High-open-voltage trans-perovskite battery based on polyhydroxy aluminum glycinate and preparation method of high-open-voltage trans-perovskite battery
By using polyhydroxy aluminum glycinate modified materials in trans perovskite solar cells, the polarity and spreadability problems of the self-assembled hole transport layer are solved, the interface defect density and stress are reduced, and the charge carrier transport performance is improved and battery stability, achieving more efficient photoelectric conversion efficiency and long-term stability.
Patent Information
- Application Number
- CN202410872673.X
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Filing Date
- 2024-07-01
- Publication Date
- 2024-10-01
AI Technical Summary
Existing trans perovskite solar cells based on self-assembled organic hole transport layers have problems such as large surface polarity, poor perovskite spreadability, high interface defect density, and inability to effectively release interface stress, resulting in low perovskite cell efficiency. It is difficult to break through to the commercial level in long-term operation.
Polyhydroxy aluminum glycinate (AG) is used as the modification material. Through interaction with the NiOx layer and the perovskite layer, it inhibits the self-polymerization of the SAM material, forms a low-defect charge transport layer, and promotes the growth of perovskite crystals. , and release the interface residual stress and improve the charge carrier transport performance.
Significantly reduces the charge carrier transport barrier, improves charge carrier transport and extraction efficiency, enhances the interface compatibility between the perovskite layer and the transport layer, increases the open circuit voltage and filling factor of the battery, and extends the battery life. Battery stability.
Smart Images

Figure CN118742166A_ABST
Abstract
Description
Technical Field
[0001] The invention belongs to the field of perovskite materials and devices, and relates to a high-opening voltage trans-perovskite battery based on polyhydroxyglycinate aluminum and a preparation method thereof. Background Art
[0002] The high-carbon economy that relies too much on traditional non-renewable fossil energy has led to serious environmental and safety issues. Solar energy has attracted widespread attention from industry and academia due to its advantages such as cleanliness, renewableness, and wide distribution. Photovoltaics (PV) is a technology that converts light energy directly into electrical energy, and its photoelectric conversion process is clean and pollution-free. Perovskite materials have the advantages of long charge carrier diffusion distance, long life, and low charge separation energy, and are widely used in the photovoltaic field. Inverted perovskite solar cells based on perovskite light-absorbing layers have the advantages of high photoelectric conversion efficiency, good stability, low preparation cost, and low hysteresis effect, and have made great progress in recent years. The laboratory photoelectric conversion efficiency of a single-cell inverse perovskite cell has increased from 3.9% in 2013 to 26.9% in 2024 (certified efficiency 26.1%), far exceeding the 26.41% (certified efficiency 26.21%) reported in the formal perovskite solar cell laboratory; after more than ten years of development, the stability of a single-cell inverse perovskite solar cell has also achieved a leap forward, and its laboratory operating stability has exceeded tens of thousands of hours.
[0003] While trans-perovskite solar cells show great application potential, the further development of trans-perovskite solar cells efficiency and stability also faces many challenges. Currently reported high-efficiency trans-perovskite solar cells are prepared based on organic self-assembled hole transport materials, but the organic self-assembled hole transport layer has the following problems:
[0004] (1) When the organic self-assembled hole transport layer is formed, the phosphoric acid molecules are prone to dehydration reactions, which reduces the ability of the SAM (Self-assembled monolayer) to bond to the conductive substrate;
[0005] (2) After the organic hole transport material is self-assembled on FTO, the polarity on its surface is relatively small, and the spreading of the highly polar perovskite precursor solution on the self-assembled hole transport layer is limited, which is not conducive to the nucleation, crystallization and growth of the perovskite film;
[0006] (3) There is a lack of interaction between the top groups of the organic self-assembled hole transport layer and the perovskite layer.
[0007] It is not conducive to the passivation of interface defects and the release of interface stress between the perovskite layer and the transport layer.
[0008] The existence of the above problems makes it difficult for the efficiency and long-term operation of perovskite batteries to reach commercial levels. Summary of the invention
[0009] The purpose of the present invention is to overcome the shortcomings of the above-mentioned prior art and provide a high-opening voltage trans perovskite cell based on polyhydroxyglycinate aluminum and a preparation method thereof, so as to solve the problems existing in the preparation of trans perovskite solar cells based on self-assembled organic hole transport layers, such as large surface polarity of the self-assembled layer, poor perovskite spreading, high interface defect density, and inability to effectively release interface stress.
[0010] In order to achieve the above object, the present invention adopts the following technical solutions:
[0011] A method for preparing a high-opening voltage inverse perovskite battery based on polyhydroxyglycinate aluminum comprises the following steps:
[0012] Step 1, pre-treating FTO glass;
[0013] Step 2: NiO X The dispersion is spin-coated on the FTO glass surface and a NiOx layer is obtained after annealing. X The dispersion is a solution prepared by dissolving NiOx powder in water;
[0014] Step 3, spin-coating the Me-4PACz solution on the NiOx layer, and obtaining the Me-4PACz layer after annealing; the solute of the Me-4PACz solution is Me-4PACz solid powder, and the solvent is isopropanol; the NiOx layer and the Me-4PACz layer constitute a charge transport layer;
[0015] Step 4, spin coating an AG solution with a concentration of 0.1-1 mg / mL on the Me-4PACz layer, and preparing an AG modified layer after annealing, wherein the AG is polyhydroxyglycinate aluminum;
[0016] Step 5: Spin-coat FA on the AG modified layer 0.9 Cs 0.1 PbI3 perovskite precursor solution is annealed to obtain a perovskite light absorbing layer;
[0017] Step 6, preparing a PDAI2 passivation layer on the perovskite light absorbing layer;
[0018] Step 7, preparing an electron transport layer on the PDAI2 passivation layer, and then preparing a hole blocking layer;
[0019] Step 8: Prepare a metal electrode on the hole blocking layer to obtain a high-opening voltage inverse perovskite cell.
[0020] A further improvement of the present invention is:
[0021] Preferably, in step 2, the concentration of the NiOx dispersion is 10 mg / mL; the spin coating speed is 2000 rpm, the spin coating time is 30 s, the annealing temperature is 120° C., and the annealing time is 20 min.
[0022] Preferably, in step 3, the concentration of the Me-4PACz solution is 0.5 mg / mL, the spin coating speed is 4000 rpm, the spin coating time is 30 s, the annealing temperature is 100° C., and the annealing time is 10 min.
[0023] Preferably, in step 4, the solute of the AG solution is polyhydroxyglycinate aluminum, and the solvent is any one of N,N-dimethylformamide, anhydrous ethanol, isopropanol or dimethyl sulfoxide.
[0024] Preferably, in step 4, the spin coating speed is 6000 rpm, the spin coating time is 20 s; the annealing temperature is 100° C., and the annealing time is 3 min.
[0025] Preferably, in step 5, the concentration of the perovskite precursor solution is 1 M, and the perovskite solution is spin-coated in two stages.
[0026] Preferably, in step 6, a PDAI2 passivation layer is prepared on the perovskite light absorbing layer by spin coating a passivation layer solution, the concentration of the passivation layer solution is 1 mg / mL, the solute is PDAI2 solid powder, and the solvent is a mixture of chlorobenzene and IPA.
[0027] Preferably, in step 7, the electron transport layer is C 60 , prepared by evaporation method.
