A method for preparing a thermoelectric film, a thermoelectric film and a thermoelectric device

Through near-space sublimation process and component adjustment, the problem of long and high cost of preparation of thick thermoelectric films in magnetron sputtering process is solved, and efficient and low-cost thermoelectric film preparation is achieved, which improves the performance and adhesion of the thermoelectric film. , suitable for mass production.

CN118742179BActive Publication Date: 2024-11-15SHANGHAI IND U TECH RES INST
View PDF 3 Cites 0 Cited by

Patent Information

Application Number
CN202411223702.6
Authority / Receiving Office
CN · China
Patent Type
Patents(China)
Current Assignee / Owner
Filing Date
2024-09-03
Publication Date
2024-11-15
Estimated Expiration
2044-09-03

AI Technical Summary

Technical Problem

The existing magnetron sputtering process takes a long time to prepare thick thermoelectric films, is costly and is not conducive to large-scale mass production, and the thermoelectric material targets are expensive and have low utilization, resulting in poor economic benefits.

Method used

The near-space sublimation process is used to prepare thermoelectric films. By pre-adjusting the components of the thermoelectric material, the content of tellurium is increased, and process parameters such as heating temperature, deposition distance and air pressure are optimized, combined with in-situ annealing treatment, the deposition efficiency and performance are improved.

Benefits of technology

It significantly improves the deposition efficiency of thermoelectric materials, reduces production costs, avoids component deviations, improves the conductivity and thermoelectric properties of the thermoelectric film, and ensures the adhesion and microstructure of the thick thermoelectric film.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN118742179B_ABST
    Figure CN118742179B_ABST
Patent Text Reader

Abstract

The present invention provides a method for preparing a thermoelectric film, a thermoelectric film and a thermoelectric device. The preparation method includes providing a substrate and a thermoelectric material, wherein the thermoelectric material is antimony telluride powder or bismuth telluride powder, and the atomic percentage of tellurium in the thermoelectric material is between 62% and 67%; and a near-space sublimation process is used to deposit the thermoelectric material on the substrate to form a thermoelectric film. The present invention adopts a near-space sublimation process to replace the common magnetron sputtering process, which significantly improves the deposition efficiency of the thermoelectric material and reduces the production cost; by pre-adjusting the components of the source material used for near-space sublimation, the content of the tellurium element is increased, and the loss caused by the volatilization of the tellurium element during deposition is effectively reduced, and a large component deviation of the thermoelectric film is avoided, thereby ensuring the performance of the thermoelectric film.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The present application relates to the technical field of thermoelectric thin film materials and devices, and in particular to a method for preparing a thermoelectric film, a thermoelectric film and a thermoelectric device. Background Art

[0002] A thermoelectric device refers to a functional electronic device built based on thermoelectric materials. Through microelectronic processes such as electrode interconnection and packaging, the thermoelectric properties of thermoelectric materials can be effectively applied. Thin-film thermoelectric devices have broad application potential and are irreplaceable.

[0003] High-performance thin-film thermoelectric devices usually require the preparation of thermoelectric arms with a thickness of tens of μm. In traditional processes, magnetron sputtering is usually used to deposit thermoelectric materials. The existing magnetron sputtering technology takes a long time to prepare thick thermoelectric films. Only 1-2 μm thick thermoelectric films can be deposited per hour, and it usually takes more than 6 hours to prepare a 10 μm thick thermoelectric film. The target material of the thermoelectric material is expensive and has a low utilization rate. A 3 mm thick 4-inch single target costs more than 3,000 yuan, and only a small circle of circular area can be used, and the rest is wasted. A 3 mm thick target can generally only be used 3-5 times, and the target needs to be frequently opened and replaced, which is troublesome to operate. The above problems make the magnetron sputtering process of thick thermoelectric films not conducive to large-scale mass production and have poor economic benefits. Therefore, it is necessary to develop other methods for quickly preparing thick thermoelectric films. Summary of the invention

[0004] In order to solve the above problems, the present invention adopts a close-space sublimation process to quickly prepare thermoelectric films, which has high deposition efficiency, simple preparation process and low cost, and is conducive to promoting large-scale mass production of thermoelectric devices.

