Laser annealing device and laser annealing method
By optimizing the shape and configuration of the beam spot in the laser annealing device, the problem of substrate bending and cracking caused by the long side of the beam spot is solved, high-quality crystallized area formation and substrate safety are achieved, and the stability of large-scale LCDs is ensured .
Patent Information
- Application Number
- CN202380023503.8
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Priority Date
- 2022-03-09
- Filing Date
- 2023-01-26
- Publication Date
- 2024-10-01
AI Technical Summary
During the laser annealing process, the heat generated due to the elongation of the rectangular long side of the beam spot causes tensile stress in the substrate, resulting in bending and cracking of the glass substrate, and the progress of thinning of large LCDs makes the glass substrate susceptible to damage and reduces the annealing Temperature affects film quality and the growth of single-crystal silicon-like films.
Design a laser annealing device in which the beam spot is parallel along the direction orthogonal to the scanning direction, and the length of the long side is set to be shorter than the length that causes damage to the substrate due to internal stress. By adjusting the distance of the beam spot and the scanning time, the thermal stress in the substrate is ensured. Within a safe range, multiple laser beams are selectively illuminated and intensity modulated to form a square beam spot to uniformly illuminate the amorphous silicon film.
It effectively avoids crystal peeling and damage to the glass substrate, improves the uniformity of the film quality, can form a high-quality strip or full-surface annealed crystallization area, reduces the thermal stress of the substrate, and avoids the breakage of the glass substrate.
Smart Images

Figure CN118742994A_ABST
Abstract
Description
Technical Field
[0001] The invention relates to a laser annealing device and a laser annealing method. Background Art
[0002] There is known a laser annealing device that can form a linearly extending single-crystal silicon film (crystallized region) in a stripe shape relative to an amorphous silicon film on a substrate (see, for example, Patent Document 1). This single-crystal silicon film is used as a semiconductor film for forming thin-film transistors (TFTs) arranged in a row along the long side direction.
[0003] The laser annealing device has an optical head on which the exit-side ends of a plurality of optical fibers are arranged. The core shape of the exit-side ends of the optical fibers is circular, and is arranged to form a row at predetermined intervals along a predetermined straight line on the light exit surface of the optical head. Usually, in the laser annealing device, the optical head is arranged in such a manner that the predetermined straight line on the light exit surface is orthogonal to the scanning direction, and the crystallization laser annealing is performed while scanning relative to the amorphous silicon film. In addition, in the laser annealing device, the optical head is rotated and moved at an arbitrary angle relative to the direction orthogonal to the scanning direction in a state where the optical head is opposed to the amorphous silicon film, thereby adjusting the intervals between the linear crystallized regions produced.
[0004] In recent years, the number of TFTs in thin displays (FPD: Flat Panel Display) such as liquid crystal displays (LCD: Liquid Crystal Display) and organic EL displays (OLED: Organic Electroluminescence Display) has increased and integration has continued to progress. Along with this, it is necessary to form a wide band-shaped crystallization region and a crystallization region that is annealed on the entire surface relative to the TFT substrate. In the case of forming such a wide crystallization region by laser annealing, in order to make the element characteristics of the TFT made in this region uniform, the in-plane uniformity of the film quality of the crystallization region becomes particularly important. Therefore, it is desired that the irradiation conditions (irradiation time, beam irradiation amount, etc.) of the laser beam irradiated to the crystallization region are the same at any position in the direction orthogonal to the scanning direction (width direction of the crystallization region). Therefore, the shape of the beam spot of the laser beam emitted from the laser annealing device is preferably a rectangle with a fixed beam width (length in the scanning direction) at any position along the direction orthogonal to the scanning direction.
[0005] Prior art literature
[0006] Patent Literature
[0007] Patent Document 1: International Publication No. 2021 / 039920 Summary of the invention
[0008] Problem that the invention aims to solve
[0009] However, when the length of the beam spot in the direction orthogonal to the scanning direction (the length of the long side of the rectangle) becomes longer, the glass substrate bends due to the tensile stress in the substrate caused by the heat generated by annealing. Therefore, problems such as crystal peeling or cracks in the glass substrate occur. From the perspective of processing efficiency, it is preferred to increase the length of the beam spot in the direction orthogonal to the scanning direction. It is speculated that this phenomenon is because when the beam spot is too long in the direction orthogonal to the scanning direction, the efficiency of heat dissipation from the area generated by annealing is reduced, and internal stress accumulates in the substrate. In recent years, the size and thinness of displays have further progressed, and there are concerns that the glass substrate is easily damaged and cracked as the width and area of the crystallization area increase. By the way, even in the case of large-scale liquid crystal displays (60 inches) in recent years, the thickness of the standard glass substrate is only about 2.8 mm. The thinner the glass substrate, the more likely it is to be mechanically damaged. Furthermore, in the production of a quasi-single-crystal silicon film having high electron mobility, if the annealing temperature is lowered in order to prevent damage to the glass substrate, the film quality will be degraded and the quasi-single-crystal growth itself will become difficult.
[0010] The present invention has been completed in view of the above-mentioned problems, and its purpose is to provide a laser annealing device and a laser annealing method that do not cause damage such as crystal peeling or cracks on the glass substrate, are of high quality and have high in-plane uniformity, and can form a band-shaped crystallized region or a crystallized region that is annealed on a substantially entire surface.
