Chamfering processing technology for improving roughness of chamfered surface of silicon wafer
By adjusting the feed amount and grinding wheel rotation speed in the chamfering process, combined with cooling water spraying and robot operation, the problem of silicon wafer chamfer surface roughness is solved, achieving lower chamfer surface roughness and efficient processing effect.
Patent Information
- Application Number
- CN202411006665.3
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Filing Date
- 2024-07-25
- Publication Date
- 2024-10-08
- Estimated Expiration
- Not applicable · inactive patent
AI Technical Summary
The existing technology is difficult to effectively improve the chamfer surface roughness in silicon wafer chamfering processing, resulting in increased costs and low processing efficiency.
By adjusting the feed amount in the chamfering process and the rotation speed of the grinding wheel, the silicon wafer rotation speed is controlled to optimize the amount of silicon powder grinded by the grinding wheel. Different feed amounts and rotation speeds of the rough grinding wheel and fine grinding wheel are used, combined with cooling water. Spraying and robot operation ensure the stability of the grinding table and grinding wheel, and achieve rounded trimming of the silicon wafer edge.
The damage to the wafer edge caused by the grinding wheel is reduced, and better chamfer surface roughness is achieved, specifically as a roughness of 5-10um, which improves processing efficiency and cost-effectiveness.
Smart Images

Figure CN118744372A_ABST
Abstract
Description
Technical Field
[0001] The invention relates to the technical field of wafer processing, and in particular to a chamfering process for improving the roughness of a chamfered surface of a silicon wafer. Background Art
[0002] In the wafer processing industry, wafer chamfering is an indispensable link. The main purpose of wafer chamfering is to use a high-speed grinding wheel to grind and trim the edge of the silicon wafer into a specific shape to eliminate the edge cutting stress caused by slicing, prevent edge cracking caused by subsequent processing, make the wafer edge round, and reduce other defects caused by the edge of the silicon wafer surface during silicon wafer epitaxy. With the improvement of the current domestic semiconductor processing level, the wafer size utilization is more perfect, and the influence of the chamfer area on the edge is gradually revealed. Therefore, solving the problem of rough chamfered surface is an important part of the progress of the semiconductor industry.
[0003] At present, domestic semiconductor wafer manufacturers generally use Tokyo Precision's equipment for wafer chamfering, and use grinding wheels to trim the chamfered edges of wafers. With the development of semiconductors, the requirements for chamfered surfaces are getting higher and higher, and the roughness of chamfered surfaces has become more and more concerned by clients. Edge polishing can obtain a relatively intact chamfered surface, but it greatly increases the cost. Therefore, improving the roughness of the chamfered surface on the original basis has become a difficult problem for many semiconductor wafer manufacturers. Summary of the invention
[0004] In view of the defects in the prior art, an object of the present invention is to provide a chamfering process for improving the roughness of the chamfered surface of a silicon wafer.
[0005] The chamfering process for improving the roughness of the chamfered surface of a silicon wafer provided by the present invention comprises the following steps:
[0006] Rough chamfering process steps: fix the silicon wafer on the chamfering grinding table, and the grinding table drives the silicon wafer close to the rough grinding wheel groove for rough chamfering. The feed rate of the rough grinding wheel is 100-1000mm / r;
[0007] Fine chamfering process steps: After the rough chamfering process is completed, the grinding table moves to align with the groove of the fine grinding wheel for fine chamfering. The feed rate of the fine grinding wheel is 50-150um / r, and the silicon wafer speed is 4-20mm / s;
[0008] During the rough chamfering and fine chamfering processes, the grinding wheel speed is 3000-6000r / min.
[0009] Preferably, the method further comprises a preparatory step, which is performed before the rough chamfering step and specifically comprises the following steps:
[0010] Step 1: Load the silicon wafer to be chamfered into a wafer box, and place the wafer box on the loading area of the chamfering machine;
[0011] Step 2: The robot takes the silicon wafer from the wafer box and places it on the machine orientation calibration table;
[0012] Step 3: The orientation calibration table rotates and calibrates the silicon wafer to the corresponding position;
[0013] Step 4: The robot picks up the calibrated silicon wafer from the orientation calibration table and places it on the grinding table.