[0005] The present invention provides a method for preparing a thermoelectric film, a thermoelectric film and a thermoelectric device. The preparation method comprises the following steps:

[0006] S1. Providing a substrate and a thermoelectric material, wherein the thermoelectric material is antimony telluride powder or bismuth telluride powder, and the atomic percentage of tellurium in the thermoelectric material is between 62% and 67%;

[0007] S2. Using a close-space sublimation process, the thermoelectric material is deposited on the substrate to form a thermoelectric film.

[0008] Using the near-space sublimation process to replace the magnetron sputtering process can significantly improve the deposition efficiency of thermoelectric materials, reduce production costs, and facilitate the large-scale mass production of thermoelectric devices; and by pre-adjusting the composition of the source material used for near-space sublimation and increasing the content of tellurium, it can effectively reduce the loss caused by the volatilization of tellurium during deposition, avoid large component deviations in the thermoelectric film, and thus ensure the performance of the thermoelectric film. Increasing the tellurium content in the thermoelectric material to between 62% and 67% can more accurately guarantee the composition of the thermoelectric film, thereby ensuring the performance of the thermoelectric film.

[0009] The close-space sublimation process parameters are: the heating temperature of the thermoelectric material is 600-800°C, the heating temperature of the substrate is 200-400°C, the deposition distance is 4-6 mm, and the deposition pressure is less than 10 -3 Pa. By optimizing the close-space sublimation process, especially the temperature of the substrate, the deposition efficiency of the thermoelectric material and the organizational structure of the thermoelectric film layer can be effectively guaranteed.

[0010] After the close-space sublimation deposition, an in-situ annealing treatment is performed, with an annealing temperature of 200-400° C. and an annealing time of 60-120 minutes. Further in-situ annealing treatment can further improve the microstructure of the thermoelectric film layer and enhance the electrical conductivity and thermoelectric performance of the thermoelectric film.

[0011] The antimony telluride powder or the bismuth telluride powder is prepared by a mechanical alloying process. Mechanical alloying can easily prepare fine powders containing excessive tellurium with uniform element distribution.

[0012] The antimony telluride powder is prepared by mechanical alloying of simple antimony powder and simple tellurium powder, and the content of the simple tellurium powder is 62%-67% by atomic percentage; the bismuth telluride powder is prepared by mechanical alloying of simple bismuth powder and simple tellurium powder, and the content of the simple tellurium powder is 62%-67% by atomic percentage. By controlling the ratio of the two simple powders, a powdered thermoelectric material with uniform element distribution and controllable component content can be obtained through the mechanical alloying process.

[0013] The surface roughness of the substrate Ra≥50 nm. Improving the surface roughness of the substrate is beneficial to improving the bonding between the thermoelectric film layer and the substrate and preventing the thick thermoelectric film from falling off.

[0014] Before step S2, the substrate is subjected to plasma cleaning. Plasma cleaning of the substrate can improve the consistency of the surface roughness of the substrate and further prevent the thick film from falling off the substrate.

[0015] A thermoelectric film is prepared according to the above-mentioned method for preparing a thermoelectric film, and can significantly improve the deposition efficiency of thermoelectric materials.

[0016] A thermoelectric device comprises an electrode layer and a thermoelectric arm, wherein the thermoelectric arm is a patterned thermoelectric film, and the thermoelectric arm is obtained by preparing a thermoelectric film on the electrode layer according to the above-mentioned method for preparing a thermoelectric film and patterning the film. The deposition efficiency of the thermoelectric material can be significantly improved.

[0017] The beneficial effects of the present invention are as follows: the present invention adopts a close-space sublimation process to replace the magnetron sputtering process, which can significantly improve the deposition efficiency of thermoelectric materials and reduce production costs; by pre-adjusting the components of the source material used for close-space sublimation and increasing the content of tellurium, the loss caused by the volatilization of tellurium during deposition can be effectively reduced, and a large component deviation of the thermoelectric film can be avoided, thereby ensuring the performance of the thermoelectric film; by optimizing the process parameters, the microstructure of the thermoelectric film can be effectively improved, and the electrical conductivity and thermoelectric performance of the thermoelectric film can be improved; by selecting a substrate with a higher roughness and performing a plasma cleaning treatment on the substrate, the consistency of the surface roughness of the substrate is improved, and the thick thermoelectric film is effectively avoided from falling off the substrate. BRIEF DESCRIPTION OF THE DRAWINGS

[0018] In order to more clearly illustrate the technical solutions in the specific embodiments of the present invention, the drawings required for use in the description of the embodiments will be briefly introduced below. Obviously, the drawings described below are only some embodiments of the present invention. For ordinary technicians in this field, other drawings can be obtained based on these drawings without paying creative work.