[0028] Preferably, in step 7, the hole blocking layer is BCP, which is prepared by evaporation.
[0029] A high-opening voltage inverted perovskite battery based on polyhydroxyglycinate aluminum prepared by any of the above preparation methods, comprising FTO / NiOx / Me-4PACz / AG / PVK / PDAI2 / C from one side to the other 60 / BCP / Ag.
[0030] Compared with the prior art, the present invention has the following beneficial effects:
[0031] The invention discloses a polyhydroxyglycine aluminum buried bottom interface material and a high-opening voltage inverse perovskite battery and a preparation method. XAfter the organic hole transport layer of / Me-4PACz, aluminum glycinate was added, wherein Me-4PACz is a SAM material; aluminum glycinate (AG), as a multifunctional organic metal material rich in functional groups such as -NH2, -OH, and organic metal Al, was used for the first time to modify the organic hole transport layer interface of trans-perovskite; the modified material has the following functions:
[0032] (1) On the surface of NiOx / SAM hole transport layer, Al-OH in AG can inhibit the self-polymerization interaction between P-OH molecules on the NiOx surface of SAM material and enhance the self-assembly efficiency of SAM molecules through the interaction between Al-OH and P-OH, thereby reducing the Ni-OH defects on the NiOx surface; on the other hand, Al-OH can passivate the freely moving -OH defects on the surface of NiOx and form Ni-O-Al bonds; the above two effects are helpful to obtain a NiOx / SAM hole transport layer with low defect density, excellent charge transport performance, good surface hydrophilicity, which is conducive to the spreading of perovskite precursor solution and promotes the crystal growth of perovskite, thereby improving the charge carrier transport and extraction and reducing the non-radiative recombination of carriers.
[0033] (2) In the hole transport layer modified by AG, Al-OH can passivate the freely moving -OH defects on the surface of NiOx and form Ni-O-Al bonds. The surface conduction band and Fermi level are significantly improved, which better matches the perovskite energy level and reduces the charge carrier transport barrier.
[0034] (3) The -NH2 in AG can passivate the under-coordinated lead defects and iodine defects on the surface of the perovskite buried substrate, induce the nucleation and crystallization of perovskite, and release the residual stress at the perovskite buried substrate interface. BRIEF DESCRIPTION OF THE DRAWINGS
[0035] Figure 1 The schematic diagram of the device structure of the FACsPbI3 perovskite solar cell in Example 1 of the present invention is as follows:
[0036] From bottom to top, they are FTO layer, NiOx layer, SAM layer, lower interface modification layer, perovskite layer, upper surface passivation layer, electron transport layer, hole blocking layer, and metal electrode;
[0037] Figure 2 This is the XPS spectrum of the effect of the modification layer material AG and PbI2 in Example 1 of the present invention;
[0038] Among them, (a) is the XPS graph of PbI2; (b) is the XPS graph of PbI2+AG film;
[0039] Figure 3This is the XPS spectrum of the effect of the modification layer material AG and NiOx in Example 1 of the present invention;
[0040] Figure 4 This is a GIXRD comparison diagram of the unmodified and AG-modified perovskite layers at the lower interface in Example 1 of the present invention;
[0041] Among them, (a) shows the GIXRD spectrum of the perovskite film on the NiOx / Me-4PACz substrate;
[0042] (b) The figure shows the GIXRD spectrum of the perovskite film on the NiOx / Me-4PACz / AG substrate;
[0043] (c) The figure shows the stress simulation diagram of the perovskite film on the NiOx / Me-4PACz substrate;
[0044] (d) The figure shows the stress simulation diagram of the perovskite film on the NiOx / Me-4PACz / AG substrate;
[0045] Figure 5 UPS comparison diagram of the unmodified and AG-modified NiOx+SAM films at the lower interface in Example 1 of the present invention;
[0046] Figure 6 JV curves of the perovskite solar cell with unmodified and AG-modified lower interfaces in Example 1 of the present invention;
[0047] Figure 7 The stability of the perovskite solar cell with unmodified and AG-modified lower interface in Example 1 of the present invention. DETAILED DESCRIPTION
[0048] The present invention is further described in detail below in conjunction with the accompanying drawings:
[0049] The first aspect of the present invention discloses a method for preparing a polyhydroxyglycine aluminum buried interface material, comprising the following steps:
[0050] Step 1, cleaning FTO glass;
[0051] The 2.5×2.5cm 2 The FTO glass was cleaned with conductive glass cleaning solution, acetone, and ethanol, and then dried with a nitrogen air gun for later use.
[0052] Step 2, preparation method of NiOx and Me-4PACz;
[0053] Add 1 mL of deionized water to a glass bottle containing 10 mg of NiOx powder to prepare a 10 mg / mL NiOx dispersion, place the glass bottle in an ultrasonic cleaner, and ultrasonicate for 40 minutes to ensure that the NiOx powder is fully dispersed in the deionized water for later use. Treat the FTO glass cleaned in step 1 with ultraviolet ozone for 20 minutes, and spin-coat the 10 mg / mL NiOx dispersion on the FTO glass surface at a spin-coating speed of 2000 rpm for 30 seconds, followed by annealing at a temperature of 120°C for 20 minutes.
[0054] 1 mg Me-4PACz solid powder was dissolved in 2 mL isopropanol (IPA) to prepare a 0.5 mg / mL Me-4PACz solution, which was stirred for 5 h and then used for later use. The 0.5 mg / mL Me-4PACz solution was spin-coated on the NiOx surface at a spin-coating speed of 4000 rpm for 30 s, followed by annealing at a temperature of 100 °C for 10 min to obtain a NiOx and Me-4PACz layer.
[0055] Among them, Me-4PACz is the abbreviation of [4-(3,6-dimethyl-9H-carbazole-9-yl)butyl]phosphoric acid, which is a SAM material.
[0056] Step 3, preparing an N,N-dimethylformamide (DMF) modification layer solution of AG;
[0057] The preparation method of the AG modification layer solution is: dissolving AG solid powder in a solvent, the solvent being any one of N,N-dimethylformamide (DMF), anhydrous ethanol (EtOH), isopropyl alcohol (IPA) or dimethyl sulfoxide (DMSO), and stirring for 4 hours to obtain an AG modification layer solution with a concentration of 0.1-1 mg / mL. AG is a polyhydroxyglycine aluminum buried interface material, and its chemical structure is:
[0058]
[0059] Step 4, preparing an AG modified layer;
[0060] The DMF solution of 0.1-1 mg / mL AG prepared in step 3 was spin-coated on the NiOx / Me-4PACz surface at a spin-coating speed of 6000 rpm for 20 s, followed by an annealing process at a temperature of 100°C for 3 min to obtain an AG modified layer. In this process, the Al-OH in the AG modified layer combines with the free -OH on the NiOx surface to exist in the form of Al-O-Ni, and the -NH2 of AG interacts with the under-coordinated Pb-related defects on the surface of the perovskite buried substrate.
[0061] Step 5: Configure FA0.9 Cs 0.1 PbI3 perovskite precursor solution
[0062] Configuring FA 0.9 Cs 0.1 The process of preparing the PbI3 perovskite precursor solution is as follows: 0.9 M formamidine hydroiodide (FAI), 0.1 M cesium iodide (CsI) and 1.05 M lead iodide (PbI2) are dissolved in a mixed solvent of DMF and DMSO (V / V = 4:1) to prepare a 1 M FAI solution. 0.9 Cs 0.1 PbI3 perovskite precursor solution. The perovskite precursor solution was stirred for 6 h and then filtered using a 0.45 μm syringe for later use.
