Paste-mixing-free tubular positive plate power type lead-acid storage battery and manufacturing method thereof
By directly preparing the positive electrode slurry and using an anti-shedding composite back seal mechanism, the problems of equipment waste and weak back seals in lead-acid battery manufacturing are solved, achieving longer cycle life and higher battery performance, meeting national standards.
Patent Information
- Application Number
- CN202410935675.9
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Filing Date
- 2024-07-12
- Publication Date
- 2024-10-01
AI Technical Summary
The existing manufacturing process of tubular grouting positive plates for lead-acid batteries has problems such as dust pollution, noise pollution, equipment waste, secondary pollution from lead paste transfer, weak back seal and short cycle life.
The paste-free tubular positive plate manufacturing method is used to directly prepare the positive electrode slurry, and an anti-falling composite back sealing mechanism is used to simplify the process, reduce equipment usage, improve back seal stability, and enhance battery performance through multi-stage curing and drying processes.
It effectively extends the battery cycle life, reduces energy consumption, reduces equipment waste, improves the initial performance and cycle durability of the battery, and meets and exceeds national standard requirements.
Smart Images

Figure CN118738592A_ABST
Abstract
Description
Technical Field
[0001] The invention relates to the technical field of power type lead acid storage batteries, in particular to a paste-free tubular positive plate power type lead acid storage battery and a manufacturing method thereof. Background Art
[0002] The manufacturing process of tubular grouting positive plates for lead-acid batteries solves the problems of dust pollution and noise pollution in the manufacturing of tubular powder-filled positive plates. The equipment has a high degree of automation, and the manufactured power lead-acid batteries have the advantages of good consistency, high specific energy, and long life. While meeting the requirements of industry access conditions, it reduces manufacturing costs, improves the working environment, enhances product performance, and improves the competitiveness of lead-acid batteries.
[0003] The general process of tubular cathode grouting is to prepare a paste with an apparent density of 4.0 to 4.5 g / cm in a paste mixing machine. 3 The positive lead paste is then transferred to the pulping equipment and diluted with a large amount of pure water to an apparent density of 1.8 to 2.0 g / cm 3 , used for tubular grouting positive plate manufacturing. This grouting method has the following disadvantages: first prepare the positive lead paste, then make the pulp, the process is cumbersome; both the paste mixing machine and the pulping equipment are needed, resulting in equipment waste; there is a problem of secondary pollution during the lead paste transfer process.
[0004] There are two commonly used bottom sealing methods. One is automatic bottom sealing by ultrasonic welding. As the battery charge and discharge cycle progresses, there is a risk of the welding part falling off, which causes the cycle life to end prematurely. The other is manual bottom sealing, which can easily lead to problems such as bottom sealing not being in place and curling during operation, which will affect the cycle life of the battery. The moisture content of the grouting positive plate is between 10% and 20%, and high temperature and high humidity or normal temperature and high humidity curing is usually used. The high temperature and high humidity curing method has high energy consumption, and the initial capacity difference between single cells is obvious; the normal temperature and high humidity curing time is long and the efficiency is low. Summary of the invention
[0005] In view of the deficiencies in the prior art, the purpose of the present invention is to provide a paste-free tubular positive plate power lead-acid battery, which can delay the falling off of the bottom seal of the positive electrode tube and obtain a longer cycle life.
[0006] The present invention also provides a preparation method thereof, which eliminates the lead paste preparation process and directly makes pulp, thereby simplifying the process flow and effectively reducing the equipment required for manufacturing grouting-type tubular lead-acid batteries.
