieve are added to the polyvinylidene fluoride sol, and ultrasonic stirring is continued for 0.5-1h. Then a certain amount of porogen dimethyl carbonate is added, and after mixing evenly, constant temperature stirring is continued to react for 4-8h to obtain a uniform and transparent casting solution. After cooling to room temperature, the solution is scraped to form a film, the film is peeled off, and the film is dried at 80-90°C for 24-36h to obtain the composite solid electrolyte membrane for the lithium battery.

[0030] The ultrasonic power is 600-800W and the frequency is 40-80kHz.

[0031] Beneficial effects of the present invention:

[0032] The present invention uses polyimidazole salt and modified mesoporous molecular sieve as additives of solid electrolyte membrane. The polyimidazole salt used is a polyimidazole salt whose main chain has alkyl chains with different carbon atoms by Debus-Radziszewski reaction synthesis, and the suitable carbon chain length can effectively enhance the ionic conductivity and flexibility of the electrolyte membrane. The modified mesoporous molecular sieve has an orderly arranged pore structure, a large specific surface area and good dispersibility, can enhance the mechanical strength of the solid polymer electrolyte, and improve the ionic conductivity and cycle stability of the lithium ion battery. The two work together to greatly improve the ionic conductivity and flexibility of the electrolyte membrane. DETAILED DESCRIPTION

[0033] In the present invention, unless otherwise specified, all equipment and raw materials can be purchased from the market or are commonly used in the industry. The methods in the following embodiments, unless otherwise specified, are conventional methods in the art.

[0034] Polyvinylidene fluoride, product number: FR904 W, Shanghai San Ai Fu New Materials Co., Ltd.

[0035] Mesoporous molecular sieve, product number: DM-2, Shandong Dengzhuo Chemical Co., Ltd.

[0036] Example 1

[0037] A composite solid electrolyte membrane for a lithium battery consists of the following components, measured by mass: 100 parts of a polymer matrix, 12 parts of a lithium salt, 16 parts of a polyimidazole salt, and 14 parts of a modified mesoporous molecular sieve.

[0038] The polymer matrix is ​​polyvinylidene fluoride.

[0039] The lithium salt is lithium tetrafluoroborate.

[0040] The preparation method of the polyimidazole salt comprises the following steps:

[0041] 100 mmol 1,4-diaminobutane and 25 mL water are mixed and placed in an ice water bath for cooling to obtain a mixed solution; 25 mL 37 wt % hydrochloric acid aqueous solution is added to the mixed solution to obtain an acidic diamine solution; a mixture of 8.12 g formaldehyde and 14.51 g glyoxal is added dropwise to the acidic diamine solution, and then refluxed at 80° C. for 4 hours, and the solvent and unreacted monomers are removed by rotary evaporation to obtain the polyimidazole salt.

[0042] The preparation method of the modified mesoporous molecular sieve comprises the following steps:

[0043] S1. Add mesoporous molecular sieve into 10mmol / L Tris buffer solution, disperse evenly by ultrasonic treatment, and obtain mesoporous molecular sieve suspension;

[0044] S2: adding dopamine to the mesoporous molecular sieve suspension obtained in step S1 to obtain a precursor suspension, stirring at 45° C. for 7 hours, filtering, washing, and drying to obtain a modified mesoporous molecular sieve.

[0045] The ultrasonic power is 600W and the frequency is 60kHz.

[0046] The concentration of dopamine in the precursor suspension is 20 mmol / L, and the mass volume ratio of the added amount of the mesoporous molecular sieve to the Tris buffer solution is 1 g:10 L.