[0011] Solutions for solving problems
[0012] In order to solve the above-mentioned problems and achieve the purpose, the scheme of the present invention is a laser annealing device, which has a plurality of beam emitting parts for emitting laser beams, wherein the laser beam is composed of a continuously oscillating laser and has a square beam spot relative to the irradiated surface, and the laser annealing device causes the laser beam to scan relative to an amorphous silicon film formed on a substrate along a scanning direction, thereby crystallizing a band-shaped area to be modified in the amorphous silicon film, characterized in that one side of the beam spot is parallel to a direction orthogonal to the scanning direction, and the length of the one side of the beam spot is set to be shorter than the length of the substrate being damaged due to internal stress, wherein the internal stress is a stress inherent to the substrate generated along with the heating caused by the irradiation of the laser beam.
[0013] As the above-mentioned scheme, it is preferred that, on the surface of the amorphous silicon film, with respect to the beam spots of the laser beam emitted from each of the beam emitting portions, within the substrate surface of the substrate, when observed from a direction orthogonal to the scanning direction, the beam spots adjacent to each other along the direction orthogonal to the scanning direction are arranged relative to each other at a distance along the scanning direction that is longer than a distance corresponding to the following scanning time, wherein the scanning time is the time for the temperature of the predetermined modification area heated by the irradiation of the laser beam to drop to below the crystallization temperature of silicon.
[0014] As the above scheme, it is preferred that the distance equivalent to the scanning time required for the temperature of the modified predetermined area heated by the irradiation of the laser beam to drop below the crystallization temperature of silicon is calculated based on the thickness of the substrate, the thickness of the amorphous silicon film, the thermal diffusion capacity of the amorphous silicon film and the material film thereunder, the irradiation amount of the laser beam, and the relative scanning speed of the laser beam.
[0015] As the above aspect, preferably, the plurality of laser beams can be selectively lit.
[0016] As the above aspect, it is preferable that the intensity of the laser beam emitted from the beam emitting section can be modulated.
[0017] As the above scheme, preferably, the beam emitting portion is one end of an optical fiber, the other end of the optical fiber is connected to a light source emitting a continuous oscillation laser, and the shape of the beam spot is set using the shape of the end face of the beam emitting portion.
[0018] Another embodiment of the present invention is a laser annealing device, which has a plurality of beam emitting parts for emitting laser beams, wherein the laser beams are composed of continuously oscillating lasers and have square beam spots relative to an irradiated surface, and the laser annealing device causes the laser beam to scan relative to an amorphous silicon film formed on a substrate along a scanning direction to crystallize a band-shaped area to be modified of the amorphous silicon film, characterized in that one side of the beam spot is parallel to a direction orthogonal to the scanning direction, and when observed from the scanning direction, the beam spots of the laser beams emitted from the plurality of beam emitting parts are continuously arranged over the entire width of the area to be modified, and within the substrate surface of the substrate, the beam spots adjacent to each other along a direction orthogonal to the scanning direction are separated from each other along the scanning direction when observed from the direction orthogonal to the scanning direction.
[0019] As the above scheme, it is preferred that the length of the side of the beam spot is set to be shorter than the length of the substrate being damaged due to internal stress, wherein the internal stress is a stress inherent to the substrate generated along with the heating caused by the irradiation of the laser beam, and the beam spots adjacent to each other along the direction orthogonal to the scanning direction are arranged to be separated from each other along the scanning direction by a distance longer than a distance corresponding to the following scanning time, wherein the scanning time is the time for the temperature of the modified predetermined area heated by the irradiation of the laser beam to drop below the crystallization temperature of silicon.
[0020] As the above scheme, it is preferred that the distance equivalent to the scanning time required for the temperature of the modified predetermined area heated by the irradiation of the laser beam to drop below the crystallization temperature of silicon is calculated based on the thickness of the substrate, the thickness of the amorphous silicon film, the thermal diffusion capacity of the amorphous silicon film and the material film thereunder, the irradiation amount of the laser beam, and the relative scanning speed of the laser beam.
[0021] As the above aspect, preferably, the plurality of laser beams can be selectively lit.
[0022] As the above aspect, it is preferable that the intensity of the laser beam emitted from the beam emitting section can be modulated.
[0023] As the above scheme, preferably, the beam emitting portion is one end of an optical fiber, the other end of the optical fiber is connected to a light source emitting a continuous oscillation laser, and the shape of the beam spot is set using the shape of the end face of the beam emitting portion.
[0024] Another embodiment of the present invention is a laser annealing method, which irradiates a plurality of laser beams composed of continuously oscillating lasers and having square beam spots relative to the irradiated surface of an amorphous silicon film formed on a substrate from a plurality of beam emitting portions, and in this state, the plurality of laser beams are scanned relative to the substrate along a scanning direction to crystallize a band-shaped predetermined modification area of the amorphous silicon film, characterized in that the laser annealing method includes the following steps: performing a preliminary test on the substrate to adjust and set the distance between the plurality of beam emitting portions so that the distance between the beam spots becomes a distance that does not cause thermal stress cracking due to laser heating; and thereafter scanning the plurality of laser beams relative to the substrate to perform laser annealing.
[0025] As the above aspect, it is preferable that the preliminary test is performed by performing a thermal stress test using the test substrate.
[0026] As the above aspect, it is preferable that the preliminary test is performed as a simulation.
[0027] Effects of the Invention
[0028] According to the laser annealing apparatus and the laser annealing method of the present invention, crystal peeling and damage to the glass substrate will not occur, the film quality is highly uniform, and a band-shaped crystallized region or a substantially entire annealed crystallized region can be formed. BRIEF DESCRIPTION OF THE DRAWINGS
[0029] Figure 1 1 is a schematic structural diagram showing a laser annealing apparatus according to an embodiment of the present invention.
[0030] Figure 2 It is an explanatory diagram of an optical fiber array of a laser annealing device according to an embodiment of the present invention.
[0031] Figure 3 It is a cross-sectional explanatory diagram showing a state where a laser beam is scanned with respect to an amorphous silicon film.