[0007] The method for manufacturing a paste-free tubular positive plate power type lead-acid battery of the present invention comprises the following steps:
[0008] 1) preparing positive electrode slurry: adding pure water to the slurry tank for the first time, and then adding the fully mixed lead-containing powder at a rate of 30 to 50 kg / min, stirring while adding; after the lead-containing powder is added and stirred evenly, adding sulfuric acid solution at a rate of 10 to 20 kg / min and stirring evenly, and finally adding pure water for the second time to adjust to the apparent density, thus obtaining the positive electrode slurry;
[0009] 2) Preparing positive electrode plates: adopting wet filling, using a pressure pump to pour the positive electrode slurry into the positive electrode tube (1) until it is full, using an anti-shedding composite bottom seal to seal the bottom, and after curing and drying, obtaining a positive electrode plate;
[0010] 3) Preparing the negative electrode plate: applying the negative electrode lead paste to the negative grid, with the coating amount being 9 to 15 g / piece, and then curing and drying to obtain the negative electrode plate;
[0011] 4) Preparation of power type lead-acid battery: Assemble the positive electrode plate and the negative electrode plate into a pole group and put them into the slot, seal the battery shell cover by heat melting, press in the sealing ring, cover the liquid injection cap, and charge by acid circulation formation to obtain a power type lead-acid battery.
[0012] Step 1) The lead-containing powder is one or both of lead powder and lead tetroxide. Preferably, the lead powder is Barton lead powder with an oxidation degree of 70-80%; and the purity of lead tetroxide is not less than 90%.
[0013] Step 1) The concentration of the sulfuric acid solution is 1.3-1.5 g / cm 3 The amount of lead powder added is 0-16% of the total mass of the lead powder, and the apparent density is 1.6-2.8 g / cm 3 .
[0014] The amount of pure water added for the first time in step 1) is 35-75% of the total mass of the lead-containing powder.
[0015] Step 2) The curing process is a multi-stage curing process:
[0016] Curing stage 1: relative humidity 95%, 30°C, 1h;
[0017] Curing stage 2: relative humidity 90%, 35°C, 1h;
[0018] Three stages of curing: relative humidity 85%, 40°C, 1h;
[0019] Four curing stages: relative humidity 80%, 45°C, 1h;
[0020] Five curing stages: relative humidity 75%, 50°C, 1h;
[0021] Six curing stages: relative humidity 70%, 55°C, 1h;
[0022] Seven stages of curing: relative humidity 65%, 60°C, 12h;
[0023] Curing stage eight: relative humidity 50%, 65°C, 12h;
[0024] The drying process is carried out at a relative humidity of 0%, 70° C., and 18 hours.
[0025] Step 2) The anti-falling composite bottom cover comprises a bottom cover mechanism and a fixing mechanism, wherein the bottom cover mechanism comprises a base, a cylindrical inner bottom cover is arranged on the upper part of the base, a curved long strip fixing claw is arranged upward on the top of the inner bottom cover, and horizontal grooves are symmetrically arranged on both sides of the base; the fixing mechanism comprises a fixing seat, a semi-arc fixing shell is fixed on the top of the fixing seat, a protrusion is arranged on the inner side of the fixing seat, and there are two fixing mechanisms, which are symmetrically arranged.
[0026] The fixing claws at the top of the inner bottom seal are in contact with the injected positive electrode slurry inside the positive electrode tube, thereby increasing the contact area. After the slurry is subsequently solidified and dried, the fixing claws can be embedded in the solidified positive electrode slurry, making the bottom seal mechanism more secure and difficult to fall off.
[0027] The protrusions and the grooves are matched, the inner diameter of the semi-arc-shaped fixed shell is equal to the outer diameter of the positive electrode tube, and the outer diameter of the inner bottom seal is equal to the inner diameter of the positive electrode tube.
[0028] The widest outer edge of the fixing claw is smaller than or equal to the inner diameter of the positive electrode tube.
[0029] The upward retracted length of the positive lead rib at the bottom of the positive electrode tube is equal to the vertical length of the inner bottom seal plus the fixing claw. The shortened length of the positive lead rib saves costs, facilitates automatic bottom sealing, and improves bottom sealing efficiency.