[0019] Figure 1 This is a schematic diagram of a close-space sublimation device provided by the present invention.

[0020] Figure 2 This is a scanning electron microscope image of the bismuth telluride film layer prepared in Example 1 of the present invention.

[0021] Figure 3 The thermoelectric performance results of the bismuth telluride film layers prepared in Examples 1 to 3 of the present invention. Figure 3 A in is the Seebeck coefficient result of the bismuth telluride film layer; Figure 3 B in it is the conductivity result of bismuth telluride film layer; Figure 3 C in the figure is the power factor result of the bismuth telluride film layer.

[0022] Figure 4 The thermoelectric performance results of the bismuth telluride film layer prepared in Comparative Example 1 of the present invention. Figure 4 A in it is the Seebeck coefficient and conductivity results of the bismuth telluride film layer; Figure 4 B in FIG. 1 is the power factor result of the bismuth telluride film layer. DETAILED DESCRIPTION

[0023] The above and other technical contents, features and effects of the present invention will be clearly presented in the following detailed description of a preferred embodiment with reference to the drawings. The directional terms mentioned in the following embodiments, such as up, down, left, right, front or back, etc., are only referenced to the directions of the attached drawings. Therefore, the directional terms used are used to illustrate and not to limit the present invention.

[0024] The following will describe the various embodiments of the present application in detail with reference to the accompanying drawings. However, it will be appreciated by those skilled in the art that in the various embodiments of the present application, many technical details are provided in order to enable the reader to better understand the present application. However, even without these technical details and various changes and modifications based on the following embodiments, the technical solution claimed in the present application can be implemented.

[0025] In the prior art, the deposition of thermoelectric materials is usually carried out by magnetron sputtering. However, the deposition efficiency of magnetron sputtering is low, and only 1-2 μm thick thermoelectric material film can be deposited per hour; and the target material used is expensive and has low utilization rate, resulting in high cost; there is no doubt that the low deposition rate and high preparation cost greatly limit the large-scale mass production of thin-film thermoelectric devices. Therefore, in order to solve the above problems, it is necessary to develop a method that can quickly prepare thick thermoelectric films.

[0026] Close Space Sublimation (CSS) is a method of depositing materials on a substrate surface by close space sublimation. Specifically, in this method, a high-temperature source material is placed close to the substrate and opposite to it, so that the source material is heated and sublimated and deposited on the substrate to form a thin film. Close space sublimation can achieve rapid deposition of source materials, so the close space sublimation method is used in the present invention to prepare thermoelectric films.

[0027] Among thermoelectric materials, P-type Sb2Te3 materials and N-type Bi2Te3 materials are the most common thermoelectric thin film materials. We have conducted in-depth research on the CSS process of the above two materials. During the research process of this invention, we found that there are several difficulties in using the CSS method to prepare thermoelectric films (Sb2Te3 films and Bi2Te3 films). First, the saturated vapor pressure of the Te element is relatively high, and it is easy to volatilize into the gas phase during the preparation process, causing deviations in the components of the thermoelectric film, thereby affecting the performance of the thermoelectric film. Second, the preparation process of the thermoelectric film deposited by the CSS method is relatively fast, which will affect the microstructure of the thermoelectric film. Third, the prepared thermoelectric film has poor adhesion and is easy to fall off.

[0028] The following is an example of a method for preparing a thermoelectric film using CSS. The steps in the following example do not correspond one to one with the summary of the invention.

[0029] Embodiment 1:

[0030] The present invention provides a method for preparing a thermoelectric film, a thermoelectric film and a thermoelectric device. It should be noted that the scheme provided in this embodiment is a preferred scheme, and not all the steps and processes used below must be consistent with those mentioned in this embodiment. Some processes or steps can be modified or omitted. The preparation method in this embodiment includes the following steps:

[0031] Step 1: Provide a substrate and perform a plasma cleaning process.

[0032] In this embodiment, the substrate used is an aluminum nitride (AlN) substrate with a relatively high roughness (Ra ≥ 50 nm). It is understood that in other embodiments, the present invention can also be implemented using a silicon substrate with an oxide layer; in other embodiments, the substrate can also be a substrate on which the electrode layer has been prepared and is to be deposited on the thermoelectric arm. The present invention does not limit the type of substrate. It is understood that in this embodiment, a substrate with a relatively high roughness is directly selected. In other embodiments, the substrate can also be processed by existing technical means to ensure the roughness of the substrate.