[0063] Step 6, preparing a perovskite light absorbing layer (PVK);
[0064] The perovskite precursor solution prepared in step 5 was spin-coated on the surface of the AG modified layer. The spin-coating process was divided into two stages. In the first stage, the rotation speed was 1000 rpm and the time was 8 s. In the second stage, the rotation speed was 4000 rpm and the time was 25 s. Five seconds before the end, the anti-solvent anisole was coated on the perovskite surface, followed by an annealing process at a temperature of 110 ° C and an annealing time of 20 min. After annealing, FTO / NiOx / Me-4PACz / AG / PVK was formed. The prepared perovskite light-absorbing layer was about 500 nm.
[0065] Step 7, preparing a PDAI2 passivation layer on the upper surface of the perovskite;
[0066] Dissolve 2 mg of PDAI2 solid powder in 2 mL of a mixed solvent of chlorobenzene and IPA (V / V = 4:1) to prepare a mixed solution with a concentration of 1 mg / mL, stir for 5 hours and set aside. Spin coat the prepared passivation layer solution on the perovskite surface at a spin coating speed of 4500 rpm for 25 seconds, followed by an annealing process at a temperature of 110°C for 5 minutes. The FTO / NiOx / Me-4PACz / AG / PVK / PDAI2 layer was obtained.
[0067] Step 8, preparing an electron transport layer;
[0068] The PDAI2 passivation layer on the perovskite prepared in step 7 is deposited with a thickness of 20 nm. 60 As the electron transport layer, FTO / NiOx / Me-4PACz / AG / perovskite light absorption layer / PDAI2 / C 60 .
[0069] Step 9, preparing a hole blocking layer;
[0070] The C prepared in step 8 60 The surface was evaporated with a thickness of more than 6nm BCP (bathcopper) as a hole blocking layer to prepare FTO / NiOx / Me-4PACz / AG / PVK / PDAI2 / C 60 / BCP.
[0071] Step 10, preparing a metal electrode;
[0072] Silver with a thickness of about 100 nm was evaporated on the surface of the hole blocking layer prepared in step 9 as a metal electrode, and finally a structure of FTO / NiOx / Me-4PACz / AG / PVK / PDAI2 / C was obtained. 60 / BCP / Ag organic-inorganic FACsPbI3 perovskite solar cells.
[0073] The following is further described in conjunction with specific embodiments.
[0074] Example 1
[0075] First, clean the FTO glass; 2 The FTO glass was cleaned with conductive glass cleaning solution, acetone, and ethanol, and then dried with a nitrogen air gun for later use.
[0076] Second, the preparation method of NiOx and Me-4PACz; add 1mL of deionized water to a glass bottle containing 10mg of NiOx powder to prepare a 10mg / mL NiOx dispersion, put the glass bottle into an ultrasonic cleaner, and ultrasonicate for 40min to ensure that the NiOx powder is fully dispersed in the deionized water for use. Dissolve 1mg of Me-4PACz solid powder in 2mL of isopropanol (IPA) to prepare a 0.5mg / mL solution and stir for 5h for use. Treat the FTO glass cleaned in step 1 with ultraviolet ozone for 20min. A 10 mg / mL NiOx dispersion was spin-coated on the FTO glass surface at a spin-coating speed of 2000 rpm for 30 s, followed by annealing at a temperature of 120°C for 20 min. After annealing, a 0.5 mg / mL Me-4PACz solution was spin-coated on the NiOx surface at a spin-coating speed of 4000 rpm for 30 s, followed by annealing at a temperature of 100°C for 10 min to obtain NiOx and Me-4PACz layers.
[0077] Third, prepare the N,N-dimethylformamide (DMF) modification layer solution of AG; the preparation method of the AG modification layer solution is: dissolve 2 mg of AG solid powder in 4 mL of DMF, stir for 4 hours and set aside.
[0078] Fourth, prepare the AG modified layer; spin-coat the 0.5 mg / mL AG DMF solution prepared in step 3 on the NiOx / Me-4PACz surface at a spin-coating speed of 6000 rpm for 20 s, followed by an annealing process at a temperature of 100°C for 3 min to obtain the AG modified layer.
[0079] Fifth, configure 1.0M FA 0.9 Cs 0.1 For the PbI3 perovskite precursor solution, formamidine hydroiodide (FAI), cesium iodide (CsI) and lead iodide (PbI2) were dissolved in a mixed solvent of DMF and DMSO (V / V = 4:1) in a stoichiometric ratio, stirred at room temperature for 6 h, and then filtered using a 0.45 μm syringe for later use.
[0080] Sixth, prepare the perovskite light-absorbing layer (PVK); spin-coat the perovskite precursor solution prepared in step 5 on the surface of the AG modified layer. The spin-coating process is divided into two stages. In the first stage, the rotation speed is 1000rpm and the time is 8s; in the second stage, the rotation speed is 4000rpm and the time is 25s. Five seconds before the end, the anti-solvent anisole is applied to the perovskite surface, followed by an annealing process, the annealing temperature is 110°C, and the annealing time is 20min. After annealing, FTO / NiOx / Me-4PACz / AG / PVK is formed. The prepared perovskite light-absorbing layer is about 500nm.
[0081] Seventh, prepare the PDAI2 passivation layer on the upper surface of the perovskite; dissolve 2 mg of PDAI2 solid powder in 2 mL of a mixed solvent of chlorobenzene and IPA (V / V = 4:1) to prepare a mixed solution with a concentration of 1 mg / mL, stir for 5 hours and set aside. Spin coat the prepared passivation layer solution on the upper surface of the perovskite at a spin coating speed of 4500 rpm and a spin coating time of 25 seconds, followed by an annealing process at an annealing temperature of 110°C and an annealing time of 5 minutes. The FTO / NiOx / Me-4PACz / AG / PVK / PDAI2 layer was obtained.
[0082] Eighth, prepare the electron transport layer; evaporate the PDAI2 passivation layer on the surface of the perovskite prepared in step 7 to form a C 60 As the electron transport layer, FTO / NiOx / Me-4PACz / AG / perovskite light absorption layer / PDAI2 / C 60 .
[0083] Ninth, prepare a hole blocking layer; the C prepared in step 8 60 The surface was evaporated with a thickness of more than 6nm BCP (bathcopper) as a hole blocking layer to prepare FTO / NiOx / Me-4PACz / AG / PVK / PDAI2 / C60 / BCP.
[0084] Tenth, prepare a metal electrode; evaporate silver with a thickness of about 100 nm on the surface of the hole blocking layer prepared in step 9 as a metal electrode, and finally obtain a structure of FTO / NiOx / Me-4PACz / AG / PVK / PDAI2 / C 60 / BCP / Ag organic-inorganic FACsPbI3 perovskite solar cells.
[0085] In this embodiment, a perovskite solar cell with an interface modification layer AG at 0.5 mg / mL was prepared.