[0030] Working principle: When sealing the bottom, first embed the cylindrical inner bottom seal of the bottom sealing mechanism into the inner bottom of the positive electrode tube, and then use two symmetrical fixing mechanisms. The semi-arc fixing shell of the fixing mechanism is buckled from both sides along the outer diameter of the positive electrode tube, and the protrusion on the inner side of the fixing seat is inserted into the groove of the base, thereby fixing the bottom sealing mechanism and the positive electrode tube, making it difficult for the bottom sealing mechanism to fall off from the bottom of the positive electrode tube, and the fixing claws on the top of the inner bottom seal are in contact with the injected positive electrode slurry, thereby increasing the contact area. After the subsequent slurry is cured and dried, the fixing claws can be embedded in the solidified positive electrode slurry, making the bottom sealing mechanism more firm and difficult to fall off.
[0031] Step 3) The negative electrode lead paste is prepared by mixing lead powder, sulfuric acid solution, barium sulfate, humic acid and polypropylene fiber evenly, and adding pure water to adjust the apparent density to 4.30-4.50 g / cm 3 get.
[0032] Preferably, the negative electrode lead paste comprises the following raw materials in parts by weight: 80-85 parts of lead powder, 4-6 parts of sulfuric acid solution, 0.4-0.6 parts of barium sulfate, 0.1-0.3 parts of humic acid, and 0.01-0.03 parts of polypropylene fiber; the concentration of the sulfuric acid solution is 1.3-1.5 g / cm 3 .
[0033] Step 3) The curing humidity of the curing is 90-100%, the time is 24-48 hours, and the temperature is 30-40° C.; when drying, a high-temperature rapid method is adopted, the drying temperature is 65-75° C., and the drying time is 20-24 hours.
[0034] Step 4) The total charging time is 48 to 72 hours, and the total charged amount is 7.0 to 9.0 C5.
[0035] Compared with the prior art, the present invention has the following beneficial effects:
[0036] 1. The method of the present invention does not require the use of a paste making machine, and the energy consumption is reduced by 30%; there is no need to prepare positive lead paste, and the process flow is shortened by 20%; the secondary pollution caused by the transfer of positive lead paste is avoided, and the initial performance and cycle endurance of the battery meet and exceed the requirements of the national standard (GB / T 7403.1-2018).
[0037] 2. The present invention uses an anti-falling composite bottom seal. The inner bottom seal of the bottom seal mechanism is embedded in the inner bottom of the positive electrode discharge pipe. The fixing claws are in contact with the injected positive electrode slurry, which increases the contact area. After the slurry is cured and dried, the fixing claws can be embedded in the solidified positive electrode slurry, making the bottom seal mechanism more firm and difficult to fall off.
[0038] 3. The present invention uses two symmetrical fixing mechanisms. The semi-arc fixing shells of the fixing mechanisms are buckled from both sides along the outer diameter of the positive electrode tube. The protrusions on the inner side of the fixing seat are inserted into the grooves of the base, thereby fixing the bottom sealing mechanism and the positive electrode tube. This makes it difficult for the bottom sealing mechanism to fall off from the bottom of the positive electrode tube, delaying the falling of active substances at the bottom sealing position, and obtaining a longer cycle life.
[0039] 4. The anti-falling composite bottom cover of the present invention adopts two semi-arc fixing shells to buckle and fix from both sides. Compared with the integrally formed hollow frustum-shaped bottom cover, the bottom cover process will not cause problems such as the bottom cover not being in place and curling, and the qualified rate of the bottom cover is high. BRIEF DESCRIPTION OF THE DRAWINGS
[0040] Figure 1 It is a schematic diagram of the three-dimensional structure of the anti-falling composite bottom cover of the present invention;
[0041] Figure 2 This is a schematic diagram of the common back cover structure described in Comparative Example 2 of the present invention;
[0042] In the figure:
[0043] 1. Positive electrode tube; 2. Base; 3. Groove; 4. Inner bottom seal; 5. Fixing claw; 6. Semi-arc fixing shell; 7. Fixing seat; 8. Protrusion. DETAILED DESCRIPTION
[0044] The present invention is further described below in conjunction with embodiments, but the protection scope of the present invention is not limited thereto.