[0033] Before deposition, a plasma cleaning machine is used to perform plasma cleaning on the provided aluminum nitride substrate to improve the consistency of the surface roughness of the substrate. The specific parameters of plasma cleaning are as follows: the ambient atmosphere is argon, the plasma power is 60 W, and the processing time is 5 minutes. In other embodiments, the ambient atmosphere is argon or nitrogen, the plasma power is 40-120 W, and the processing time is 3-10 minutes.

[0034] It should be noted that during the research process of the technical solution of this application, it was found that when CSS is used to prepare a thick thermoelectric film, the prepared thermoelectric film may have poor adhesion and easy to fall off (especially during the cooling process). In this embodiment, by selecting a substrate with a large surface roughness (Ra ≥ 50 nm) to deposit a thick film, and the substrate is plasma cleaned, the consistency of the substrate surface roughness is further improved, thereby effectively preventing the thick thermoelectric film from falling off the substrate.

[0035] Step 2: Prepare powdered thermoelectric materials.

[0036] In the present application, the CSS process is used to deposit thermoelectric materials. For the CSS process, the source material used is usually required to be in fine powder form, so the powder raw material must be prepared first. In this embodiment, the most common thermoelectric thin film materials, namely P-type Sb2Te3 materials and N-type Bi2Te3 materials, are studied. During the research process of this application, it was found that due to the high saturated vapor pressure of the Te (tellurium) element, in the process of depositing Sb2Te3 or Bi2Te3 materials using the CSS process, the tellurium element is easy to volatilize into the gas phase, which eventually causes the components of the deposited film layer to deviate (that is, due to the lack of tellurium elements, the deposited Sb2Te3 or Bi2Te3 film layer is non-stoichiometric), thereby affecting the performance of the thermoelectric material film layer. If Sb2Te3 or Bi2Te3 powder with normal composition is directly used (that is, the atomic percentage content of Te is 60%), the atomic percentage content of Te in the final thermoelectric film component is only about 50%, the thermoelectric performance is extremely poor, and the power factor is less than 1μW / K 2 .cm.

[0037] In order to solve the problem of the lack of tellurium in the thermoelectric material film layer obtained by CSS deposition, in this embodiment, the components of the powder raw materials used for CSS deposition are pre-adjusted in advance, that is, an excess of tellurium is added to the thermoelectric material powder in advance to compensate for the loss caused by the volatilization of tellurium during CSS deposition.

[0038] Specifically, in this embodiment, two thermoelectric materials, namely antimony telluride powder or bismuth telluride powder, are prepared by mechanical alloying (high-energy ball milling) process. Here, the preparation of antimony telluride powder is taken as an example for introduction, and the preparation process of bismuth telluride powder can refer to that of antimony telluride powder.

[0039] First, select an appropriate amount of elemental antimony powder and elemental tellurium powder to prepare the ball milling raw material powder. In the normal process, in order to prepare antimony telluride powder, the amount of the two elemental powders used is 40% antimony and 60% tellurium in atomic percentage (that is, according to the stoichiometric ratio of Sb2Te3 material). In order to make up for the loss caused by the volatilization of the tellurium element, in this embodiment, the atomic percentages of elemental antimony powder and elemental tellurium powder are 35% and 65%, respectively. According to the above ratio, weigh an appropriate amount of antimony powder and tellurium powder and mix them thoroughly. In this embodiment, the elemental antimony powder and elemental tellurium powder used are 100 mesh, and then the mixed powder is passed through a 20-mesh round hole sieve, and the coarse powder is weighed in an appropriate amount for use.

[0040] Then, mechanical alloying treatment is carried out. Specifically, the coarse powder is weighed in an appropriate amount and put into a ball mill, and an appropriate amount of agate balls are put in according to a ball-to-material ratio of 5:1 and a large-small ball ratio of 1:1. The total mass of the agate balls should not exceed 150 g. Then, 95% alcohol is poured into the ball mill, and the agate balls are not covered. The ball mill is sealed and the air is exhausted with a large flow of N2. The N2 flushing time is 10 minutes. The powder is refined with a ball mill. The speed of the ball mill is 300-500rpm, and the time is 15 hours. The specific program setting is forward rotation for 20 minutes, reverse rotation for 20 minutes, and interval of 1.5 minutes. The alloying treatment is completed.