[0047] A composite solid electrolyte membrane for a lithium battery and a preparation method thereof, comprising the following steps:

[0048] By mass, 100 parts of polyvinylidene fluoride and 600 parts of acetone solution are mixed, and stirred at 55°C until polyvinylidene fluoride is dissolved in acetone to form a transparent sol. After 0.5h, 12 parts of lithium salt, 16 parts of polyimidazole salt, and 14 parts of modified mesoporous molecular sieve are added to the polyvinylidene fluoride sol, and ultrasonic stirring is continued for 0.5h. Then a certain amount of porogen dimethyl carbonate is added, and after mixing evenly, constant temperature stirring is continued to react for 6h to obtain a uniform and transparent casting solution. After cooling to room temperature, it is scraped to form a film, the film is peeled off, and dried at 90°C for 36h to obtain the composite solid electrolyte membrane for the lithium battery.

[0049] The ultrasonic power is 600W and the frequency is 60kHz.

[0050] Example 2

[0051] A composite solid electrolyte membrane for a lithium battery consists of the following components, measured by mass: 100 parts of a polymer matrix, 12 parts of a lithium salt, 16 parts of a polyimidazole salt, and 14 parts of a modified mesoporous molecular sieve.

[0052] The polymer matrix is ​​polyvinylidene fluoride.

[0053] The lithium salt is lithium tetrafluoroborate.

[0054] The preparation method of the polyimidazole salt comprises the following steps:

[0055] 100 mmol 1,6-diaminohexane and 25 mL water are mixed and placed in an ice water bath for cooling to obtain a mixed solution; 25 mL 37 wt % aqueous hydrochloric acid solution is added to the mixed solution to obtain an acidic diamine solution; a mixture of 8.12 g formaldehyde and 14.51 g glyoxal is added dropwise to the acidic diamine solution, and then refluxed at 80° C. for 4 hours, and the solvent and unreacted monomers are removed by rotary evaporation to obtain the polyimidazole salt.

[0056] The preparation method of the modified mesoporous molecular sieve comprises the following steps:

[0057] S1. Add mesoporous molecular sieve into 10mmol / L Tris buffer solution, disperse evenly by ultrasonic treatment, and obtain mesoporous molecular sieve suspension;

[0058] S2: adding dopamine to the mesoporous molecular sieve suspension obtained in step S1 to obtain a precursor suspension, stirring at 45° C. for 7 hours, filtering, washing, and drying to obtain a modified mesoporous molecular sieve.

[0059] The ultrasonic power is 600W and the frequency is 60kHz.

[0060] The concentration of dopamine in the precursor suspension is 20 mmol / L, and the mass volume ratio of the added amount of the mesoporous molecular sieve to the Tris buffer solution is 1 g:10 L.

[0061] A composite solid electrolyte membrane for a lithium battery and a preparation method thereof, comprising the following steps:

[0062] By mass, 100 parts of polyvinylidene fluoride and 600 parts of acetone solution are mixed, and stirred at 55°C until polyvinylidene fluoride is dissolved in acetone to form a transparent sol. After 0.5h, 12 parts of lithium salt, 16 parts of polyimidazole salt, and 14 parts of modified mesoporous molecular sieve are added to the polyvinylidene fluoride sol, and ultrasonic stirring is continued for 0.5h. Then a certain amount of porogen dimethyl carbonate is added, and after mixing evenly, constant temperature stirring is continued to react for 6h to obtain a uniform and transparent casting solution. After cooling to room temperature, it is scraped to form a film, the film is peeled off, and dried at 90°C for 36h to obtain the composite solid electrolyte membrane for the lithium battery.

[0063] The ultrasonic power is 600W and the frequency is 60kHz.

[0064] Example 3

[0065] A composite solid electrolyte membrane for a lithium battery consists of the following components, measured by mass: 100 parts of a polymer matrix, 12 parts of a lithium salt, 16 parts of a polyimidazole salt, and 14 parts of a modified mesoporous molecular sieve.

[0066] The polymer matrix is ​​polyvinylidene fluoride.

[0067] The lithium salt is lithium tetrafluoroborate.