[0045] Unless otherwise specified, all raw materials used in the examples are commercially available.
[0046] Patton lead powder, oxidation degree 75%;
[0047] Lead tetroxide, with a purity greater than 90%, was purchased from Linzi Qile Industry and Trade Company in Zibo City.
[0048] Example 1
[0049] like Figure 1 As shown, the anti-falling composite bottom cover comprises a bottom cover mechanism and a fixing mechanism, wherein the bottom cover mechanism comprises a base 2, a cylindrical inner bottom cover 4 is provided on the upper part of the base 2, a curved long strip fixing claw 5 is provided on the top of the inner bottom cover 4, and horizontal grooves 3 are symmetrically provided on both sides of the base 2; the fixing mechanism comprises a fixing seat 7, a semi-arc fixing shell 6 is fixed on the top of the fixing seat 7, a protrusion 8 is provided on the inner side of the fixing seat 7, and there are two fixing mechanisms, which are symmetrically arranged.
[0050] The protrusion 8 and the groove 3 are matched, the inner diameter of the semi-arc-shaped fixed shell 6 is equal to the outer diameter of the positive electrode tube 1 , and the outer diameter of the inner bottom seal 4 is equal to the inner diameter of the positive electrode tube 1 .
[0051] The widest outer edge of the fixing claw 5 is smaller than or equal to the inner diameter of the positive electrode tube 1 .
[0052] The upwardly retracted length of the positive lead rib at the bottom of the positive electrode tube 1 is equal to the vertical length of the inner bottom seal 4 plus the fixing claw 5 .
[0053] Working principle: When sealing the bottom, first embed the cylindrical inner bottom seal 4 of the bottom sealing mechanism into the inner bottom of the positive electrode tube 1, and then use two symmetrical fixing mechanisms. The semi-arc fixing shell 6 of the fixing mechanism is buckled from both sides along the outer diameter of the positive electrode tube 1, and the protrusion 8 on the inner side of the fixing seat 7 is inserted into the groove of the base 2, thereby fixing the bottom sealing mechanism and the positive electrode tube 1, making it difficult for the bottom sealing mechanism to fall off from the bottom of the positive electrode tube, and the fixing claw 5 on the top of the inner bottom seal 4 is in contact with the injected positive electrode slurry, thereby increasing the contact area. After the subsequent slurry is cured and dried, the fixing claw 5 can be embedded in the cured positive electrode slurry, making the bottom sealing mechanism more firm and difficult to fall off.
[0054] Example 2
[0055] The method for manufacturing the paste-free tubular positive plate power type lead-acid battery (model 5PzS350) comprises the following steps:
[0056] 1) Preparation of positive electrode slurry: Add 70 kg of pure water to the slurry tank, then add 100 kg of fully mixed lead powder (the mass ratio of Barton lead powder and lead tetroxide is 1:1) at a rate of 40 kg / min, stirring while adding until it is evenly stirred; after the lead powder is added and stirred evenly, add 1.3 g / cm2 of 16% of the mass of the lead powder at a rate of 15 kg / min. 3 Sulfuric acid solution and stir evenly, and finally add pure water to adjust the apparent density to 1.60g / cm 3 , that is, the positive electrode slurry is obtained;
[0057] 2) Preparation of positive electrode plates: adopting wet filling, using a pressure pump to pour the positive electrode slurry into the positive electrode tube 1 until it is full, using an anti-shedding composite bottom seal to seal the bottom, and after curing and drying, obtain the positive electrode plate;
[0058] 3) Preparation of negative electrode plate: 80 parts of Barton lead powder, 0.6 parts of barium sulfate, 0.1 parts of humic acid, and 0.03 parts of polypropylene fiber were mixed evenly by weight, and pure water accounting for 8% of the above raw materials was added and stirred evenly, and then 4 parts of 1.3g / cm 3 The sulfuric acid solution was stirred evenly, and then pure water was added to adjust the apparent density to 4.30 g / cm 3 , and the negative lead paste is obtained; the negative lead paste is applied to the negative grid, and the coating amount is 13g / sheet, and then cured at a humidity of 90% and a temperature of 30°C for 24h, and then dried at a temperature of 70°C for 20h to obtain a negative green plate;
[0059] 4) Preparation of power lead-acid battery: Assemble the positive electrode plate and the negative electrode plate into a pole group and put them into the slot, seal the battery shell cover by heat melting, press in the sealing ring, cover the liquid filling cap, and charge by acid circulation formation. The total charging time is 48h and the total charged amount is 7.0C5 to obtain a power lead-acid battery.