[0041] Finally, the powder in the ball mill is separated and dried to obtain the antimony telluride powder (i.e., antimony telluride containing excess tellurium element) in this embodiment. Specifically, after the ball milling is completed, the ball mill is opened, the suspension therein is transferred to a centrifuge tube with a plastic straw, and the agate balls and the remaining powder on the ball mill are washed with alcohol and transferred to the centrifuge tube; the alcohol and powder are separated by a centrifuge at a speed of 2500 rpm for 2 min, and the alcohol is poured out for storage; a certain amount of deionized water is poured into the centrifuge tube, and after dispersion, the solid and liquid are separated by a centrifuge with the same parameters, and the water is poured out after centrifugation; then the centrifuge tube containing the powder is placed in a freezer until it freezes, and the freeze dryer is turned on, and the temperature is lowered to about -45 ° C and stabilized for 30 min; the frozen centrifuge tube is placed in the freeze dryer, the lid is covered, the vacuum pump is turned on, and it is dried for more than 10 h; the dried powder is sieved with a vibrating sieve to obtain a 325 mesh powder, and the sieving time is 30 min. As described above, the dried antimony telluride powder is obtained. It can be understood that, since the atomic percentages of the elemental antimony powder and the elemental tellurium powder are 35% and 65% respectively during the preparation, the antimony telluride powder obtained at this time is non-stoichiometric, wherein the tellurium content is relatively high, which is 65% (atomic percentage), while the antimony content is 35% (atomic percentage).

[0042] In this embodiment, the preparation process of bismuth telluride powder is the same as that of antimony telluride powder, except for the selection of ball-milled raw material powder. It can be understood that for bismuth telluride powder, the raw materials used are elemental bismuth powder and elemental tellurium powder, and the atomic percentages of the two are 35% and 65%, respectively. Similarly, since the atomic percentages of elemental bismuth powder and elemental tellurium powder are 35% and 65%, respectively, during preparation, the obtained bismuth telluride powder is non-stoichiometric, wherein the tellurium content is relatively high, 65% (atomic percentage), and the bismuth content is 35% (atomic percentage).

[0043] It should be noted that the process for preparing antimony telluride powder or bismuth telluride powder is not limited to the above-mentioned mechanical alloying process, and other processes may also be used, such as gas atomization, water atomization, etc. In the present application, the method for obtaining antimony telluride powder or bismuth telluride powder is not limited. By pre-adjusting the components in the source material used in CSS to ensure that the tellurium element is excessive, the loss caused by the volatilization of the tellurium element can be reduced accordingly during subsequent deposition.

[0044] Step 3: Deposit thermoelectric material on the substrate using a close-space sublimation process to form a thermoelectric film.

[0045] In this embodiment, a close-space sublimation process is used to deposit thermoelectric materials. The close-space sublimation technology is to place the source material and the substrate close to each other, heat the source material to make it sublime and deposit it on the substrate to form a film layer. The schematic diagram of the close-space sublimation equipment is shown in FIG. Figure 1 Reference Figure 1 Typically, a near-space sublimation device includes a cavity 30 and an upper box body 10 and a lower box body 20 that are relatively arranged. The upper box body 10 and the lower box body 20 are both arranged inside the cavity 30, wherein the upper box body 10 is used to carry the substrate, and the lower box body 20 is used to carry the evaporation source material.

[0046] It should be noted that the preparation process of thermoelectric film deposited by CSS method is relatively fast and can easily affect the microstructure of the thermoelectric film. Therefore, we have optimized the process steps and parameters.

[0047] In this step, the aluminum nitride substrate after plasma cleaning in step 1 is first fixed on the upper box body 10 of the CSS device, and the side on which the thermoelectric material film layer is to be deposited is set downward; the source material powder (i.e., antimony telluride powder or bismuth telluride powder) prepared in step 2 is spread flat in the lower box body 20 of the CSS device. Then, the thermoelectric material is deposited. In this embodiment, the specific parameters of the close-space sublimation are as follows: the heating temperature of the lower box body (i.e., antimony telluride powder or bismuth telluride powder) is 600°C, and the heating temperature of the upper box body (i.e., substrate) is 400°C; the distance between the upper and lower boxes ( Figure 1 The deposition distance (d in the figure) is 5 mm, the deposition time is 1 minute, and the deposition pressure is less than 10 -3 Pa, the thickness of the deposited thermoelectric film is about 10 μm.