[0068] The preparation method of the polyimidazole salt comprises the following steps:

[0069] 100 mmol 1,8-diaminooctane and 25 mL water are mixed and placed in an ice water bath for cooling to obtain a mixed solution; 25 mL 37 wt % aqueous hydrochloric acid solution is added to the mixed solution to obtain an acidic diamine solution; a mixture of 8.12 g formaldehyde and 14.51 g glyoxal is added dropwise to the acidic diamine solution, and then refluxed at 80° C. for 4 hours, and the solvent and unreacted monomers are removed by rotary evaporation to obtain the polyimidazole salt.

[0070] The preparation method of the modified mesoporous molecular sieve comprises the following steps:

[0071] S1. Add mesoporous molecular sieve into 10mmol / L Tris buffer solution, disperse evenly by ultrasonic treatment, and obtain mesoporous molecular sieve suspension;

[0072] S2: adding dopamine to the mesoporous molecular sieve suspension obtained in step S1 to obtain a precursor suspension, stirring at 45° C. for 7 hours, filtering, washing, and drying to obtain a modified mesoporous molecular sieve.

[0073] The ultrasonic power is 600W and the frequency is 60kHz.

[0074] The concentration of dopamine in the precursor suspension is 20 mmol / L, and the mass volume ratio of the added amount of the mesoporous molecular sieve to the Tris buffer solution is 1 g:10 L.

[0075] A composite solid electrolyte membrane for a lithium battery and a preparation method thereof, comprising the following steps:

[0076] By mass, 100 parts of polyvinylidene fluoride and 600 parts of acetone solution are mixed, and stirred at 55°C until polyvinylidene fluoride is dissolved in acetone to form a transparent sol. After 0.5h, 12 parts of lithium salt, 16 parts of polyimidazole salt, and 14 parts of modified mesoporous molecular sieve are added to the polyvinylidene fluoride sol, and ultrasonic stirring is continued for 0.5h. Then a certain amount of porogen dimethyl carbonate is added, and after mixing evenly, constant temperature stirring is continued to react for 6h to obtain a uniform and transparent casting solution. After cooling to room temperature, it is scraped to form a film, the film is peeled off, and dried at 90°C for 36h to obtain the composite solid electrolyte membrane for the lithium battery.

[0077] The ultrasonic power is 600W and the frequency is 60kHz.

[0078] Example 4

[0079] A composite solid electrolyte membrane for a lithium battery consists of the following components, measured by mass: 100 parts of a polymer matrix, 12 parts of a lithium salt, 16 parts of a polyimidazole salt, and 14 parts of a modified mesoporous molecular sieve.

[0080] The polymer matrix is ​​polyvinylidene fluoride.

[0081] The lithium salt is lithium tetrafluoroborate.

[0082] The preparation method of the polyimidazole salt comprises the following steps:

[0083] 100 mmol 1,10-diaminodecane and 25 mL water are mixed and placed in an ice water bath for cooling to obtain a mixed solution; 25 mL 37 wt % aqueous hydrochloric acid solution is added to the mixed solution to obtain an acidic diamine solution; a mixture of 8.12 g formaldehyde and 14.51 g glyoxal is added dropwise to the acidic diamine solution, and then refluxed at 80° C. for 4 hours, and the solvent and unreacted monomers are removed by rotary evaporation to obtain the polyimidazole salt.

[0084] The preparation method of the modified mesoporous molecular sieve comprises the following steps:

[0085] S1. Add mesoporous molecular sieve into 10mmol / L Tris buffer solution, disperse evenly by ultrasonic treatment, and obtain mesoporous molecular sieve suspension;

[0086] S2: adding dopamine to the mesoporous molecular sieve suspension obtained in step S1 to obtain a precursor suspension, stirring at 45° C. for 7 hours, filtering, washing, and drying to obtain a modified mesoporous molecular sieve.

[0087] The ultrasonic power is 600W and the frequency is 60kHz.

[0088] The concentration of dopamine in the precursor suspension is 20 mmol / L, and the mass volume ratio of the added amount of the mesoporous molecular sieve to the Tris buffer solution is 1 g:10 L.