[0086] like Figure 1 FA shown 0.9 Cs 0.1 The device structure of the PbI3 perovskite solar cell is, from bottom to top, FTO layer, NiOx layer, SAM layer Me-4PACz, lower interface modification layer AG, perovskite light absorption layer, upper surface passivation layer PDAI2, electron transport layer C60, hole blocking layer BCP, and metal electrode Ag.
[0087] like Figure 2 The XPS spectrum of the interaction between the modification layer material AG and PbI2 is shown. After modification by AG, Pb moves toward the direction of high binding energy and I moves toward the direction of low binding energy, which indicates that AG can passivate the under-coordinated lead defects and iodine defects on the surface of the buried perovskite.
[0088] like Figure 3 The XPS spectrum of the modified layer material AG and NiOx, Ni 3+ The peak moves toward the high energy level, which indicates that the Al-OH in AG can passivate the freely moving -OH defects on the surface of NiOx and form Ni-O-Al bonds; it is helpful to obtain high-quality NiOx / SAM charge transport layer, improve charge carrier transport and extraction, and reduce non-radiative recombination of carriers.
[0089] like Figure 4 This is the GIXRD comparison diagram of the unmodified and AG-modified perovskite layer at the lower interface. It can be seen from the figure that AG induces perovskite nucleation and crystallization, releasing the residual stress at the buried perovskite interface.
[0090] like Figure 5 As shown, after modification by AG, the surface conduction band and Fermi level of NiOx+SAM are significantly improved, better matching the perovskite energy level, reducing the charge carrier transport barrier, and improving the charge carrier transport and extraction efficiency.
[0091] like Figure 6As shown, the open circuit voltage and fill factor of the perovskite solar cell are improved after lower interface modification, and the modified cell obtains a high open circuit voltage of 1.20V and a fill factor of 83.716%.
[0092] like Figure 7 As shown in the figure, the stability of the modified film was tested. The AG-optimized battery device can maintain 92.7% of its initial efficiency after running for 850 hours under air conditions, which is higher than the unmodified device.
[0093] Comparative Example 1
[0094] Comparative Example 1 differs from Example 1 only in steps 3 and 4. In step 3, no DNF solution of AG is prepared in Comparative Example 1, and no AG modification layer is spin-coated in step 4. The remaining steps and parameters are the same.
[0095] Figure 4 GIXRD comparison diagram of the unmodified and AG-modified perovskite layers at the lower interface. AG modification can improve the crystallinity and the quality of the film.
[0096] Figure 5 From the UPS comparison diagram of the unmodified and lower interface modified AG films, it can be seen that after AG modification, the NiOx+SAM surface conduction band and Fermi level are significantly improved, better matching the perovskite energy level and reducing the charge carrier transport barrier.
[0097] Figure 6 The JV curves of the lower interface modified and unmodified perovskite solar cells are shown in Table 1. It can be seen that compared with the unmodified control sample, the fill factor and open circuit voltage of the modified device are improved, with the highest values of 1.20V and 83.716%, and the efficiency of the best device prepared is 25.906%.
[0098] Table 1
[0099]
[0100] The figure shows the stability of the device efficiency of unmodified and modified ATFC under air temperature of 25°C and humidity of about 20%. After 850 hours, the optimized sample can still maintain 92.7% of the initial efficiency, which is higher in stability than the unmodified device.
[0101] Example 2
[0102] First, clean the FTO glass; 2 The FTO glass was cleaned with conductive glass cleaning solution, acetone, and ethanol, and then dried with a nitrogen air gun for later use.
[0103] Second, the preparation method of NiOx and Me-4PACz; add 1mL of deionized water to a glass bottle containing 10mg of NiOx powder to prepare a 10mg / mL NiOx dispersion, put the glass bottle into an ultrasonic cleaner, and ultrasonicate for 40min to ensure that the NiOx powder is fully dispersed in the deionized water for use. Dissolve 1mg of Me-4PACz solid powder in 2mL of isopropanol (IPA) to prepare a 0.5mg / mL solution and stir for 5h for use. Treat the FTO glass cleaned in step 1 with ultraviolet ozone for 20min. A 10 mg / mL NiOx dispersion was spin-coated on the FTO glass surface at a spin-coating speed of 2000 rpm for 30 s, followed by annealing at a temperature of 120°C for 20 min. After annealing, a 0.5 mg / mL Me-4PACz solution was spin-coated on the NiOx surface at a spin-coating speed of 4000 rpm for 30 s, followed by annealing at a temperature of 100°C for 10 min to obtain NiOx and Me-4PACz layers.
[0104] Third, prepare an AG modification layer solution of anhydrous ethanol (EtOH); the preparation method of the AG modification layer solution is: dissolve 2 mg of AG solid powder in 4 mL of EtOH, stir for 4 hours and set aside.
[0105] Fourth, prepare the AG modification layer; spin-coat the 0.5 mg / mL AG EtOH solution prepared in step 3 on the NiOx / Me-4PACz surface at a spin-coating speed of 6000 rpm for 20 s, followed by an annealing process at a temperature of 100°C for 3 min to obtain the AG modification layer.
[0106] Fifth, configure FA 0.9 Cs 0.1 PbI3 perovskite precursor solution: 0.9 M formamidine hydroiodide (FAI), 0.1 M cesium iodide (CsI) and 1.05 M lead iodide (PbI2) were dissolved in a mixed solvent of DMF and DMSO (V / V = 4:1) to prepare a 1 M FAI solution. 0.9 Cs 0.1 PbI3 perovskite precursor solution. The perovskite precursor solution was stirred for 6 h and then filtered using a 0.45 μm syringe for later use.
[0107] Sixth, prepare the perovskite light-absorbing layer (PVK); spin-coat the perovskite precursor solution prepared in step 5 on the surface of the AG modified layer. The spin-coating process is divided into two stages. In the first stage, the rotation speed is 1000rpm and the time is 8s; in the second stage, the rotation speed is 4000rpm and the time is 25s. Five seconds before the end, the anti-solvent anisole is applied to the perovskite surface, followed by an annealing process, the annealing temperature is 110°C, and the annealing time is 20min. After annealing, FTO / NiOx / Me-4PACz / AG / PVK is formed. The prepared perovskite light-absorbing layer is about 500nm.
[0108] Seventh, prepare the PDAI2 passivation layer on the upper surface of the perovskite; dissolve 2 mg of PDAI2 solid powder in 2 mL of a mixed solvent of chlorobenzene and IPA (V / V = 4:1) to prepare a mixed solution with a concentration of 1 mg / mL, stir for 5 hours and set aside. Spin coat the prepared passivation layer solution on the upper surface of the perovskite at a spin coating speed of 4500 rpm and a spin coating time of 25 seconds, followed by an annealing process at an annealing temperature of 110°C and an annealing time of 5 minutes. The FTO / NiOx / Me-4PACz / AG / PVK / PDAI2 layer was obtained.
[0109] Eighth, prepare the electron transport layer; evaporate the PDAI2 passivation layer on the surface of the perovskite prepared in step 7 to form a C 60 As the electron transport layer, FTO / NiOx / Me-4PACz / AG / perovskite light absorption layer / PDAI2 / C 60 .
[0110] Ninth, prepare a hole blocking layer; the C prepared in step 8 60 The surface was evaporated with a thickness of more than 6nm BCP (bathcopper) as a hole blocking layer to prepare FTO / NiOx / Me-4PACz / AG / PVK / PDAI2 / C 60 / BCP.