[0014] Preferably, a cleaning step is further included, and the cleaning step is performed after the fine chamfering step, and specifically includes the following steps:
[0015] After the fine chamfering process is completed, the robot picks up the silicon wafer and moves it to the cleaning table, where it is rinsed with pure water and blown dry with air.
[0016] Preferably, it also includes a material unloading step, which is performed after the cleaning step and specifically includes the following steps:
[0017] After cleaning, the robot picks up the silicon wafer and moves it to the unloading area of the chamfering machine, and puts the chamfered silicon wafer into the receiving box.
[0018] Preferably, during the rough chamfering process and the fine chamfering process, cooling water is sprayed on the chamfering area and the grinding wheel groove, and the water flow rate is 2-4 L / min.
[0019] Preferably, in the rough chamfering step, the mesh number of the rough grinding wheel is 800 meshes.
[0020] Preferably, in the fine chamfering step, the mesh number of the fine grinding wheel is 3000 mesh.
[0021] Preferably, during the rough chamfering and fine chamfering processes, the vibration of each operating axis of the chamfering grinding table is less than 5um, the vibration of the grinding table surface is less than 10um, the vibration of the grinding wheel axis is less than 5um, and the vibration of the grinding wheel surface is less than 10um.
[0022] Preferably, the silicon wafer rotation speed is designed according to the amount of silicon powder removed during the fine chamfering process.
[0023] Compared with the prior art, the present invention has the following beneficial effects:
[0024] The present invention improves the chamfering processing technology by adjusting the coordination optimization of the chamfering feed amount and the grinding wheel rotation speed in the processing technology, and controls the amount of silicon powder ground by the grinding wheel per unit time by controlling the silicon wafer rotation speed, thereby reducing the damage of the grinding wheel to the wafer edge during the chamfering process, and obtaining a better wafer chamfered surface. BRIEF DESCRIPTION OF THE DRAWINGS
[0025] Other features, objects and advantages of the present invention will become more apparent from the detailed description of non-limiting embodiments made with reference to the following drawings:
[0026] Figure 1 It is a schematic diagram of the process flow of the present invention;
[0027] Figure 2 This is a real picture of the chamfered silicon wafer obtained in Example 1 of the present invention;
[0028] Figure 3 This is a real picture of the chamfered plane of the silicon wafer obtained in the comparative example of the present invention. DETAILED DESCRIPTION
[0029] The present invention is described in detail below in conjunction with specific embodiments. The following embodiments will help those skilled in the art to further understand the present invention, but are not intended to limit the present invention in any form. It should be noted that, for those of ordinary skill in the art, several changes and improvements can also be made without departing from the concept of the present invention. These all belong to the protection scope of the present invention.
[0030] The present invention discloses a chamfering process for improving the roughness of the chamfered surface of a silicon wafer, with the focus on improving the chamfering process, by adjusting the coordination optimization of the chamfering feed amount and the grinding wheel rotation speed in the processing process, by controlling the amount of silicon powder ground by the grinding wheel per unit time, and reducing the damage of the grinding wheel to the wafer edge during the chamfering process, thereby achieving a better wafer chamfered surface.
[0031] The chamfering process for improving the roughness of the chamfered surface of a silicon wafer provided by the present invention specifically comprises the following steps:
[0032] Step 1: Load the wafer to be chamfered into a specific wafer box and place it in the loading area of the chamfering machine.
[0033] Step 2: The robot takes the silicon wafer from the wafer box and places it on the machine orientation calibration table.
[0034] Step 3: The orientation calibration stage rotates and calibrates the silicon wafer to the corresponding position.
[0035] Step 4: The robot picks up the calibrated silicon wafer from the calibration table and places it on the grinding table.
[0036] Step 5: Turn on the vacuum on the grinding table to fix the silicon wafer on the grinding table. The grinding table drives the silicon wafer to slowly approach the high-speed rotating grinding wheel to roughly grind the groove (set the wafer target diameter according to the required feed amount).