[0089] A composite solid electrolyte membrane for a lithium battery and a preparation method thereof, comprising the following steps:

[0090] By mass, 100 parts of polyvinylidene fluoride and 600 parts of acetone solution are mixed, and stirred at 55°C until polyvinylidene fluoride is dissolved in acetone to form a transparent sol. After 0.5h, 12 parts of lithium salt, 16 parts of polyimidazole salt, and 14 parts of modified mesoporous molecular sieve are added to the polyvinylidene fluoride sol, and ultrasonic stirring is continued for 0.5h. Then a certain amount of porogen dimethyl carbonate is added, and after mixing evenly, constant temperature stirring is continued to react for 6h to obtain a uniform and transparent casting solution. After cooling to room temperature, it is scraped to form a film, the film is peeled off, and dried at 90°C for 36h to obtain the composite solid electrolyte membrane for the lithium battery.

[0091] The ultrasonic power is 600W and the frequency is 60kHz.

[0092] Example 5

[0093] A composite solid electrolyte membrane for a lithium battery consists of the following components, measured by mass: 100 parts of a polymer matrix, 12 parts of a lithium salt, 16 parts of a polyimidazole salt, and 14 parts of a modified mesoporous molecular sieve.

[0094] The polymer matrix is ​​polyvinylidene fluoride.

[0095] The lithium salt is lithium tetrafluoroborate.

[0096] The preparation method of the polyimidazole salt comprises the following steps:

[0097] 100 mmol 1,12-diaminododecane and 25 mL water are mixed and placed in an ice water bath for cooling to obtain a mixed solution; 25 mL 37 wt % aqueous hydrochloric acid solution is added to the mixed solution to obtain an acidic diamine solution; a mixture of 8.12 g formaldehyde and 14.51 g glyoxal is added dropwise to the acidic diamine solution, and then refluxed at 80° C. for 4 hours, and the solvent and unreacted monomers are removed by rotary evaporation to obtain the polyimidazole salt.

[0098] The preparation method of the modified mesoporous molecular sieve comprises the following steps:

[0099] S1. Add mesoporous molecular sieve into 10mmol / L Tris buffer solution, disperse evenly by ultrasonic treatment, and obtain mesoporous molecular sieve suspension;

[0100] S2: adding dopamine to the mesoporous molecular sieve suspension obtained in step S1 to obtain a precursor suspension, stirring at 45° C. for 7 hours, filtering, washing, and drying to obtain a modified mesoporous molecular sieve.

[0101] The ultrasonic power is 600W and the frequency is 60kHz.

[0102] The concentration of dopamine in the precursor suspension is 20 mmol / L, and the mass volume ratio of the added amount of the mesoporous molecular sieve to the Tris buffer solution is 1 g:10 L.

[0103] A composite solid electrolyte membrane for a lithium battery and a preparation method thereof, comprising the following steps:

[0104] By mass, 100 parts of polyvinylidene fluoride and 600 parts of acetone solution are mixed, and stirred at 55°C until polyvinylidene fluoride is dissolved in acetone to form a transparent sol. After 0.5h, 12 parts of lithium salt, 16 parts of polyimidazole salt, and 14 parts of modified mesoporous molecular sieve are added to the polyvinylidene fluoride sol, and ultrasonic stirring is continued for 0.5h. Then a certain amount of porogen dimethyl carbonate is added, and after mixing evenly, constant temperature stirring is continued to react for 6h to obtain a uniform and transparent casting solution. After cooling to room temperature, it is scraped to form a film, the film is peeled off, and dried at 90°C for 36h to obtain the composite solid electrolyte membrane for the lithium battery.

[0105] The ultrasonic power is 600W and the frequency is 60kHz.

[0106] Comparative Example 1

[0107] A composite solid electrolyte membrane for a lithium battery consists of the following components, measured by mass: 100 parts of a polymer matrix and 12 parts of a lithium salt.