[0111] Tenth, prepare a metal electrode; evaporate silver with a thickness of about 100 nm on the surface of the hole blocking layer prepared in step 9 as a metal electrode, and finally obtain a structure of FTO / NiOx / Me-4PACz / AG / PVK / PDAI2 / C 60 / BCP / Ag organic-inorganic FACsPbI3 perovskite solar cells.
[0112] In this example, ethanol was used as the solvent for a 0.5 mg / mL AG solution, and the perovskite solar cell with the lower interface modification layer AG obtained an open circuit voltage of 1.186 V and a current of 25.84 mA / cm 2 short-circuit current, fill factor of 81.42%, and photoelectric conversion efficiency of 24.96%.
[0113] Example 3
[0114] First, clean the FTO glass; 2 The FTO glass was cleaned with conductive glass cleaning solution, acetone, and ethanol, and then dried with a nitrogen air gun for later use.
[0115] Second, the preparation method of NiOx and Me-4PACz; add 1mL of deionized water to a glass bottle containing 10mg of NiOx powder to prepare a 10mg / mL NiOx dispersion, put the glass bottle into an ultrasonic cleaner, and ultrasonicate for 40min to ensure that the NiOx powder is fully dispersed in the deionized water for use. Dissolve 1mg of Me-4PACz solid powder in 2mL of isopropanol (IPA) to prepare a 0.5mg / mL solution and stir for 5h for use. Treat the FTO glass cleaned in step 1 with ultraviolet ozone for 20min. A 10 mg / mL NiOx dispersion was spin-coated on the FTO glass surface at a spin-coating speed of 2000 rpm for 30 s, followed by annealing at a temperature of 120°C for 20 min. After annealing, a 0.5 mg / mL Me-4PACz solution was spin-coated on the NiOx surface at a spin-coating speed of 4000 rpm for 30 s, followed by annealing at a temperature of 100°C for 10 min to obtain a NiOx / Me-4PACz layer.
[0116] Third, prepare an isopropyl alcohol (IPA) modification layer solution of AG; the preparation method of the AG modification layer solution is: dissolve 2 mg of AG solid powder in 4 mL of IPA, stir for 4 hours and set aside.
[0117] Fourth, prepare the AG modification layer; spin-coat the 0.5 mg / mL AG IPA solution prepared in step 3 on the NiOx / Me-4PACz surface at a spin-coating speed of 6000 rpm for 20 s, followed by an annealing process at a temperature of 100°C for 3 min to obtain the AG modification layer.
[0118] Fifth, configure FA 0.9 Cs 0.1 PbI3 perovskite precursor solution: 0.9 M formamidine hydroiodide (FAI), 0.1 M cesium iodide (CsI) and 1.05 M lead iodide (PbI2) were dissolved in a mixed solvent of DMF and DMSO (V / V = 4:1) to prepare a 1 M FAI solution. 0.9 Cs 0.1 PbI3 perovskite precursor solution. The perovskite precursor solution was stirred for 6 h and then filtered using a 0.45 μm syringe for later use.
[0119] Sixth, prepare the perovskite light-absorbing layer (PVK); spin-coat the perovskite precursor solution prepared in step 5 on the surface of the AG modified layer. The spin-coating process is divided into two stages. In the first stage, the rotation speed is 1000rpm and the time is 8s; in the second stage, the rotation speed is 4000rpm and the time is 25s. Five seconds before the end, the anti-solvent anisole is applied to the perovskite surface, followed by an annealing process, the annealing temperature is 110°C, and the annealing time is 20min. After annealing, FTO / NiOx / Me-4PACz / AG / PVK is formed. The prepared perovskite light-absorbing layer is about 500nm.
[0120] Seventh, prepare the PDAI2 passivation layer on the upper surface of the perovskite; dissolve 2 mg of PDAI2 solid powder in 2 mL of a mixed solvent of chlorobenzene and IPA (V / V = 4:1) to prepare a mixed solution with a concentration of 1 mg / mL, stir for 5 hours and set aside. Spin coat the prepared passivation layer solution on the upper surface of the perovskite at a spin coating speed of 4500 rpm and a spin coating time of 25 seconds, followed by an annealing process at an annealing temperature of 110°C and an annealing time of 5 minutes. The FTO / NiOx / Me-4PACz / AG / PVK / PDAI2 layer was obtained.
[0121] Eighth, prepare the electron transport layer; evaporate the PDAI2 passivation layer on the surface of the perovskite prepared in step 7 to form a C 60 As the electron transport layer, FTO / NiOx / Me-4PACz / AG / perovskite light absorption layer / PDAI2 / C 60 .
[0122] Ninth, prepare a hole blocking layer; the C prepared in step 8 60 The surface was evaporated with a thickness of more than 6nm BCP (bathcopper) as a hole blocking layer to prepare FTO / NiOx / Me-4PACz / AG / PVK / PDAI2 / C 60 / BCP.
[0123] Tenth, prepare a metal electrode; evaporate silver with a thickness of about 100 nm on the surface of the hole blocking layer prepared in step 9 as a metal electrode, and finally obtain a structure of FTO / NiOx / Me-4PACz / AG / PVK / PDAI2 / C 60 / BCP / Ag organic-inorganic FACsPbI3 perovskite solar cells.
[0124] In this example, IPA was used as the solvent to prepare a 0.5 mg / mL lower interface modification layer AG solution. The prepared perovskite solar cell obtained an open circuit voltage of 1.178 V and a current of 25.58 mA / cm 2short-circuit current, fill factor of 81.53%, and photoelectric conversion efficiency of 24.57%.
[0125] Example 4
[0126] First, clean the FTO glass; 2 The FTO glass was cleaned with conductive glass cleaning solution, acetone, and ethanol, and then dried with a nitrogen air gun for later use.
[0127] Second, the preparation method of NiOx and Me-4PACz; add 1mL of deionized water to a glass bottle containing 10mg of NiOx powder to prepare a 10mg / mL NiOx dispersion, put the glass bottle into an ultrasonic cleaner, and ultrasonicate for 40min to ensure that the NiOx powder is fully dispersed in the deionized water for use. Dissolve 1mg of Me-4PACz solid powder in 2mL of isopropanol (IPA) to prepare a 0.5mg / mL solution and stir for 5h for use. Treat the FTO glass cleaned in step 1 with ultraviolet ozone for 20min. A 10 mg / mL NiOx dispersion was spin-coated on the FTO glass surface at a spin-coating speed of 2000 rpm for 30 s, followed by annealing at a temperature of 120°C for 20 min. After annealing, a 0.5 mg / mL Me-4PACz solution was spin-coated on the NiOx surface at a spin-coating speed of 4000 rpm for 30 s, followed by annealing at a temperature of 100°C for 10 min to obtain NiOx and Me-4PACz layers.
[0128] Third, prepare a dimethyl sulfoxide (DMSO)-dissolved AG modification layer solution; the preparation method of the AG modification layer solution is: dissolve 2 mg of AG solid powder in 4 mL of DMSO, stir for 4 hours and set aside.
[0129] Fourth, prepare the AG modified layer; spin-coat the DMSO solution of 0.5 mg / mL AG prepared in step 3 on the NiOx / Me-4PACz surface at a spin-coating speed of 6000 rpm for 20 s, followed by an annealing process at a temperature of 100°C for 3 min to obtain the AG modified layer.