[0032] Figure 4 This is a plan view for explaining the arrangement relationship of beam spots in the laser annealing device according to the embodiment of the present invention based on the arrangement of the core of the optical fiber.
[0033] Figure 5 It is an explanatory diagram showing the relationship between the length of the long side of the beam spot in the laser annealing apparatus and the bending stress on the back surface of the substrate.
[0034] Figure 6 This is a diagram showing the relationship between the distance in the scanning direction from the center of the beam of the laser annealing device and the temperature in the film to be processed.
[0035] Figure 7 The graph shows the relationship between the distance in the scanning direction from the beam center of the laser beam and the temperature, and illustrates the stable temperature distribution on the surface of the amorphous silicon film accompanying the movement of the laser beam.
[0036] Figure 8 This is an explanatory diagram showing Example 1 in which a plurality of linear crystallized regions are formed in stripe shapes using the laser annealing apparatus according to the embodiment of the present invention.
[0037] Fig. 9 This is an explanatory diagram showing Example 2 in which a plurality of band-shaped crystallized regions are formed in a stripe shape using the laser annealing apparatus according to the embodiment of the present invention.
[0038] Fig.10 This is an explanatory diagram showing Example 3 in which a crystallized region annealed substantially over the entire surface is formed using the laser annealing apparatus according to the embodiment of the present invention.
[0039] Fig.11 This is a plan view for explaining a modified example of the arrangement relationship of beam spots of the laser annealing device according to the embodiment of the present invention based on the arrangement of the core of the optical fiber. DETAILED DESCRIPTION
[0040] The laser annealing device according to the embodiment of the present invention is described in detail below based on the accompanying drawings. However, it should be noted that the accompanying drawings are schematic, and the number of components, the size of each component, the ratio of the size, the shape, etc. are different from the actual ones. In addition, the drawings also include parts with different size relationships, ratios, or shapes.
[0041] (Schematic Structure of Laser Annealing Device)
[0042] like Figure 1 As shown, the laser annealing apparatus 1 of this embodiment is generally configured to include a light source unit 2, an optical head 3, a stage 20 for mounting a substrate 10 to be processed, and a substrate transport mechanism (not shown) for moving the substrate 10 to be processed in a predetermined scanning direction.
[0043] The light source unit 2 includes, for example, 24 semiconductor lasers LD as light sources. Figure 1 In FIG. 1 , only four semiconductor lasers LD1 a to LD1 d are shown. It should be noted that in the present embodiment, for convenience of description, the number of semiconductor lasers LD is set to 24, but the present invention is not limited thereto and can be appropriately changed.
[0044] These semiconductor lasers LD oscillate continuously oscillated lasers (CW lasers). Here, continuously oscillated lasers are a concept that also includes so-called quasi-continuous oscillations that continuously irradiate laser light to a target area. That is, the laser can be a pulsed laser, or a quasi-continuous oscillation laser whose pulse interval is shorter than the cooling time of the heated silicon thin film (amorphous silicon film) (irradiated with the next pulse before solidification). It should be noted that in this embodiment, as the semiconductor laser LD, a semiconductor laser with a wavelength of 445nm to 455nm is used.
[0045] As the light source, various lasers such as a solid-state laser, a liquid laser, and a gas laser can be used in addition to the semiconductor laser LD.
[0046] The light source unit 2 includes the above-mentioned plurality of semiconductor lasers LD, a plurality of coupling lenses 21 arranged at positions corresponding to the light emitting sides of the semiconductor lasers LD, respectively, a driving circuit (not shown), and the like.
[0047] The driving circuit is connected to a plurality of semiconductor lasers LD respectively to drive each semiconductor laser LD. In the present embodiment, these semiconductor lasers LD are configured to be selectively lit. Furthermore, the driving circuit is configured to be capable of driving the laser beams emitted from these semiconductor lasers LD to modulate the intensity.
[0048] The optical head 3 includes an optical fiber array 31 and an imaging optical system 32. Figure 1 and Figure 2 As shown, the optical fiber array 31 has one end of optical fibers 41 to 44, 51 to 54, 61 to 64, 71 to 74, 81 to 84, and 91 to 94 serving as waveguides. Figure 2 The configuration relationships shown are connected in this manner.
[0049] The following describes the arrangement relationship between the beam spots of the laser beam LB emitted from these optical fibers 41 to 94. The other ends of the optical fibers 41 to 94 are connected to positions corresponding to the light emitting side of the coupling lens 21. In this embodiment, multimode optical fibers are used as the optical fibers 41 to 94.
[0050] like Figure 1 As shown, the imaging optical system 32 includes at least a first lens 33 on the incident side and a second lens 34 on the emission side. In this embodiment, the imaging optical system 32 is configured to project the laser light incident from the optical fiber array 31 side onto the irradiated surface of the substrate 10 at the same magnification.
[0051] like Figure 3 As shown, the substrate to be processed 10 mainly comprises a glass substrate 11. On the glass substrate 11, an insulating film 12 such as a silicon nitride film (Si3N4) or a silicon oxide film (SiO2) and a processed film 13 made of amorphous silicon are formed.
[0052] The substrate transport unit (not shown) is provided with a mechanism for transporting the substrate 10 to be processed by laser annealing at an arbitrary speed in the scanning direction. Therefore, by transporting the substrate 10 to be processed in the direction opposite to the scanning direction while the position of the optical head 3 is fixed, the laser beam LB is scanned relative to the substrate 10.
[0053] (Arrangement Relationship of Optical Fibers in the Present Embodiment)
[0054] As described above, in the present embodiment, the imaging optical system 32 is configured to project the laser light incident from the optical fiber array 31 side onto the irradiated surface of the substrate 10 at equal magnification. Therefore, the configuration relationship between the ends of the optical fibers 41 to 94 on the light emitting surface of the optical fiber array 31 is set to be the same as the configuration relationship between the beam points of the laser beam LB emitted from the ends of the optical fibers 41 to 94 onto the irradiated surface.