[0108] The polymer matrix is ​​polyvinylidene fluoride.

[0109] The lithium salt is lithium tetrafluoroborate.

[0110] A composite solid electrolyte membrane for a lithium battery and a preparation method thereof, comprising the following steps:

[0111] By mass, 100 parts of polyvinylidene fluoride and 600 parts of acetone solution are mixed, and stirred at 55°C until the polyvinylidene fluoride is dissolved in acetone to form a transparent sol. After 0.5h, 12 parts of lithium salt are added to the polyvinylidene fluoride sol, and ultrasonic stirring is continued for 0.5h. Then a certain amount of porogen dimethyl carbonate is added, and after mixing evenly, constant temperature stirring is continued to react for 6h to obtain a uniform and transparent casting liquid. After cooling to room temperature, it is scraped to form a film, the film is peeled off, and dried at 90°C for 36h to obtain the composite solid electrolyte membrane for the lithium battery.

[0112] The ultrasonic power is 600W and the frequency is 60kHz.

[0113] Comparative Example 2

[0114] A composite solid electrolyte membrane for a lithium battery consists of the following components, measured by mass: 100 parts of a polymer matrix, 12 parts of a lithium salt, and 16 parts of a polyimidazole salt.

[0115] The polymer matrix is ​​polyvinylidene fluoride.

[0116] The lithium salt is lithium tetrafluoroborate.

[0117] The preparation method of the polyimidazole salt comprises the following steps:

[0118] 100 mmol 1,8-diaminooctane and 25 mL water are mixed and placed in an ice water bath for cooling to obtain a mixed solution; 25 mL 37 wt % aqueous hydrochloric acid solution is added to the mixed solution to obtain an acidic diamine solution; a mixture of 8.12 g formaldehyde and 14.51 g glyoxal is added dropwise to the acidic diamine solution, and then refluxed at 80° C. for 4 hours, and the solvent and unreacted monomers are removed by rotary evaporation to obtain the polyimidazole salt.

[0119] A composite solid electrolyte membrane for a lithium battery and a preparation method thereof, comprising the following steps:

[0120] By mass, 100 parts of polyvinylidene fluoride and 600 parts of acetone solution are mixed, and stirred at 55°C until polyvinylidene fluoride is dissolved in acetone to form a transparent sol. After 0.5h, 12 parts of lithium salt and 30 parts of polyimidazole salt are added to the polyvinylidene fluoride sol, and ultrasonic stirring is continued for 0.5h. Then a certain amount of porogen dimethyl carbonate is added, and after mixing evenly, constant temperature stirring is continued to react for 6h to obtain a uniform and transparent casting liquid. After cooling to room temperature, it is scraped to form a film, the film is peeled off, and dried at 90°C for 36h to obtain the composite solid electrolyte membrane for the lithium battery.

[0121] The ultrasonic power is 600W and the frequency is 60kHz.

[0122] Comparative Example 3

[0123] A composite solid electrolyte membrane for a lithium battery consists of the following components, measured by mass: 100 parts of a polymer matrix, 12 parts of a lithium salt, and 14 parts of a modified mesoporous molecular sieve.

[0124] The polymer matrix is ​​polyvinylidene fluoride.

[0125] The lithium salt is lithium tetrafluoroborate.

[0126] The preparation method of the modified mesoporous molecular sieve comprises the following steps:

[0127] S1. Add mesoporous molecular sieve into 10mmol / L Tris buffer solution, disperse evenly by ultrasonic treatment, and obtain mesoporous molecular sieve suspension;

[0128] S2: adding dopamine to the mesoporous molecular sieve suspension obtained in step S1 to obtain a precursor suspension, stirring at 45° C. for 7 hours, filtering, washing, and drying to obtain a modified mesoporous molecular sieve.

[0129] The ultrasonic power is 600W and the frequency is 60kHz.