[0130] Fifth, configure FA 0.9 Cs 0.1 PbI3 perovskite precursor solution: 0.9 M formamidine hydroiodide (FAI), 0.1 M cesium iodide (CsI) and 1.05 M lead iodide (PbI2) were dissolved in a mixed solvent of DMF and DMSO (V / V = 4:1) to prepare a 1 M FAI solution. 0.9 Cs 0.1PbI3 perovskite precursor solution. The perovskite precursor solution was stirred for 6 h and then filtered using a 0.45 μm syringe for later use.
[0131] Sixth, prepare the perovskite light-absorbing layer (PVK); spin-coat the perovskite precursor solution prepared in step 5 on the surface of the AG modified layer. The spin-coating process is divided into two stages. In the first stage, the rotation speed is 1000rpm and the time is 8s; in the second stage, the rotation speed is 4000rpm and the time is 25s. Five seconds before the end, the anti-solvent anisole is applied to the perovskite surface, followed by an annealing process, the annealing temperature is 110°C, and the annealing time is 20min. After annealing, FTO / NiOx / Me-4PACz / AG / PVK is formed. The prepared perovskite light-absorbing layer is about 500nm.
[0132] Seventh, prepare the PDAI2 passivation layer on the upper surface of the perovskite; dissolve 2 mg of PDAI2 solid powder in 2 mL of a mixed solvent of chlorobenzene and IPA (V / V = 4:1) to prepare a mixed solution with a concentration of 1 mg / mL, stir for 5 hours and set aside. Spin coat the prepared passivation layer solution on the upper surface of the perovskite at a spin coating speed of 4500 rpm and a spin coating time of 25 seconds, followed by an annealing process at an annealing temperature of 110°C and an annealing time of 5 minutes. The FTO / NiOx / Me-4PACz / AG / PVK / PDAI2 layer was obtained.
[0133] Eighth, prepare the electron transport layer; evaporate the PDAI2 passivation layer on the surface of the perovskite prepared in step 7 to form a C 60 As the electron transport layer, FTO / NiOx / Me-4PACz / AG / perovskite light absorption layer / PDAI2 / C 60 .
[0134] Ninth, prepare a hole blocking layer; the C prepared in step 8 60 The surface was evaporated with a thickness of more than 6nm BCP (bathcopper) as a hole blocking layer to prepare FTO / NiOx / Me-4PACz / AG / PVK / PDAI2 / C 60 / BCP.
[0135] Tenth, prepare a metal electrode; evaporate silver with a thickness of about 100 nm on the surface of the hole blocking layer prepared in step 9 as a metal electrode, and finally obtain a structure of FTO / NiOx / Me-4PACz / AG / PVK / PDAI2 / C 60 / BCP / Ag organic-inorganic FACsPbI3 perovskite solar cells.
[0136] In this example, DMSO was used as the solvent to prepare a 0.5 mg / mL lower interface modification layer AG solution. The prepared perovskite solar cell obtained an open circuit voltage of 1.179 V and a current of 24.96 mA / cm 2 short-circuit current, fill factor of 82.37%, photoelectric conversion efficiency of 24.25%.
[0137] Example 5
[0138] First, clean the FTO glass; 2 The FTO glass was cleaned with conductive glass cleaning solution, acetone, and ethanol, and then dried with a nitrogen air gun for later use.
[0139] Second, the preparation method of NiOx and Me-4PACz; add 1mL of deionized water to a glass bottle containing 10mg of NiOx powder to prepare a 10mg / mL NiOx dispersion, put the glass bottle into an ultrasonic cleaner, and ultrasonicate for 40min to ensure that the NiOx powder is fully dispersed in the deionized water for use. Dissolve 1mg of Me-4PACz solid powder in 2mL of isopropanol (IPA) to prepare a 0.5mg / mL solution and stir for 5h for use. Treat the FTO glass cleaned in step 1 with ultraviolet ozone for 20min. A 10 mg / mL NiOx dispersion was spin-coated on the FTO glass surface at a spin-coating speed of 2000 rpm for 30 s, followed by annealing at a temperature of 120°C for 20 min. After annealing, a 0.5 mg / mL Me-4PACz solution was spin-coated on the NiOx surface at a spin-coating speed of 4000 rpm for 30 s, followed by annealing at a temperature of 100°C for 10 min to obtain NiOx and Me-4PACz layers.
[0140] Third, prepare the N,N-dimethylformamide (DMF) modification layer solution of AG; the preparation method of the AG modification layer solution is: dissolve 1 mg of AG solid powder in 10 mL of DMF, stir for 4 hours and set aside.
[0141] Fourth, prepare an AG modified layer; spin coat the 0.1 mg / mL AG DMF solution prepared in step 3 on the NiOx / Me-4PACz surface at a spin coating speed of 6000 rpm for 20 s, followed by an annealing process at a temperature of 100°C for 3 min to obtain an AG modified layer.
[0142] Fifth, configure FA 0.9 Cs 0.1PbI3 perovskite precursor solution: 0.9 M formamidine hydroiodide (FAI), 0.1 M cesium iodide (CsI) and 1.05 M lead iodide (PbI2) were dissolved in a mixed solvent of DMF and DMSO (V / V = 4:1) to prepare a 1 M FAI solution. 0.9 Cs 0.1 PbI3 perovskite precursor solution. The perovskite precursor solution was stirred for 6 h and then filtered using a 0.45 μm syringe for later use.
[0143] Sixth, prepare the perovskite light-absorbing layer (PVK); spin-coat the perovskite precursor solution prepared in step 5 on the surface of the AG modified layer. The spin-coating process is divided into two stages. In the first stage, the rotation speed is 1000rpm and the time is 8s; in the second stage, the rotation speed is 4000rpm and the time is 25s. Five seconds before the end, the anti-solvent anisole is applied to the perovskite surface, followed by an annealing process, the annealing temperature is 110°C, and the annealing time is 20min. After annealing, FTO / NiOx / Me-4PACz / AG / PVK is formed. The prepared perovskite light-absorbing layer is about 500nm.
[0144] Seventh, prepare the PDAI2 passivation layer on the upper surface of the perovskite; dissolve 2 mg of PDAI2 solid powder in 2 mL of a mixed solvent of chlorobenzene and IPA (V / V = 4:1) to prepare a mixed solution with a concentration of 1 mg / mL, stir for 5 hours and set aside. Spin coat the prepared passivation layer solution on the upper surface of the perovskite at a spin coating speed of 4500 rpm and a spin coating time of 25 seconds, followed by an annealing process at an annealing temperature of 110°C and an annealing time of 5 minutes. The FTO / NiOx / Me-4PACz / AG / PVK / PDAI2 layer was obtained.
[0145] Eighth, prepare the electron transport layer; evaporate the PDAI2 passivation layer on the surface of the perovskite prepared in step 7 to form a C 60 As the electron transport layer, FTO / NiOx / Me-4PACz / AG / perovskite light absorption layer / PDAI2 / C 60 .
[0146] Ninth, prepare a hole blocking layer; the C prepared in step 8 60 The surface was evaporated with a thickness of more than 6nm BCP (bathcopper) as a hole blocking layer to prepare FTO / NiOx / Me-4PACz / AG / PVK / PDAI2 / C 60 / BCP.