[0055] Therefore, in this embodiment, for convenience of explanation, as the arrangement relationship of the beam spots, the arrangement relationship of one end portions of the optical fibers 41 to 94 which are the emission surfaces of the laser beams will be used for explanation.
[0056] Figure 21 is an explanatory diagram showing the arrangement positions of one end portions (light emitting surfaces) of the optical fibers 41 to 94 when the optical fiber array 31 is viewed from above. Figure 2 This is an explanatory diagram showing the optical fiber array 31 projected onto the side of the substrate to be processed 10 located below. Each of the optical fibers 41 to 94 is composed of a core passing through the center and a cladding covering the periphery thereof.
[0057] If Figure 1 The optical fibers 41 to 44 are shown as follows. Figure 2 As shown, these optical fibers 41 to 44 have cores 41a, 42a, 43a, 44a and claddings 41b, 42b, 43b, 44b covering the periphery thereof. Other optical fibers 51 to 54, 61 to 64, 71 to 74, 81 to 84, 91 to 94 also have the same structure of having a core and a cladding, and are marked with reference numerals in the figure and their description is omitted.
[0058] At least one end of the core of each of the optical fibers 41 to 44, 51 to 54, 61 to 64, 71 to 74, 81 to 84, and 91 to 94 is in the shape of a rectangular prism. Figure 2 As shown, one end face (light beam emitting portion) of each core is formed into a rectangle of the same size. One end face of the core is configured so that the long side (one side) of the rectangle is parallel to the direction (X) orthogonal to the scanning direction (Y). It should be noted that in the present embodiment, one end face of the core is a rectangle, but is not limited to a rectangle, as long as it is a square including a square. That is, as in the present embodiment, one end face of the core is a rectangle that is long in the direction orthogonal to the scanning direction, but it can also be a rectangle that is long in the scanning direction.
[0059] Figure 4 1 is a diagram for explaining the configuration in which the cores 44a, 54a, 64a of the optical fibers 44, 54, 64 are projected onto the side of the substrate 10 to be processed. Figure 4 As shown in FIG. 1 , the length (L) of the long side of one end face (beam emitting portion) of each core 44a, 54a, 64a is set to be shorter than the length obtained by the simulation described later. The length (L) is set to be shorter than the length at which the glass substrate 11 is damaged due to internal stress, wherein the internal stress is a stress inherent to the substrate 10 to be processed that is generated by heating caused by irradiation with the laser beam. In the present embodiment, the length (L) of the long side is less than 1 mm, preferably less than 0.5 mm.
[0060] Incidentally, in this embodiment, the beam spot size of the laser beam is set to a rectangular shape with a long side of 100 μm (0.1 mm) and a short side of 20 μm (0.02 mm). In addition, the power density of the laser beam is set to 170 kW / cm 2 .
[0061] Figure 5 The simulation results are obtained by simulating the stress generated during annealing (bending stress on the back of the substrate) when the length of the long side (L) is changed based on the rectangular beam spot under the above conditions. The simulation was performed by thermal stress analysis using the finite element method. Figure 5 It can be seen that when the length (L) of the long side exceeds 2 mm, the bending stress on the back of the substrate becomes about 55 [MPa]. Incidentally, at this time, the stress generated on the surface of the processed substrate 10 and the end of the beam spot exceeds 100 MPa, and the glass substrate 11 becomes a broken state. When the length (L) of the long side is less than 1 mm, the bending stress on the back of the substrate is suppressed to less than 30 [MPa]. In addition, when the length (L) of the long side becomes less than 0.5 mm, the bending stress on the back of the substrate can be suppressed to a very low level.
[0062] like Figure 2 As shown, the optical fiber array 31 is formed by combining six support blocks 40, 50, 60, 70, 80, and 90. For example, optical fibers 41, 42, 43, and 44 are arranged at equal intervals on the support block 40. Optical fibers are also arranged at equal intervals on the other support blocks 50, 60, 70, 80, and 90.
[0063] In addition, in each of the support blocks 40, 50, 60, 70, 80, and 90, the optical fiber is arranged so that the arrangement position is sequentially shifted by the length (L) of the long side of one core along the long side direction (X direction). Figure 2 As shown, when the six support blocks 40, 50, 60, 70, 80, and 90 are overlapped to form the optical fiber array 31, when viewed from the Y direction, the cores 41a, 51a, 61a, 71a, 81a, and 91a are arranged adjacent to each other in sequence along the X direction.
[0064] Similarly, cores 42a, 52a, 62a, 72a, 82a, and 92a are arranged adjacent to each other in order along the X direction when viewed from the Y direction. Here, core 94a and core 43a are arranged adjacent to each other along the X direction when viewed from the Y direction.
[0065] The cores 43a, 53a, 63a, 73a, 83a, and 93a are arranged so as to be adjacent to each other in order along the X direction when viewed from the Y direction. Here, the core 93a and the core 42a are arranged at positions adjacent to each other along the X direction when viewed from the Y direction.
[0066] The cores 44a, 54a, 64a, 74a, 84a, and 94a are arranged so as to be adjacent to each other in sequence along the X direction when viewed from the Y direction. Here, the core 92a and the core 41a are arranged at positions adjacent to each other along the X direction when viewed from the Y direction. As described above, in the present embodiment, the beam spots are arranged continuously when viewed from the scanning direction. In addition, when viewed from a direction orthogonal to the scanning direction, the beam spots adjacent to each other in the direction orthogonal to the scanning direction are arranged to be spaced apart from each other by a predetermined distance (Dy).