[0048] We found that appropriately increasing the temperature of the substrate helps to improve the morphology and structure of the deposited thick thermoelectric film. In this embodiment, in order to further improve the morphology and structure of the thick thermoelectric film, the deposited film layer was subjected to in-situ annealing. Specifically, after the CSS deposition process is completed, the heating temperature of the substrate (i.e., 400 ° C) is maintained for 60 minutes, and the deposited thermoelectric film is subjected to in-situ annealing, thereby improving the morphology and structure of the thermoelectric film, and increasing the conductivity of the film layer by about 7 times at room temperature, from 10000-20000 S / m to about 105000 S / m.

[0049] In other embodiments, the heating temperature of the thermoelectric material is 600-800°C, the heating temperature of the substrate is 200-400°C; the deposition distance is 4-6 mm, the deposition time is 0.5-5 minutes, and the deposition pressure is less than 10 -3 Pa. Similarly, in-situ heat treatment can also be continued, with the heat treatment temperature being 200-400 °C and the time being 60-120 minutes.

[0050] The above is the preparation method of the thermoelectric film in this embodiment. Taking the prepared N-type thermoelectric material bismuth telluride film layer as an example, its morphology and structure are as follows: Figure 2 As shown. Using the CSS process, a thermoelectric film with a thickness of about 10 μm can be prepared in just 1 minute, which is significantly faster than the preparation speed of the magnetron sputtering process (about 1-2 μm per hour); and through the selection and processing of the substrate and the optimization of the CSS process, the thermoelectric film deposited by the CSS process has a good microstructure and is tightly bonded to the substrate without falling off.

[0051] In this application, the components and thermoelectric properties of the prepared thermoelectric film are further tested and analyzed. For the antimony telluride and bismuth telluride materials involved in this application, because the properties of the two are basically the same, one of them is selected for relevant testing. In this application, the prepared N-type thermoelectric material bismuth telluride film layer is tested and analyzed in detail, and the results are as follows.

[0052] The elemental composition of the prepared bismuth telluride film layer (when the atomic ratio of tellurium in the raw material is 65%) was analyzed, and the results are shown in Table 1. By taking three points on the film layer for elemental analysis, the content of bismuth element (atomic percentage) was between 40.7% and 41.5%, and its average content (atomic percentage) was about 41.1%; the content of tellurium element (atomic percentage) was between 58.5% and 59.3%, and its average content (atomic percentage) was about 58.9%. The deviation of the relative stoichiometric ratio of the two components was small, basically reaching the predetermined target.

[0053] Table 1: Elemental composition statistics of bismuth telluride films deposited by CSS process

[0054]

[0055] The thermoelectric properties of the prepared bismuth telluride film (when the atomic ratio of tellurium in the raw material is 65%) were tested. Figure 3 In this application, the thermoelectric performance test equipment is a thermoelectric comprehensive performance tester (CTA-3S / 1150), which can measure the Seebeck coefficient and conductivity of thermoelectric materials at different temperatures, and according to the formula PF=S 2 The power factor of the material is calculated by σ, where PF is the power factor, S is the Seebeck coefficient, and σ is the electrical conductivity. The test of thermoelectric performance is a prior art and will not be described in detail in this application. Figure 3 A and Figure 3 Figure B shows the Seebeck coefficient and conductivity of the bismuth telluride film at different test temperatures. It can be found that the film composition is ideal due to the optimization of the original powder composition formula, and the Seebeck coefficient of the film is high, reaching about -100 μV / K. Due to the effect of in-situ annealing, the conductivity of the film is greatly improved, exceeding 100,000 S / m at room temperature. The power factor of the film is also optimized to 10 μW / K 2 .cm, with good performance, meeting the requirements for thermoelectric materials in the preparation of thermoelectric devices.

[0056] Embodiment 2:

[0057] This embodiment provides a method for preparing a thermoelectric film, which is different from the first embodiment in the prepared thermoelectric material, that is, the atomic percentage of tellurium element in antimony telluride powder and bismuth telluride powder. In the first embodiment, the atomic percentage of tellurium element is 65%, while in the present embodiment, the atomic percentage of tellurium element is 62%, that is, in the present embodiment, for antimony telluride powder, the raw materials used are single antimony powder and single tellurium powder, respectively, and the atomic percentages of the two are 38% and 62%, respectively; similarly, for bismuth telluride powder, the raw materials used are single bismuth powder and single tellurium powder, respectively, and the atomic percentages of the two are 38% and 62%, respectively. In addition, the preparation method in this embodiment is consistent with that in the first embodiment.