[0147] Tenth, prepare a metal electrode; evaporate silver with a thickness of about 100 nm on the surface of the hole blocking layer prepared in step 9 as a metal electrode, and finally obtain a structure of FTO / NiOx / Me-4PACz / AG / PVK / PDAI2 / C 60 / BCP / Ag organic-inorganic FACsPbI3 perovskite solar cells.
[0148] In this example, DMF was used as the solvent to prepare a 0.1 mg / mL lower interface modification layer AG solution. The prepared perovskite solar cell obtained an open circuit voltage of 1.187 V and a current of 24.64 mA / cm 2 short-circuit current, fill factor of 81.35%, and photoelectric conversion efficiency of 24.77%.
[0149] Example 6
[0150] First, clean the FTO glass; 2 The FTO glass was cleaned with conductive glass cleaning solution, acetone, and ethanol, and then dried with a nitrogen air gun for later use.
[0151] Second, the preparation method of NiOx and Me-4PACz; add 1mL of deionized water to a glass bottle containing 10mg of NiOx powder to prepare a 10mg / mL NiOx dispersion, put the glass bottle into an ultrasonic cleaner, and ultrasonicate for 40min to ensure that the NiOx powder is fully dispersed in the deionized water for use. Dissolve 1mg of Me-4PACz solid powder in 2mL of isopropanol (IPA) to prepare a 0.5mg / mL solution and stir for 5h for use. Treat the FTO glass cleaned in step 1 with ultraviolet ozone for 20min. A 10 mg / mL NiOx dispersion was spin-coated on the FTO glass surface at a spin-coating speed of 2000 rpm for 30 s, followed by annealing at a temperature of 120°C for 20 min. After annealing, a 0.5 mg / mL Me-4PACz solution was spin-coated on the NiOx surface at a spin-coating speed of 4000 rpm for 30 s, followed by annealing at a temperature of 100°C for 10 min to obtain NiOx and Me-4PACz layers.
[0152] Third, prepare the N,N-dimethylformamide (DMF) modification layer solution of AG; the preparation method of the AG modification layer solution is: dissolve 1 mg of AG solid powder in 3 mL of DMF, stir for 4 hours and set aside.
[0153] Fourth, prepare an AG modified layer; spin coat the 0.33 mg / mL AG DMF solution prepared in step 3 on the NiOx / Me-4PACz surface at a spin coating speed of 6000 rpm for 20 s, followed by an annealing process at a temperature of 100°C for 3 min to obtain an AG modified layer.
[0154] Fifth, configure FA 0.9 Cs 0.1 PbI3 perovskite precursor solution: 0.9 M formamidine hydroiodide (FAI), 0.1 M cesium iodide (CsI) and 1.05 M lead iodide (PbI2) were dissolved in a mixed solvent of DMF and DMSO (V / V = 4:1) to prepare a 1 M FAI solution. 0.9 Cs 0.1 PbI3 perovskite precursor solution. The perovskite precursor solution was stirred for 6 h and then filtered using a 0.45 μm syringe for later use.
[0155] Sixth, prepare the perovskite light-absorbing layer (PVK); spin-coat the perovskite precursor solution prepared in step 5 on the surface of the AG modified layer. The spin-coating process is divided into two stages. In the first stage, the rotation speed is 1000rpm and the time is 8s; in the second stage, the rotation speed is 4000rpm and the time is 25s. Five seconds before the end, the anti-solvent anisole is applied to the perovskite surface, followed by an annealing process, the annealing temperature is 110°C, and the annealing time is 20min. After annealing, FTO / NiOx / Me-4PACz / AG / PVK is formed. The prepared perovskite light-absorbing layer is about 500nm.
[0156] Seventh, prepare the PDAI2 passivation layer on the upper surface of the perovskite; dissolve 2 mg of PDAI2 solid powder in 2 mL of a mixed solvent of chlorobenzene and IPA (V / V = 4:1) to prepare a mixed solution with a concentration of 1 mg / mL, stir for 5 hours and set aside. Spin coat the prepared passivation layer solution on the upper surface of the perovskite at a spin coating speed of 4500 rpm and a spin coating time of 25 seconds, followed by an annealing process at an annealing temperature of 110°C and an annealing time of 5 minutes. The FTO / NiOx / Me-4PACz / AG / PVK / PDAI2 layer was obtained.
[0157] Eighth, prepare the electron transport layer; evaporate the PDAI2 passivation layer on the surface of the perovskite prepared in step 7 to form a C 60 As the electron transport layer, FTO / NiOx / Me-4PACz / AG / perovskite light absorption layer / PDAI2 / C 60 .
[0158] Ninth, prepare a hole blocking layer; the C prepared in step 8 60The surface was evaporated with a thickness of more than 6nm BCP (bathcopper) as a hole blocking layer to prepare FTO / NiOx / Me-4PACz / AG / PVK / PDAI2 / C 60 / BCP.
[0159] Tenth, prepare a metal electrode; evaporate silver with a thickness of about 100 nm on the surface of the hole blocking layer prepared in step 9 as a metal electrode, and finally obtain a structure of FTO / NiOx / Me-4PACz / AG / PVK / PDAI2 / C 60 / BCP / Ag organic-inorganic FACsPbI3 perovskite solar cells.
[0160] In this embodiment, DMF was used as solvent to prepare a 0.3 mg / mL lower interface modification layer AG solution. The prepared perovskite solar cell obtained an open circuit voltage of 1.193 V and a current of 25.72 mA / cm 2 short-circuit current, fill factor of 82.29%, and photoelectric conversion efficiency of 25.26%.
[0161] Example 7
[0162] First, clean the FTO glass; 2 The FTO glass was cleaned with conductive glass cleaning solution, acetone, and ethanol, and then dried with a nitrogen air gun for later use.
[0163] Second, the preparation method of NiOx and Me-4PACz; add 1mL of deionized water to a glass bottle containing 10mg of NiOx powder to prepare a 10mg / mL NiOx dispersion, put the glass bottle into an ultrasonic cleaner, and ultrasonicate for 40min to ensure that the NiOx powder is fully dispersed in the deionized water for use. Dissolve 1mg of Me-4PACz solid powder in 2mL of isopropanol (IPA) to prepare a 0.5mg / mL solution and stir for 5h for use. Treat the FTO glass cleaned in step 1 with ultraviolet ozone for 20min. A 10 mg / mL NiOx dispersion was spin-coated on the FTO glass surface at a spin-coating speed of 2000 rpm for 30 s, followed by annealing at a temperature of 120°C for 20 min. After annealing, a 0.5 mg / mL Me-4PACz solution was spin-coated on the NiOx surface at a spin-coating speed of 4000 rpm for 30 s, followed by annealing at a temperature of 100°C for 10 min to obtain NiOx and Me-4PACz layers.
[0164] Third, prepare the N,N-dimethylformamide (DMF) modification layer solution of AG; the preparation method of the AG modification layer solution is: dissolve 2 mg of AG solid powder in 2 mL of DMF, stir for 4 hours and set aside.
[0165] Fourth, prepare the AG modified layer; spin-coat the 1.0 mg / mL AG DMF solution prepared in step 3 on the NiOx / Me-4PACz surface at a spin-coating speed of 6000 rpm for 20 s, followed by an annealing process at a temperature of 100°C for 3 min to obtain the AG modified layer.