[0067] Figure 6 This is a diagram obtained by simulating multiple situations with different scanning speeds, showing the stable temperature distribution on the surface of the silicon film formed by the movement of the laser beam LB. Figure 6 In the simulation, the scanning direction of the laser beam LB is the (+) direction of the x-axis. The scanning speed is 100 to 500 [mm / s] (100 mm / s interval). The highest temperature (peak temperature) moves backward from the center of the beam [0]. According to the simulation results, for example, Figure 6 As shown in the figure, when the scanning speed is 400 mm / s, Figure 4 The distance (Dy) shown may be 0.05 mm (50 μm) or more. When the scanning speed is 300 mm / s, the distance (Dy) may be 0.08 mm (80 μm).
[0068] Figure 7 This is a diagram showing an example of simulation results of the film temperature change after annealing, that is, after scanning by the laser beam LB, and is plotted by changing the scale of the horizontal axis (the distance from the center of the beam). Figure 6 The graph of the curve of v = 200mm / s. The film temperature during laser annealing temporarily exceeds the melting point of silicon 1410°C. Depending on the conditions, it sometimes exceeds 2000°C. After the laser beam LB passes, the temperature decreases as the distance from the beam point increases. It should be noted that in the above simulation, the calculation is based on the thickness of the substrate, the thickness of the amorphous silicon film, the thermal diffusion capacity of the amorphous silicon film and the material film below it, the irradiation amount of the laser beam, and the relative scanning speed of the laser beam.
[0069] like Figure 7 As shown in FIG. 1 , when the scanning distance from the center of the beam is 6 mm, the substrate temperature (film temperature) becomes less than 200°C. When the distance is 13 mm, it becomes less than 150°C. Figure 2 and Figure 4In the configuration relationship shown, in the case of full-surface annealing, the area to be modified can be annealed uniformly by leaving a distance (Dy) longer than a distance corresponding to the following scanning time, wherein the scanning time refers to the time it takes for the temperature of the area to be modified to drop below the crystallization temperature of silicon after being heated by the laser beam previously performed during the scanning.
[0070] It is desirable that, among beam spots adjacent to each other in the direction X perpendicular to the scanning direction, the film temperature is sufficiently lowered when the subsequent beam spot reaches the vicinity of the position heated by the preceding beam spot during scanning. Figure 7 As shown in FIG. 1 , the desired film temperature is 200° C. or less, and further 150° C. or less. Figure 7 According to the simulation results, the desired distance Dy is greater than 7 mm, and more preferably greater than 13 mm.
[0071] The distance Dy corresponding to the scanning time required for the temperature of the amorphous silicon 13a in the modified predetermined area to drop to below the temperature at which silicon crystallizes (approximately 1406°C) after being heated by the irradiation of the above-mentioned laser beam LB can be calculated based on the thickness of the processed substrate 10, the thickness of the amorphous silicon 13a, the thermal diffusion capacity of the amorphous silicon 13a and the material film beneath it, the irradiation amount of the laser beam, and the relative scanning speed of the laser beam LB.
[0072] In addition, as for the film temperature, good crystals can be obtained between 1400°C and 1600°C, but when it exceeds about 1600°C, film ablation occurs. Therefore, it is preferable to control the temperature within the range of 1400°C to 1600°C.
[0073] In the case where the distance Dy cannot be made greater than 5 mm, for example, it may be considered to modulate the intensity of the subsequent beam spot to a low irradiation energy based on the temperature rise caused by the preceding beam spot. In the above-mentioned embodiment, all semiconductor lasers LD are driven by inputting the same power. However, in Figure 2 and Figure 4 In the arrangement shown, it is also possible to set the input power of the semiconductor laser LD to be independently controllable, and to perform current control on the input power of each semiconductor laser LD under the condition that the film temperature becomes constant.
[0074] In the above-mentioned embodiment, the scanning speed at which the laser beam LB relatively scans the film to be processed 13 is preferably 200 mm to 500 mm / sec, but the present invention is not limited thereto.
[0075] It should be noted that, in this embodiment, Figure 2As shown, a structure is adopted in which each of the six support blocks 40, 50, 60, 70, 80, and 90 has four cores, but a structure in which each has one core may also be adopted. The number of support blocks and cores is not limited to the number in the above embodiment.
[0076] (Configuration relationship of the beam spot on the substrate of the present invention)
[0077] The original arrangement conditions of the beam spot on the irradiated surface (processed surface) in the present invention including this embodiment are as follows.
[0078] That is, the arrangement relationship of the beam spots of the present invention may satisfy the following conditions (1) to (5).
[0079] (1) The beam spot is square.
[0080] (2) One side of the square of the beam spot is parallel to a direction (X direction) orthogonal to the scanning direction (Y direction).
[0081] (3) The length (L) of one side of the rectangle of the beam spot is set to be shorter than the length that causes the glass substrate 11 to be damaged due to internal stress, wherein the internal stress is stress inherent to the substrate 10 to be processed that is generated by heating caused by irradiation with the laser beam LB.
[0082] (4) On the surface of the film to be processed 13, the respective beam spots are arranged continuously when viewed from the scanning direction (Y direction).
[0083] (5) When viewed from a direction (X direction) perpendicular to the scanning direction (Y direction), the beam spots adjacent to each other along the direction (X) perpendicular to the scanning direction (Y direction) are separated from each other by a distance Dy (refer to Figure 4 ) are mutually configured, wherein the scanning time refers to the time it takes for the temperature of the processed film 13, which has been heated by the irradiation of the laser beam LB, to drop below the crystallization temperature of silicon.
[0084] (Operation and Effect of Laser Annealing Apparatus of the Present Embodiment)
[0085] First, the substrate 10 to be processed is placed on the stage 20 , and the optical head 3 is positioned at the annealing start position of the substrate 10 to be processed.