[0060] Step 2) The curing process is a multi-stage curing process:
[0061] Curing stage 1: relative humidity 95%, 30°C, 1h;
[0062] Curing stage 2: relative humidity 90%, 35°C, 1h;
[0063] Three stages of curing: relative humidity 85%, 40°C, 1h;
[0064] Four curing stages: relative humidity 80%, 45°C, 1h;
[0065] Five curing stages: relative humidity 75%, 50°C, 1h;
[0066] Six curing stages: relative humidity 70%, 55°C, 1h;
[0067] Seven stages of curing: relative humidity 65%, 60°C, 12h;
[0068] Curing stage eight: relative humidity 50%, 65°C, 12h;
[0069] The drying process is carried out at a relative humidity of 0%, 70° C., and 18 hours.
[0070] After testing, the power lead-acid battery prepared in this embodiment has an initial capacity of up to 108%, a high-rate discharge performance of 34 minutes, and a cycle endurance of ≥1250 times. The main performance of the battery meets the national standard requirements, and the cycle endurance is significantly improved.
[0071] Example 3
[0072] The method for manufacturing the paste-free tubular positive plate power type lead-acid battery (model 5PzS350) comprises the following steps:
[0073] 1) Preparation of positive electrode slurry: Add 55 kg of pure water to the slurry tank, then add 100 kg of fully mixed lead powder (Barton lead powder) at a rate of 40 kg / min, stirring while adding until it is evenly mixed; after the lead powder is added and stirred evenly, add 1.5 g / cm2 of 6% of the mass of the lead powder at a rate of 15 kg / min. 3 Sulfuric acid solution and stir evenly, and finally add pure water to adjust the apparent density to 2.20g / cm 3 , that is, the positive electrode slurry is obtained;
[0074] 2) Preparation of positive electrode plates: adopting wet filling, using a pressure pump to pour the positive electrode slurry into the positive electrode tube 1 until it is full, using an anti-shedding composite bottom seal to seal the bottom, and after curing and drying, obtain the positive electrode plate;
[0075] 3) Preparation of negative electrode plate: 80 parts of lead powder, 0.6 parts of barium sulfate, 0.1 parts of humic acid, and 0.03 parts of polypropylene fiber were mixed evenly by weight, and pure water accounting for 8% of the above raw materials was added and stirred evenly, and then 4 parts of 1.3g / cm 3 The sulfuric acid solution was stirred evenly, and then pure water was added to adjust the apparent density to 4.30 g / cm 3 , and the negative lead paste is obtained; the negative lead paste is applied to the negative grid, and the coating amount is 13g / sheet, and then cured at a humidity of 90% and a temperature of 30°C for 24h, and then dried at a temperature of 70°C for 20h to obtain a negative green plate;
[0076] 4) Preparation of power lead-acid battery: Assemble the positive electrode plate and the negative electrode plate into a pole group and put them into the slot, seal the battery shell cover by heat melting, press in the sealing ring, cover the liquid filling cap, and charge by acid circulation formation. The total charging time is 60h and the total charged amount is 8.0C5 to obtain a power lead-acid battery.