[0130] The concentration of dopamine in the precursor suspension is 20 mmol / L, and the mass volume ratio of the added amount of the mesoporous molecular sieve to the Tris buffer solution is 1 g:10 L.

[0131] A composite solid electrolyte membrane for a lithium battery and a preparation method thereof, comprising the following steps:

[0132] By mass, 100 parts of polyvinylidene fluoride and 600 parts of acetone solution are mixed, and stirred at 55°C until the polyvinylidene fluoride is dissolved in acetone to form a transparent sol. After 0.5h, 12 parts of lithium salt and 30 parts of modified mesoporous molecular sieves are added to the polyvinylidene fluoride sol, and ultrasonic stirring is continued for 0.5h. Then a certain amount of porogen dimethyl carbonate is added, and after mixing evenly, constant temperature stirring is continued to react for 6h to obtain a uniform and transparent casting liquid. After cooling to room temperature, it is scraped to form a film, the film is peeled off, and dried at 90°C for 36h to obtain the composite solid electrolyte membrane for the lithium battery.

[0133] The ultrasonic power is 600W and the frequency is 60kHz.

[0134] Comparative Example 4

[0135] A composite solid electrolyte membrane for a lithium battery consists of the following components, measured by mass: 100 parts of a polymer matrix, 12 parts of a lithium salt, 16 parts of a polyimidazole salt, and 14 parts of a mesoporous molecular sieve.

[0136] The polymer matrix is ​​polyvinylidene fluoride.

[0137] The lithium salt is lithium tetrafluoroborate.

[0138] The preparation method of the polyimidazole salt comprises the following steps:

[0139] 100 mmol 1,8-diaminooctane and 25 mL water are mixed and placed in an ice water bath for cooling to obtain a mixed solution; 25 mL 37 wt % aqueous hydrochloric acid solution is added to the mixed solution to obtain an acidic diamine solution; a mixture of 8.12 g formaldehyde and 14.51 g glyoxal is added dropwise to the acidic diamine solution, and then refluxed at 80° C. for 4 hours, and the solvent and unreacted monomers are removed by rotary evaporation to obtain the polyimidazole salt.

[0140] A composite solid electrolyte membrane for a lithium battery and a preparation method thereof, comprising the following steps:

[0141] By mass, 100 parts of polyvinylidene fluoride and 600 parts of acetone solution are mixed, and stirred at 55°C until the polyvinylidene fluoride is dissolved in acetone to form a transparent sol. After 0.5h, 12 parts of lithium salt, 16 parts of polyimidazole salt, and 14 parts of mesoporous molecular sieve are added to the polyvinylidene fluoride sol, and ultrasonic stirring is continued for 0.5h. Then a certain amount of porogen dimethyl carbonate is added, and after mixing evenly, constant temperature stirring is continued to react for 6h to obtain a uniform and transparent casting solution. After cooling to room temperature, it is scraped to form a film, the film is peeled off, and dried at 90°C for 36h to obtain the composite solid electrolyte membrane for the lithium battery.

[0142] The ultrasonic power is 600W and the frequency is 60kHz.

[0143] Test Example 1

[0144] The composite solid electrolyte membrane for lithium batteries was placed between stainless steel electrodes, and then the ionic conductivity (δ) was measured by AC impedance measurement in the frequency band of 100 MHz to 0.1 Hz using a VMP3 measuring device and 4294 (δ = l / (R×A), δ is the ionic conductivity (mS / cm), l is the thickness of the electrolyte (cm), R is the measured resistance (mS), and A is the area of ​​the electrolyte (cm 2 ))

[0145] Table 1: Ionic conductivity test results

[0146] Ionic conductivity (mS / cm) Example 1 0.88 Example 2 0.86 Example 3 0.83 Example 4 0.71 Example 5 0.62 Comparative Example 1 0.34 Comparative Example 2 0.67 Comparative Example 3 0.64 Comparative Example 4 0.72

[0147] Test Example 2

[0148] The tensile properties of the composite solid electrolyte membrane for lithium batteries prepared in the examples were measured with reference to GB / T 1040.2-2006 "Determination of tensile properties of plastics Part 2: Test conditions for molded and extruded plastics". The test instrument was a universal tensile testing machine. The test conditions were at 25°C, the tensile rate was 15mm / min, and each sample was tested more than 5 times. Before the test, the prepared samples were left at room temperature of 25°C for more than 48 hours. The results are shown in Table 3.