[0086] At this time, the light beam emitting part (core in this embodiment) to be lit in the optical head is set in advance according to the planned modification area. It should be noted that here, the case where a plurality of light beam emitting parts adjacent to each other when viewed from the scanning direction are lit to crystallize the processed film 13 into a strip shape is described.
[0087] Next, the substrate 10 to be processed starts to move in the scanning direction at a predetermined speed by a transport mechanism (not shown), and at the same time, irradiation of the laser beam LB from the optical head starts. Figure 3 As shown, the laser beam LB is scanned relative to the substrate 10 to be processed, and the amorphous silicon 13a forming the film 13 to be processed irradiated by the rectangular beam spot is melted into molten silicon 13m, and after a predetermined time, a band-shaped quasi-single crystal silicon 13p is crystallized.
[0088] By scanning with the laser beam LB in this way, the crystallization of the region to be modified of the film 13 to be processed is completed.
[0089] In the present embodiment, the long side of the rectangular beam spot is parallel to a direction orthogonal to the scanning direction, and the length (L) of the long side is set to be shorter than the length of the glass substrate 11 that is damaged due to internal stress, wherein the internal stress is a stress inherent to the processed substrate 10 that is generated along with the heating caused by the irradiation of the laser beam LB. Therefore, it is possible to suppress the occurrence of damage to the glass substrate 11 and crystal peeling associated with laser annealing.
[0090] In addition, in the present embodiment, the beam spots are arranged continuously when viewed from the scanning direction. In addition, when viewed from a direction perpendicular to the scanning direction, the beam spots adjacent to each other in the direction perpendicular to the scanning direction are arranged at a predetermined distance (Dy) from each other. The distance (Dy) is a distance longer than the scanning time corresponding to the temperature of the modified area (film to be processed 13) heated by the irradiation of the laser beam is reduced to below the crystallization temperature of silicon.
[0091] Therefore, when the area of the processed film 13 irradiated by the beam spot of the previous scan moves to the vicinity of the beam spot of the subsequent scan among the beam spots adjacent to each other when viewed from the scanning direction, the film temperature of the area irradiated in advance can be sufficiently lowered. Therefore, it is possible to prevent excessive temperature rise caused by the subsequent scan, and it is possible to suppress damage to the glass substrate 11 or peeling of crystals.
[0092] It should be noted that in this embodiment, based on the thickness of the processed substrate 10, the thickness of the amorphous silicon film (processed film 13), the thermal diffusion capacity of the amorphous silicon film and the material film beneath it, the irradiation amount of the laser beam LB, and the relative scanning speed of the laser beam LB, the distance equivalent to the scanning time required for the temperature of the planned modification area (film temperature) heated by the irradiation of the laser beam to drop to below the crystallization temperature of silicon is calculated, so that the distance can be easily calculated.
[0093] (Laser Annealing Method of This Embodiment)
[0094] The laser annealing method of the present embodiment is the following laser annealing method: a plurality of laser beams LB having square beam spots composed of continuously oscillating lasers are irradiated from a plurality of beam emitting parts. In this state, the plurality of laser beams LB are scanned relative to the substrate to be processed 10 along a scanning direction to crystallize the band-shaped predetermined modification area of the amorphous silicon film (film to be processed) 13.
[0095] First, a preliminary test is performed on the substrate 10 to be processed, and the distances between the multiple beam emitting parts are adjusted and set so that the distances between the beam spots are such that thermal stress cracking caused by laser heating will not occur. Thereafter, the multiple laser beams LB are scanned relative to the substrate 10 to be processed to perform laser annealing. Specifically, the long side (one side) of the beam spot is set to be parallel to the direction orthogonal to the scanning direction. Furthermore, when viewed from the scanning direction, the beam spots of the laser beams LB emitted from the multiple beam emitting parts are continuously arranged over the entire width of the predetermined modification area in the processed film 13. Within the substrate surface of the glass substrate 11, the beam spots adjacent to each other in the direction orthogonal to the scanning direction are arranged to be separated from each other along the scanning direction by the distance obtained in the above-mentioned preliminary test when viewed from the scanning direction.
[0096] In this laser annealing method, the length of the long side (one side) of the beam spot is set shorter than the length at which the glass substrate 11 is damaged by internal stress inherent to the glass substrate 11 generated by heating due to irradiation with the laser beam.
[0097] In addition, in the laser annealing method, the beam spots adjacent to each other in the direction orthogonal to the scanning direction are arranged to be separated from each other by a distance along the scanning direction that is longer than a distance corresponding to a scanning time for the temperature of the region to be modified, which is heated by irradiation of the laser beam, to be lowered to a temperature below the crystallization temperature of silicon. It should be noted that, as a preliminary test, a thermal stress test or simulation is performed using a test substrate.
[0098] (Example 1)
[0099] Figure 8 1 is a top view illustrating Example 1 in which linear quasi-single-crystal silicon 13p is produced in a stripe shape using the laser annealing device of this embodiment. This Example 1 is an example in which cores 44a, 53a, 62a, and 71a corresponding to the positions separating the linear quasi-single-crystal silicon 13p to be formed in a stripe shape are selected as cores to be lit in the optical fiber array 31. According to Example 1, a thin and long region of quasi-single-crystal silicon 13p can be formed along the scanning direction.
[0100] (Example 2)
[0101] Fig. 91 is a top view of Example 2 in which a wide-width strip-shaped quasi-single-crystal silicon 13p is produced in a stripe shape using the laser annealing device of the present embodiment. This Example 2 is an example in which a plurality of cores 44a, 54a, 64a, 74a, 84a, 94a that are continuous with each other when viewed from the scanning direction (Y direction) are selected as cores to be lit in the optical fiber array 31. According to Example 2, a wide-width quasi-single-crystal silicon 13p region can be formed along the scanning direction. It should be noted that by moving the optical fiber array 31 in which the cores 44a, 54a, 64a, 74a, 84a, 94a are selected in this way in the X direction to scan again, a wide-width quasi-single-crystal silicon 13p region can be formed in a stripe shape.