[0077] Step 2) The curing process is a multi-stage curing process:
[0078] Curing stage 1: relative humidity 95%, 30°C, 1h;
[0079] Curing stage 2: relative humidity 90%, 35°C, 1h;
[0080] Three stages of curing: relative humidity 85%, 40°C, 1h;
[0081] Four curing stages: relative humidity 80%, 45°C, 1h;
[0082] Five curing stages: relative humidity 75%, 50°C, 1h;
[0083] Six curing stages: relative humidity 70%, 55°C, 1h;
[0084] Seven stages of curing: relative humidity 65%, 60°C, 12h;
[0085] Curing stage eight: relative humidity 50%, 65°C, 12h;
[0086] The drying process is carried out at a relative humidity of 0%, 70° C., and 18 hours.
[0087] After testing, the power lead-acid battery prepared in this embodiment has an initial capacity of up to 110%, a high-rate discharge performance of 37 minutes, and a cycle endurance of ≥1350 times. The main performance of the battery meets the national standard requirements, and the cycle endurance is significantly improved.
[0088] Example 4
[0089] The method for manufacturing the paste-free tubular positive plate power type lead-acid battery (model 5PzS350) comprises the following steps:
[0090] 1) Prepare positive electrode slurry: add 40 kg of pure water into the slurry tank and stir continuously, then add 100 kg of fully mixed lead powder (lead tetroxide) at a rate of 40 kg / min, stir while adding, and stir until it is evenly mixed; after the lead powder is added and stirred evenly, finally add pure water to adjust the apparent density to 2.80 g / cm 3 , that is, the positive electrode slurry is obtained;
[0091] 2) Preparation of positive electrode plates: adopting wet filling, using a pressure pump to pour the positive electrode slurry into the positive electrode tube 1 until it is full, using an anti-shedding composite bottom seal to seal the bottom, and after curing and drying, obtain the positive electrode plate;
[0092] 3) Preparation of negative electrode plate: 80 parts of lead powder, 0.6 parts of barium sulfate, 0.1 parts of humic acid, and 0.03 parts of polypropylene fiber were mixed evenly by weight, and pure water accounting for 8% of the above raw materials was added and stirred evenly, and then 4 parts of 1.3g / cm 3 The sulfuric acid solution was stirred evenly, and then pure water was added to adjust the apparent density to 4.30 g / cm 3 , and the negative lead paste is obtained; the negative lead paste is applied to the negative grid, and the coating amount is 13g / sheet, and then cured at a humidity of 90% and a temperature of 30°C for 24h, and then dried at a temperature of 70°C for 20h to obtain a negative green plate;
[0093] 4) Preparation of power lead-acid battery: Assemble the positive electrode plate and the negative electrode plate into a pole group and put them into the slot, seal the battery shell cover by heat melting, press in the sealing ring, cover the liquid filling cap, and charge by acid circulation formation. The total charging time is 60h and the total charged amount is 8.0C5 to obtain a power lead-acid battery.
[0094] Step 2) The curing process is a multi-stage curing process:
[0095] Curing stage 1: relative humidity 95%, 30°C, 1h;
[0096] Curing stage 2: relative humidity 90%, 35°C, 1h;
[0097] Three stages of curing: relative humidity 85%, 40°C, 1h;
[0098] Four curing stages: relative humidity 80%, 45°C, 1h;
[0099] Five curing stages: relative humidity 75%, 50°C, 1h;
[0100] Six curing stages: relative humidity 70%, 55°C, 1h;
[0101] Seven stages of curing: relative humidity 65%, 60°C, 12h;
[0102] Curing stage eight: relative humidity 50%, 65°C, 12h;
[0103] The drying process is carried out at a relative humidity of 0%, 70° C., and 18 hours.
[0104] After testing, the power lead-acid battery prepared in this embodiment has an initial capacity of up to 105%, a high-rate discharge performance of 33 minutes, and a cycle endurance of ≥1200 times. The main performance of the battery meets the national standard requirements, and the cycle endurance is significantly improved.