[0149] Table 3: Tensile strength test results

[0150] Tensile strength / MPa Example 1 7.3 Example 2 7.4 Example 3 8.9 Example 4 9.0 Example 5 9.1 Comparative Example 1 3.4 Comparative Example 2 5.1 Comparative Example 3 4.5 Comparative Example 4 8.1

[0151] It can be seen from Table 1 and Table 2 that the composite solid electrolyte membrane for lithium battery prepared in Example 3 of the present invention has similar ions to those in Examples 2 and 3, and similar flexibility to those in Examples 4 and 5, and has the advantages of both.

[0152] As can be seen from the comparison of Examples 1-5, polyimidazolates have a greater impact on the ionic conductivity and flexibility of the composite solid electrolyte membrane for lithium batteries, and the length of the main chain carbon chain is a key factor affecting ionic conductivity and flexibility. Longer carbon chains can better enhance the flexibility, high temperature resistance and corrosion resistance of the electrolyte membrane, but longer carbon chains are not conducive to ion conduction, which can reduce the ionic conductivity of the electrolyte membrane, and when the carbon chain is shorter, the addition of polyimidazolates reduces the toughness of the electrolyte membrane, showing more obvious brittleness, making the electrolyte membrane prone to cracking or fracture in actual use. This may affect the mechanical stability and life of the electrolyte membrane. The polyimidazolates with eight carbon atoms length synthesized with 1,8-diaminooctane as raw material have excellent flexibility, high temperature resistance and corrosion resistance, and are also less influential on the ionic conductivity of the electrolyte membrane.

[0153] It can be seen from the comparison of comparative examples 1-4 and embodiment 3 that polyimidazole salts and modified mesoporous molecular sieves have a greater impact on the ionic conductivity and flexibility of composite solid electrolyte membranes for lithium batteries. When the two are not added, comparative example 1 shows extremely poor ionic conductivity and flexibility, which greatly limits the scope of application and service life of the electrolyte membrane. However, when a single polyimidazole salt or modified mesoporous molecular sieve is added, its ionic conductivity and mechanical properties are much worse than adding both at the same time. When the added mesoporous molecular sieve mass fraction is too high, a dense network structure cannot be formed between the polymer chains, the molecular sieve cannot be wrapped in the network structure, and the molecular sieve is easily agglomerated when added too much, which does not play a reinforcing role, resulting in a decrease in the mechanical strength of the film. Polyimidazole salts are limited to their own properties, and they are limited to improving the toughness of polyvinylidene fluoride. The content of polyimidazole salts is too high, and its molecular arrangement is chaotic, which not only increases its brittleness, but also blocks the ion transmission channel, resulting in a decrease in conductivity. Therefore, when the two are combined and the appropriate amount of addition is screened out through experiments, a synergistic effect can be achieved, while enhancing the ionic conductivity and flexibility of the electrolyte membrane, and improving the service life and application range of the electrolyte membrane.

Claims

1. A composite solid electrolyte membrane for a lithium battery, characterized in that: The invention comprises the following components: polymer matrix, lithium salt, polyimidazole salt and modified mesoporous molecular sieve.

2. The composite solid electrolyte membrane for lithium battery according to claim 1, characterized in that: The polymer matrix is ​​a polymer electrolyte commonly used in the art, and can be selected from at least one of polyethylene oxide, polyacrylonitrile, polyvinylidene fluoride, polycarbonate, and polyacrylate.