[0102] In this second embodiment, by irradiation with the laser beam LB from each core, linear regions of the quasi-single-crystal silicon 13p can be fused together to form a crystallized region of uniform film quality.
[0103] (Example 3)
[0104] Fig.10 This is a top view of Example 3 showing the case where substantially whole-surface annealing is performed in a wider region using the laser annealing apparatus of this embodiment to produce a region of quasi-single-crystal silicon 13p. This Example 3 uses all the cores in the optical fiber array 31 by lighting them. According to Example 3, substantially whole-surface annealing can be performed efficiently.
[0105] In this third embodiment, by irradiation with the laser beam LB from the entire core, a large number of adjacent linear regions of quasi-single-crystal silicon 13p can be fused together to form a crystallized region having a uniform film quality that is annealed over substantially the entire surface.
[0106] According to the present embodiment and Examples 1 to 3 described above, no crystal peeling or cracking of the glass substrate 11 will occur, and the glass substrate 11 has high quality and in-plane uniformity, and can form linear crystallized regions, band-shaped crystallized regions, and wide crystallized regions that are annealed over the entire surface.
[0107] (Other embodiments)
[0108] Although the embodiments of the present invention have been described above, it should not be understood that the description and drawings forming part of the disclosure of the embodiments limit the present invention. Various alternative embodiments, examples, and operation techniques will be apparent to those skilled in the art from this disclosure.
[0109] In the above-described embodiment, the imaging optical system 32 employs equal-magnification projection for projecting the laser light incident from the optical head 3 side onto the processing surface of the processing substrate 10 with the same size, but the present invention is not limited thereto.
[0110] In the above-mentioned embodiment, a substrate transport mechanism is used to transport the substrate 10 to be processed by laser annealing in the scanning direction at an arbitrary speed, but it can also be configured to have a gantry that moves the optical head 3 side along the scanning direction while the position of the substrate 10 side is fixed.
[0111] In the above-mentioned embodiment, the configuration relationship of the cores 41a~94a at one end of the optical fibers 41~94 is described. However, when the imaging optical system 32 is a structure that does not perform equal-magnification projection, the shape and configuration relationship of the light beam spot only need to satisfy the configuration relationship of the light beam spot on the substrate described in (1)~(5) above.
[0112] In addition, in the present invention, the original arrangement relationship of the beam spots is not limited to Figure 2 and Figure 4 The configuration shown can also be Fig.11 In this modification, the core 44a and the core 64a, which are separated and arranged in the X direction with the core 54a interposed therebetween, are arranged at the same position in the Y direction.
[0113] In this modification, when viewed from the scanning direction, the beam spots (in the X direction) are arranged in parallel in the direction orthogonal to the scanning direction. Fig.11 Fiber cores 44a, 54a, 64a) are shown adjacent to each other.
[0114] Furthermore, when viewed from a direction (X direction) perpendicular to the scanning direction (Y direction), the beam spots adjacent to each other along the direction (X) perpendicular to the scanning direction (Y) are mutually spaced (in Fig.11 In the figure, the core 44a and the core 54a, and the core 54a and the core 64a) are arranged to be separated from each other by a predetermined distance (Dy).
[0115] This distance (Dy) is longer than a distance corresponding to a scanning time required for the temperature of the film to be processed 13 heated by the irradiation of the laser beam LB to drop to a temperature equal to or lower than the crystallization temperature of silicon.
[0116] In the above-mentioned embodiment, the shapes of all the beam emitting parts (cores) are set to be the same, but as long as the above-mentioned arrangement relationship of the beam spots on the substrate is satisfied, the lengths (L) of the long sides may be set to be different from each other.
[0117] In the above-mentioned embodiment, at least one end of the core of each of the optical fibers 41 to 44, 51 to 54, 61 to 64, 71 to 74, 81 to 84, and 91 to 94 is set to a rectangular prism shape, and one end face thereof is set as a beam emitting portion, but the structure of the beam emitting portion is not limited thereto. For example, laser beams may be generated from a plurality of semiconductor lasers LD, and the laser beams LB may be formed into a rectangular beam spot using a focusing lens and a biconvex lens, and the amorphous silicon film may be directly irradiated and scanned without passing through an optical fiber. This case is also the same as the above-mentioned embodiment, and the configuration conditions of the plurality of beam spots may be set.
[0118] In the above embodiment, a plurality of light sources are used, but it is also possible to use a single or a plurality of light sources to generate a wide laser beam LB, and use a MEMS (Micro Electro Mechanical Systems) or a mask array as a reflection device having a plurality of reflectors to decompose the wide laser beam LB into a plurality of laser beams LB, so as to control the shape and configuration of the plurality of beam spots to the configuration conditions of the present invention. In addition, the present invention can also be implemented by applying a scheme of dividing a single mother beam into sub-beams via a diffraction grating, a projection lens, etc.