[0105] Example 5
[0106] The same as Example 2, except that the positive electrode plate curing method described in step 2) adopts a high temperature and high humidity (temperature 80° C., relative humidity 95%, curing time 48 hours) process.
[0107] After testing, the power lead-acid battery prepared in this embodiment has an initial capacity of up to 103%, a high-rate discharge performance of 32 minutes, and a cycle endurance of ≥1200 times. The battery performance meets the national standard requirements, but the initial capacity of the battery is significantly lower. Due to the high water content of the wet positive plate, the high-temperature and high-humidity curing process cannot ensure the consistent curing process of each plate (that is, at the end of curing, some plate lead pastes have a high free lead content and cannot be completely converted into lead dioxide during formation).
[0108] Comparative Example 1
[0109] Same as Example 2, except that conventional curing method is used:
[0110] The manufacturing method of the paste-type tubular positive plate power lead-acid battery (model 5PzS350) is as follows:
[0111] (1) Preparation of positive electrode lead paste: Add 500 kg of lead-containing powder (mixture of Barton powder and lead tetroxide) into the paste mixer and stir for 3 minutes in a dry state. Add battery water over 5 minutes and continue stirring for 3 minutes. Add sulfuric acid solution over 15 minutes and continue stirring for 20 minutes. Stir well and set aside.
[0112] (2) Preparation of positive electrode slurry: Add pure water to the slurry tank, transfer the lead paste prepared above into the slurry tank, and stir while adding. Adjust to an apparent density of 1.60 g / cm 3 , and the positive electrode slurry is obtained.
[0113] The preparation of the positive electrode plate, the negative electrode plate and the battery is the same as that in the embodiment.
[0114] In Comparative Example 1, the stirring time for preparing the positive electrode lead paste is 46 min, and the lead powder is calculated as 500 kg; the stirring time for preparing the positive electrode slurry is 20 min, and the lead paste is calculated based on the amount of lead paste prepared by 500 kg of lead powder.
[0115] The stirring time for preparing the positive electrode slurry in the embodiment is 40 min, and the lead powder is calculated as 500 kg.
[0116] The stirring time of the comparative example is 66 minutes, and the stirring time of Example 2 is 40 minutes. Roughly calculated, the energy consumption of the example is saved by more than 30% (the friction force of the dry stirring of the comparative example is large, and the energy consumption per unit time is higher. That is, the example actually saves more energy consumption).
[0117] Comparative Example 2
[0118] The same as Example 2, except that the positive electrode plate back cover adopts the common back cover of ultrasonic welding, and its structure is as follows: Figure 2 As shown, after the bottom is sealed, the bottom is welded and fixed.
[0119] After testing, the power lead-acid battery prepared in this comparative example has a maximum initial capacity of 107%, a high rate discharge performance of 35min, and a cycle durability of ≥1000 times. The battery performance meets the national standard requirements, but the cycle durability of the battery in this comparative example is significantly lower than that in Example 2. The reason for the termination of the cycle durability is the fall-off of the bottom cover and the loss of active substances.
Claims
1. A method for manufacturing a paste-free tubular positive plate power lead-acid battery, characterized in that: The following steps are involved: 1) preparing positive electrode slurry: adding pure water to the slurry tank for the first time, and then adding the fully mixed lead-containing powder at a rate of 30 to 50 kg / min, stirring while adding; after the lead-containing powder is added and stirred evenly, adding sulfuric acid solution at a rate of 10 to 20 kg / min and stirring evenly, and finally adding pure water for the second time to adjust to the apparent density, thus obtaining the positive electrode slurry; 2) Preparing positive electrode plates: adopting wet filling, using a pressure pump to pour the positive electrode slurry into the positive electrode tube (1) until it is full, using an anti-shedding composite bottom seal to seal the bottom, and after curing and drying, obtaining a positive electrode plate; 3) preparing the negative electrode plate: applying the negative electrode lead paste to the negative grid, and then curing and drying to obtain the negative electrode plate; 4) Preparation of power type lead-acid battery: Assemble the positive electrode plate and the negative electrode plate into a pole group and put them into the slot, seal the battery shell cover by heat melting, press in the sealing ring, cover the liquid injection cap, and charge by acid circulation formation to obtain a power type lead-acid battery.