3. The composite solid electrolyte membrane for lithium battery according to claim 1, characterized in that The lithium salt is at least one of lithium perchlorate, lithium hexafluorophosphate, lithium difluorooxalatoborate, lithium trifluoromethanesulfonate, lithium bis(trifluoromethanesulfonyl imide), lithium tetrafluoroborate, lithium dioxalatoborate, and lithium nitrate.

4. The composite solid electrolyte membrane for lithium battery according to claim 1, characterized in that The polyimidazolium salt is a main chain alkylated polyimidazolium salt, and the main chain thereof is composed of imidazole groups and alkyl groups alternately.

5. The composite solid electrolyte membrane for lithium battery according to claim 4, characterized in that The preparation method of the polyimidazole salt comprises the following steps: 90-110 mmol of a diamine and 20-30 mL of water are mixed and placed in an ice water bath for cooling to obtain a mixed solution; 20-30 mL of a 37 wt% aqueous hydrochloric acid solution is added to the mixed solution to obtain an acidic diamine solution; a mixture of 8-9 g of formaldehyde and 14-15 g of glyoxal is added dropwise to the acidic diamine solution, and then refluxed at 75-85° C. for 4-5 hours, and the solvent and unreacted monomers are removed by rotary evaporation to obtain the polyimidazole salt.

6. The composite solid electrolyte membrane for lithium battery according to claim 5, characterized in that The diamine is one of 1,4-diaminobutane, 1,6-diaminohexane, 1,8-diaminooctane, 1,10-diaminodecane and 1,12-diaminododecane.

7. The composite solid electrolyte membrane for lithium battery according to claim 1, characterized in that The preparation method of the modified mesoporous molecular sieve comprises the following steps: S1. Add mesoporous molecular sieve into 9-11 mmol / L Tris buffer solution, and disperse it evenly by ultrasonic treatment to obtain a mesoporous molecular sieve suspension; S2: adding dopamine to the mesoporous molecular sieve suspension obtained in step S1 to obtain a precursor suspension, stirring at 40-50° C. for 6-8 hours, filtering, washing and drying to obtain a modified mesoporous molecular sieve.

8. The composite solid electrolyte membrane for lithium battery according to claim 7, characterized in that: The concentration of dopamine in the precursor suspension is 10-30 mmol / L, and the mass volume ratio of the added amount of the mesoporous molecular sieve to the Tris buffer solution is 1 g: (5-20) L.

9. A composite solid electrolyte membrane for lithium battery and a preparation method thereof, characterized in that: The following steps are involved: The polyvinylidene fluoride and acetone solution are mixed, and stirred at 50-60°C until the polyvinylidene fluoride is dissolved in the acetone to form a transparent sol. After 0.5-1h, lithium salt, polyimidazole salt, and modified mesoporous molecular sieve are added to the polyvinylidene fluoride sol, and ultrasonic stirring is continued for 0.5-1h. Then a certain amount of porogen dimethyl carbonate is added, and after mixing evenly, constant temperature stirring is continued to react for 4-8h to obtain a uniform and transparent casting solution. After cooling to room temperature, the solution is scraped to form a film, the film is peeled off, and the film is dried at 80-90°C for 24-36h to obtain the composite solid electrolyte membrane for the lithium battery.

Citation Information

Patent Citations

  • Method for preparing ionic liquid plasticized composite polymer electrolyte for lithium ion battery

    CN102244293A

  • Gel polymer electrolyte and preparation method thereof

    CN103579671A

Cited By

  • Composite solid electrolyte containing oxygen-vacancy-rich filler and preparation method of composite solid electrolyte

    CN120637573A

  • Amine functionalized molecular sieve composite electrolyte membrane and preparation method and application thereof

    CN120749222A

  • An amine-functionalized molecular sieve composite electrolyte membrane, a preparation method and application thereof

    CN120749222B