[0166] Fifth, configure FA 0.9 Cs 0.1 PbI3 perovskite precursor solution: 0.9 M formamidine hydroiodide (FAI), 0.1 M cesium iodide (CsI) and 1.05 M lead iodide (PbI2) were dissolved in a mixed solvent of DMF and DMSO (V / V = 4:1) to prepare a 1 M FAI solution. 0.9 Cs 0.1 PbI3 perovskite precursor solution. The perovskite precursor solution was stirred for 6 h and then filtered using a 0.45 μm syringe for later use.
[0167] Sixth, prepare the perovskite light-absorbing layer (PVK); spin-coat the perovskite precursor solution prepared in step 5 on the surface of the AG modified layer. The spin-coating process is divided into two stages. In the first stage, the rotation speed is 1000rpm and the time is 8s; in the second stage, the rotation speed is 4000rpm and the time is 25s. Five seconds before the end, the anti-solvent anisole is applied to the perovskite surface, followed by an annealing process, the annealing temperature is 110°C, and the annealing time is 20min. After annealing, FTO / NiOx / Me-4PACz / AG / PVK is formed. The prepared perovskite light-absorbing layer is about 500nm.
[0168] Seventh, prepare the PDAI2 passivation layer on the upper surface of the perovskite; dissolve 2 mg of PDAI2 solid powder in 2 mL of a mixed solvent of chlorobenzene and IPA (V / V = 4:1) to prepare a mixed solution with a concentration of 1 mg / mL, stir for 5 hours and set aside. Spin coat the prepared passivation layer solution on the upper surface of the perovskite at a spin coating speed of 4500 rpm and a spin coating time of 25 seconds, followed by an annealing process at an annealing temperature of 110°C and an annealing time of 5 minutes. The FTO / NiOx / Me-4PACz / AG / PVK / PDAI2 layer was obtained.
[0169] Eighth, prepare the electron transport layer; evaporate the PDAI2 passivation layer on the surface of the perovskite prepared in step 7 to form a C 60As the electron transport layer, FTO / NiOx / Me-4PACz / AG / perovskite light absorption layer / PDAI2 / C 60 .
[0170] Ninth, prepare a hole blocking layer; the C prepared in step 8 60 The surface was evaporated with a thickness of more than 6nm BCP (bathcopper) as a hole blocking layer to prepare FTO / NiOx / Me-4PACz / AG / PVK / PDAI2 / C 60 / BCP.
[0171] Tenth, prepare a metal electrode; evaporate silver with a thickness of about 100 nm on the surface of the hole blocking layer prepared in step 9 as a metal electrode, and finally obtain a structure of FTO / NiOx / Me-4PACz / AG / PVK / PDAI2 / C 60 / BCP / Ag organic-inorganic FACsPbI3 perovskite solar cells.
[0172] In this example, DMF was used as the solvent to prepare a 1 mg / mL lower interface modification layer AG solution. The prepared perovskite solar cell obtained an open circuit voltage of 1.193 V and a current of 25.87 mA / cm 2 short-circuit current, fill factor of 81.4%, photoelectric conversion efficiency of 25.15%.
[0173] The above description is only a preferred embodiment of the present invention and is not intended to limit the present invention. Any modifications, equivalent substitutions, improvements, etc. made within the spirit and principle of the present invention should be included in the protection scope of the present invention.
Claims
1. A method for preparing a high-opening voltage inverse perovskite battery based on polyhydroxyglycinate aluminum, characterized in that: The following steps are involved: Step 1, pre-treating FTO glass; Step 2: NiO X The dispersion is spin-coated on the FTO glass surface and a NiOx layer is obtained after annealing. X The dispersion is a solution prepared by dissolving NiOx powder in water; Step 3, spin-coating the Me-4PACz solution on the NiOx layer, and obtaining the Me-4PACz layer after annealing; the solute of the Me-4PACz solution is Me-4PACz solid powder, and the solvent is isopropanol; the NiOx layer and the Me-4PACz layer constitute a charge transport layer; Step 4, spin coating an AG solution with a concentration of 0.1-1 mg / mL on the Me-4PACz layer, and preparing an AG modified layer after annealing, wherein the AG is polyhydroxyglycinate aluminum; Step 5: Spin-coat FA on the AG modified layer 0.9 Cs 0.1 PbI3 perovskite precursor solution is annealed to obtain a perovskite light absorbing layer; Step 6, preparing a PDAI2 passivation layer on the perovskite light absorbing layer; Step 7, preparing an electron transport layer on the PDAI2 passivation layer, and then preparing a hole blocking layer; Step 8: Prepare a metal electrode on the hole blocking layer to obtain a high-opening voltage inverse perovskite cell.
2. The method for preparing a high-opening voltage inverse perovskite battery based on polyhydroxyglycinate aluminum according to claim 1, characterized in that: In step 2, the concentration of the NiOx dispersion is 10 mg / mL; the spin coating speed is 2000 rpm, the spin coating time is 30 s, the annealing temperature is 120° C., and the annealing time is 20 min.
3. The method for preparing a high-opening voltage inverse perovskite battery based on polyhydroxyglycinate aluminum according to claim 1, characterized in that: In step 3, the concentration of the Me-4PACz solution is 0.5 mg / mL, the spin coating speed is 4000 rpm, the spin coating time is 30 s, the annealing temperature is 100° C., and the annealing time is 10 min.
4. The method for preparing a high-opening voltage inverse perovskite battery based on polyhydroxyglycinate aluminum according to claim 1, characterized in that: In step 4, the solute of the AG solution is polyhydroxyglycinate aluminum, and the solvent is any one of N,N-dimethylformamide, anhydrous ethanol, isopropanol or dimethyl sulfoxide.
5. The method for preparing a high-opening voltage inverse perovskite battery based on polyhydroxyglycinate aluminum according to claim 1, characterized in that: In step 4, the spin coating speed is 6000 rpm, the spin coating time is 20 s; the annealing temperature is 100° C., and the annealing time is 3 min.
6. The method for preparing a high-opening voltage inverse perovskite battery based on polyhydroxyglycinate aluminum according to claim 1, characterized in that: In step 5, the concentration of the perovskite precursor solution is 1 M, and the perovskite solution is spin-coated in two stages.
7. The method for preparing a high-opening voltage inverse perovskite battery based on polyhydroxyglycinate aluminum according to claim 1, characterized in that: In step 6, a PDAI2 passivation layer is prepared on the perovskite light absorbing layer by spin coating a passivation layer solution, the concentration of the passivation layer solution is 1 mg / mL, the solute is PDAI2 solid powder, and the solvent is a mixture of chlorobenzene and IPA.
8. The method for preparing a high-opening voltage inverse perovskite battery based on polyhydroxyglycinate aluminum according to claim 1, characterized in that: In step 7, the electron transport layer is C 60 , prepared by evaporation method.
9. The method for preparing a high-opening voltage inverse perovskite battery based on polyhydroxyglycinate aluminum according to claim 1, characterized in that: In step 7, the hole blocking layer is BCP, which is prepared by evaporation.
10. A high-opening voltage inverse perovskite battery based on polyhydroxyglycinate aluminum prepared by the preparation method according to any one of claims 1 to 9, characterized in that: Including FTO / NiOx / Me-4PACz / AG / PVK / PDAI2 / C from one side to the other 60 / BCP / Ag.