2. The method for manufacturing a paste-free tubular positive plate power type lead-acid battery according to claim 1, characterized in that: In step 1), the lead-containing powder is one or both of lead powder and lead tetroxide.
3. The method for manufacturing a paste-free tubular positive plate power type lead-acid battery according to claim 1, characterized in that: Step 1) The concentration of the sulfuric acid solution is 1.3-1.5 g / cm 3 The amount of lead powder added is 0-16% of the total mass of the lead powder, and the apparent density is 1.6-2.8 g / cm 3 .
4. The method for manufacturing a paste-free tubular positive plate power type lead-acid battery according to claim 1, characterized in that: The amount of pure water added for the first time in step 1) is 35-75% of the total mass of the lead-containing powder.
5. The method for manufacturing a paste-free tubular positive plate power type lead-acid battery according to claim 1, characterized in that: Step 2) The curing process is a multi-stage curing process: Curing stage 1: relative humidity 95%, 30°C, 1h; Curing stage 2: relative humidity 90%, 35°C, 1h; Three stages of curing: relative humidity 85%, 40°C, 1h; Four curing stages: relative humidity 80%, 45°C, 1h; Five curing stages: relative humidity 75%, 50°C, 1h; Six curing stages: relative humidity 70%, 55°C, 1h; Seven stages of curing: relative humidity 65%, 60°C, 12h; Curing stage eight: relative humidity 50%, 65°C, 12h; The drying process is carried out at a relative humidity of 0%, 70° C., and 18 hours.
6. The method for manufacturing a paste-free tubular positive plate power type lead-acid battery according to claim 1, characterized in that: Step 2) The anti-falling composite bottom seal comprises a bottom seal mechanism and a fixing mechanism, wherein the bottom seal mechanism comprises a base (2), a cylindrical inner bottom seal (4) is provided on the upper part of the base (2), a curved long strip fixing claw (5) is provided on the top of the inner bottom seal (4), and horizontal grooves (3) are symmetrically provided on both sides of the base (2); the fixing mechanism comprises a fixing seat (7), a semi-arc fixing shell (6) is fixed on the top of the fixing seat (7), a protrusion (8) is provided on the inner side of the fixing seat (7), and there are two fixing mechanisms, which are symmetrically arranged.
7. The method for manufacturing a paste-free tubular positive plate power type lead-acid battery according to claim 6, characterized in that: The protrusion (8) and the groove (3) are matched, the inner diameter of the semi-arc-shaped fixed shell (6) is equal to the outer diameter of the positive electrode tube (1), and the outer diameter of the inner bottom seal (4) is equal to the inner diameter of the positive electrode tube (1).
8. The method for manufacturing a paste-free tubular positive plate power type lead-acid battery according to claim 6, characterized in that: The widest outer edge of the fixing claw (5) is smaller than or equal to the inner diameter of the positive electrode tube (1).
9. The method for manufacturing a paste-free tubular positive plate power type lead-acid battery according to claim 1, characterized in that: The upwardly retracted length of the positive lead rib at the inner bottom of the positive electrode tube (1) is equal to the vertical length of the inner bottom seal (4) plus the fixing claw (5).
10. A paste-free tubular positive plate power lead-acid battery, characterized in that: The invention is prepared by the manufacturing method according to any one of claims 1 to 9.
Citation Information
Cited By
High-power dynamic lead-acid storage battery and manufacturing method thereof
CN119725791A
High-power motive lead-acid battery and its manufacturing method
CN119725791B
Lead-acid storage battery and acid cycle equalization formation charging method thereof
CN121584050A