[0058] In this embodiment, the bismuth telluride film layer was also tested and analyzed. The elemental composition of the bismuth telluride film layer prepared in this embodiment (when the atomic ratio of tellurium in the raw material is 62%) was analyzed, and the average content (atomic percentage) of bismuth element was about 43.6%, and the average content (atomic percentage) of tellurium element was about 56.4%. The thermoelectric performance of the bismuth telluride film layer (when the atomic ratio of tellurium in the raw material is 62%) was tested, and the results are as follows: Figure 3The Seebeck coefficient of the bismuth telluride film layer is slightly lower than that of the bismuth telluride film layer in Example 1, but it is also basically -80 μV / K to -100 μV / K. Its conductivity is relatively high, basically exceeding 100,000 S / m, and its power factor is also basically exceeding 8 μW / K. 2 .cm, which can basically meet the requirements of thermoelectric devices.

[0059] Embodiment three:

[0060] This embodiment provides a method for preparing a thermoelectric film, which is different from the first embodiment in the prepared thermoelectric material, that is, the atomic percentage of tellurium element in antimony telluride powder and bismuth telluride powder. In the first embodiment, the atomic percentage of tellurium element is 65%, while in the present embodiment, the atomic percentage of tellurium element is 67%, that is, in the present embodiment, for antimony telluride powder, the raw materials used are elemental antimony powder and elemental tellurium powder, respectively, and the atomic percentages of the two are 33% and 67%, respectively; similarly, for bismuth telluride powder, the raw materials used are elemental bismuth powder and elemental tellurium powder, respectively, and the atomic percentages of the two are 33% and 67%, respectively. In addition, the preparation method in this embodiment is consistent with that in the first embodiment.

[0061] In this embodiment, the bismuth telluride film layer is also tested and analyzed. The elemental composition of the bismuth telluride film layer prepared in this embodiment (when the atomic ratio of tellurium in the raw material is 67%) is analyzed, and the average content of bismuth element (atomic percentage) is about 39.2%; the average content of tellurium element (atomic percentage) is about 60.8%. The bismuth telluride film layer prepared at this ratio is already very close to the stoichiometric ratio. According to past experience, the film layer with the best thermoelectric performance should have a tellurium content slightly lower than 60%. In this embodiment, when the tellurium content of the original powder reaches 67%, the tellurium content of the prepared film layer has reached 60.8%, and the tellurium content of the original powder does not need to be further increased. The thermoelectric properties of the bismuth telluride film layer (when the atomic ratio of tellurium in the raw material is 67%) were tested, and the results are as follows: Figure 3 The Seebeck coefficient of the bismuth telluride film layer is slightly higher than that of the bismuth telluride film layer in Example 1, which is basically around -100 μV / K. Its conductivity is lower, which is roughly around 60000-80000 S / m, and its power factor is also over 8 μW / K. 2 .cm, which can also meet the requirements of thermoelectric devices.

[0062] Embodiment 4:

[0063] This embodiment provides a thermoelectric film, which is prepared according to the above-mentioned method for preparing a thermoelectric film.

[0064] Embodiment five:

[0065] The present embodiment provides a thermoelectric device, which includes an electrode layer and a thermoelectric arm, wherein the thermoelectric arm is prepared by the above-mentioned method for preparing a thermoelectric film. Specifically, the thermoelectric arm is a patterned thermoelectric film prepared on the surface of the electrode layer. After an antimony telluride film layer or a bismuth telluride film layer is prepared on the electrode layer according to the above-mentioned method for preparing a thermoelectric film, the patterning of the thermoelectric material can be achieved by wet etching or other process methods to obtain the thermoelectric arm. The specific parameters are not repeated here.

[0066] Comparative Example 1:

[0067] The difference between the preparation method of the thermoelectric film in this comparative example and that in Example 1 lies in the atomic percentage of tellurium element in the prepared thermoelectric material, i.e., antimony telluride powder and bismuth telluride powder. In this comparative example, the atomic percentage of tellurium element is 60%, that is, in this comparative example, for antimony telluride powder, the raw materials used are elemental antimony powder and elemental tellurium powder, respectively, and the atomic percentages of the two are 40% and 60%, respectively; similarly, for bismuth telluride powder, the raw materials used are elemental bismuth powder and elemental tellurium powder, respectively, and the atomic percentages of the two are 40% and 60%, respectively. In addition, the preparation method in this comparative example is consistent with that in Example 1.