[0119] Description of Reference Numerals
[0120] LB laser beam
[0121] LD semiconductor laser (light source)
[0122] 1 Laser annealing device
[0123] 2 Light source unit
[0124] 3 Optical head
[0125] 10. Processed substrate
[0126] 11 Glass Substrate
[0127] 13 Treated film
[0128] 13a Amorphous silicon
[0129] 13m Molten Silicon
[0130] 13p type monocrystalline silicon
[0131] 20 Stage
[0132] 21 Coupling lens
[0133] 31 Fiber Array
[0134] 32 Imaging Optical System
[0135] 40, 50, 60, 70, 80, 90 support blocks
[0136] 41~44 optical fibers
[0137] 41a~44a core
[0138] 41b~44b cladding
Claims
1. A laser annealing device comprising a plurality of beam emitting units for emitting laser beams, wherein the laser beams are composed of continuous oscillation lasers and have square beam spots with respect to an irradiated surface, The laser annealing device scans the laser beam relative to the amorphous silicon film formed on the substrate along a scanning direction to crystallize a band-shaped modification-planned region of the amorphous silicon film. The laser annealing device is characterized in that: One side of the beam spot is parallel to a direction orthogonal to the scanning direction, The length of the side of the beam spot is set to be shorter than the length at which the substrate is damaged due to internal stress, wherein The internal stress is stress inherent to the substrate that is generated due to heating caused by irradiation with the laser beam.
2. The laser annealing device according to claim 1, wherein: On the surface of the amorphous silicon film, with respect to the beam spot of the laser beam emitted from each of the beam emitting portions, Within the substrate surface of the substrate, when observed from a direction orthogonal to the scanning direction, the beam spots adjacent to each other along the direction orthogonal to the scanning direction are arranged to be spaced apart from each other along the scanning direction by a distance longer than a distance corresponding to the following scanning time, wherein the scanning time is the time for the temperature of the modified predetermined area heated by the irradiation of the laser beam to drop below the crystallization temperature of silicon.
3. The laser annealing device according to claim 2, wherein: The distance equivalent to the scanning time required for the temperature of the modified predetermined area heated by the irradiation of the laser beam to drop below the crystallization temperature of silicon is calculated based on the thickness of the substrate, the thickness of the amorphous silicon film, the thermal diffusion capacity of the amorphous silicon film and the material film beneath it, the irradiation amount of the laser beam, and the relative scanning speed of the laser beam.
4. The laser annealing device according to any one of claims 1 to 3, wherein: The plurality of laser beams are capable of being selectively illuminated.
5. According to claims 1 to 3 4. The laser annealing device according to any one of the preceding claims, wherein: The intensity of the laser beam emitted from the beam emitting portion can be modulated.
6. According to claims 1 to 3 5. The laser annealing device according to any one of claims 5, wherein: The beam emitting portion is one end of an optical fiber, and the other end of the optical fiber is connected to a light source that emits a continuous oscillation laser. The shape of the beam spot is set by the shape of the end face of the beam emitting portion.
7. A laser annealing device comprising a plurality of beam emitting units for emitting laser beams, wherein the laser beams are composed of continuous oscillation lasers and have square beam spots with respect to an irradiated surface, The laser annealing device scans the laser beam relative to the amorphous silicon film formed on the substrate along a scanning direction to crystallize a band-shaped modification-planned region of the amorphous silicon film. The laser annealing device is characterized in that: One side of the beam spot is parallel to a direction orthogonal to the scanning direction, When viewed from the scanning direction, the beam spots of the laser beams emitted from the plurality of beam emitting portions are continuously arranged over the entire width of the region to be modified, In the substrate surface of the substrate, the beam spots adjacent to each other in a direction perpendicular to the scanning direction are spaced apart along the scanning direction when viewed from the direction perpendicular to the scanning direction.
8. The laser annealing device according to claim 7, wherein: The length of the side of the beam spot is set to be shorter than a length at which the substrate is damaged due to internal stress, wherein the internal stress is a stress inherent to the substrate that is generated due to heating caused by irradiation with the laser beam, The beam spots adjacent to each other along the direction orthogonal to the scanning direction are arranged relative to each other at a distance along the scanning direction that is longer than a distance corresponding to the following scanning time, wherein the scanning time is the time for the temperature of the modified predetermined area heated by the irradiation of the laser beam to drop below the crystallization temperature of silicon.
9. The laser annealing device according to claim 8, wherein: The distance equivalent to the scanning time required for the temperature of the modified predetermined area heated by the irradiation of the laser beam to drop below the crystallization temperature of silicon is calculated based on the thickness of the substrate, the thickness of the amorphous silicon film, the thermal diffusion capacity of the amorphous silicon film and the material film beneath it, the irradiation amount of the laser beam, and the relative scanning speed of the laser beam.
10. The laser annealing device according to any one of claims 7 to 9, wherein: The plurality of laser beams are capable of being selectively illuminated.
11. According to claims 7 to 9 10. The laser annealing device according to any one of claims 10, wherein: The intensity of the laser beam emitted from the beam emitting portion can be modulated.
12. According to claims 7 to 9 11. The laser annealing device according to any one of claims 11, wherein: The beam emitting portion is one end of an optical fiber, and the other end of the optical fiber is connected to a light source that emits a continuous oscillation laser. The shape of the beam spot is set by the shape of the end face of the beam emitting portion.
13. A laser annealing method, wherein a plurality of laser beams consisting of continuous oscillation laser light and having square beam spots relative to an irradiated surface of an amorphous silicon film formed on a substrate are irradiated from a plurality of beam emitting portions, and in this state, the plurality of laser beams are scanned relative to the substrate along a scanning direction to crystallize a band-shaped modification target region of the amorphous silicon film, characterized in that: The laser annealing method comprises the following steps: Conducting a preliminary test on the substrate to adjust and set the distances between the plurality of beam emitting portions so that the distances between the beam spots are such that thermal stress cracking due to laser heating does not occur; as well as Then, the plurality of laser beams are scanned relative to the substrate to perform laser annealing.
14. The laser annealing method according to claim 13, wherein: The preliminary test is performed by performing a thermal stress test using the test substrate.
15. The laser annealing method according to claim 13, wherein: The preliminary test was simulated.