[0068] The comparative example uses a normal composition of bismuth telluride powder (i.e., the atomic percentage of Te is 60%) to prepare the thermoelectric film component, and the atomic percentage of tellurium in the component is about 51.9%, which is quite different from the ideal composition. The thermoelectric performance of the bismuth telluride film layer of the comparative example was tested, and the results are as follows: Figure 4 The results show that its thermoelectric performance is extremely poor. The Seebeck coefficient of the bismuth telluride film is extremely low and has no obvious regular trend, only around -20 μV / K to -30 μV / K, while the conductivity is around 80000-90000 S / m, and the power factor is less than 1 μW / K. 2 .cm, basically 0.4-0.8 μW / K 2 The bismuth telluride film layer in this comparative example has basically no characteristics and properties of thermoelectric materials and cannot be used in the preparation of thermoelectric material film layers.

[0069] In order to facilitate the description, some common English nouns or letters used in the present invention are only used for exemplary reference rather than restrictive interpretation or specific usage, and the protection scope of the present invention should not be limited by their possible Chinese translations or specific letters.

[0070] It should also be noted that, in this document, relational terms such as "first" and "second" are merely used to distinguish one entity or operation from another entity or operation, and do not necessarily require or imply any actual relationship or order between these entities or operations.

Claims

1. A method for preparing a thermoelectric film, characterized in that: The steps include: S1. Providing a substrate and a thermoelectric material, wherein the thermoelectric material is antimony telluride powder or bismuth telluride powder, and the atomic percentage of tellurium in the thermoelectric material is between 62% and 67%; S2, using a close-space sublimation process to deposit the thermoelectric material on the substrate to form a thermoelectric film; The close-space sublimation process parameters are: the heating temperature of the thermoelectric material is 600-800°C, the heating temperature of the substrate is 200-400°C, the deposition distance is 4-6 mm, and the deposition pressure is less than 10 -3 Pa.

2. The method for preparing a thermoelectric film according to claim 1, characterized in that: After the close-space sublimation deposition, an in-situ annealing treatment is performed, with an annealing temperature of 200-400° C. and an annealing time of 60-120 minutes.

3. The method for preparing a thermoelectric film according to claim 1, characterized in that: The antimony telluride powder or the bismuth telluride powder is prepared by a mechanical alloying process.

4. The method for preparing a thermoelectric film according to claim 3, characterized in that: The antimony telluride powder is prepared by mechanical alloying of simple antimony powder and simple tellurium powder, and the content of the simple tellurium powder is 62%-67% by atomic percentage; The bismuth telluride powder is prepared by mechanical alloying single-substance bismuth powder and single-substance tellurium powder, and the content of the single-substance tellurium powder is 62%-67% in atomic percentage.

5. The method for preparing a thermoelectric film according to claim 1, characterized in that: The surface roughness of the substrate Ra is ≥50 nm.

6. The method for preparing a thermoelectric film according to claim 5, characterized in that: Before step S2, the substrate is subjected to plasma cleaning.

7. A thermoelectric film, characterized in that: The thermoelectric film is prepared according to the method for preparing the thermoelectric film according to any one of claims 1 to 6.

8. A thermoelectric device, characterized in that: It comprises an electrode layer and a thermoelectric arm, wherein the thermoelectric arm is a patterned thermoelectric film, and the thermoelectric arm is obtained by preparing a thermoelectric film on the electrode layer and patterning the thermoelectric film according to the method for preparing a thermoelectric film according to any one of claims 1 to 6.

Citation Information

Patent Citations

  • Preparation method of P-type bismuth telluride-based bulk thermoelectric material (Bi1-xSbx)2Te3

    CN109851360A

  • Fabrication Methods of Bismuth Telluride-based Thermoelectric Thin Films Using Co-evaporation of Alloy Composition Source and Tellurium Source and Thermoelectric Thin Films produced using ...

    KR101268609B1

  • Bismuth telluride-based thermoelectric nanocomposites with dispersed nano-sized silicon carbide based on the recycling of bismuth telluride processing scraps and preparation method thereof

    US20220254976A1