[0037] Step 6: The machine starts rough chamfering according to the set parameters (the grinding table drives the silicon wafer to rotate, and uses the high-speed grinding wheel to round the edge of the silicon wafer).
[0038] Step 7: After the rough chamfering process is completed, the grinding table moves to align with the fine grinding groove of the grinding wheel, and the machine starts the fine chamfering process according to the set parameters;
[0039] Step 8: After the fine chamfering process is completed, the vacuum on the grinding table is released, and the robot picks up the silicon wafer and moves it to the cleaning table, where it is rinsed with pure water and blown dry with air.
[0040] Step 9: After cleaning, the robot picks up the silicon wafer and moves it to the unloading area of the chamfering machine, and puts the chamfered silicon wafer into the receiving box.
[0041] Preferably, during the fine chamfering process, the chamfering speed is controlled. If the chamfering process is too fast, the damage to the silicon wafer will increase. If it is too slow, not only the efficiency will be delayed, but also chamfer lines will exist. The silicon wafer rotation speed during the chamfering process is optimized to 4-20mm / s, and the chamfering speed is designed according to the amount of silicon powder removed during the chamfering process.
[0042] During the chamfering process, the machine processing accuracy is controlled, the vibration of each running axis of the chamfering grinding table is less than 5um, the vibration of the grinding table surface is less than 10um, the vibration of the grinding wheel axis is less than 5um, and the vibration of the grinding wheel surface is less than 10um.
[0043] The chamfering grinding wheel is designed as follows: the rough grinding wheel is 800 mesh, the fine grinding wheel is 3000 mesh, the grinding wheel speed is 3000-6000r / min, the feed amount of the rough grinding wheel is 100-1000mm each time, and the feed amount of the fine grinding wheel is 50-150um each time.
[0044] Cooling water is sprayed during the rough chamfering and fine chamfering processes. The cooling water is divided into chamfering cooling water and grinding wheel groove flushing cooling water. The water flow rate is 2-4L / min.
[0045] Example 1
[0046] This embodiment provides a specific parameter selection in a chamfering process for improving the roughness of the chamfered surface of a silicon wafer. Specifically, through experiments, it is found that the amount of silicon powder removed during the lapping process is about 2.5 mm 3 / s, it is possible to ensure that a good wafer chamfer surface is obtained. In this embodiment, the two parameters of grinding wheel feed rate and silicon wafer rotation speed are carefully managed to make the amount of silicon powder removed as close to 2.5mm as possible. 3 / s, thereby obtaining a chamfered surface with lower roughness.
[0047] The specific parameter selections are shown in the following table:
[0048] Feed rate Wafer diameter Chamfer Type Wafer thickness Wafer speed priority 80um / r 6mm RHK(0.21) 640mm 5-13mm / s 9mm / s 80um / r 6mm RHK(0.23) 640mm 7-15mm / s 11mm / s 80um / r 6mm RHK(0.26) 640mm 10-18mm / s 14mm / s 150um / r 6mm RHK(0.21) 640mm 4-12mm / s 8mm / s 150um / r 6mm RHK(0.23) 640mm 5-13mm / s 9mm / s 150um / r 6mm RHK(0.26) 640mm 7-15mm / s 11mm / s 80um / r 6mm RGK(0.21) 640mm 7-15mm / s 11mm / s 80um / r 6mm RGK(0.23) 640mm 9-17mm / s 13mm / s 80um / r 6mm RGK(0.26) 640mm 11-19mm / s 15mm / s 150um / r 6mm RGK(0.21) 640mm 5-13mm / s 9mm / s 150um / r 6mm RGK(0.23) 640mm 6-14mm / s 10mm / s 150um / r 6mm RGK(0.26) 640mm 8-16mm / s 12mm / s
[0049] Table 1: Parameter selection table
[0050] Table 1 discloses the processing technology for different chamfer types. In the chamfer type, R indicates that the chamfer is an R-type chamfer, H indicates that the bevel angle of the chamfer is 11°, G indicates that the bevel angle of the chamfer is 22°, K indicates that the particle size of the lapping wheel is greater than 1500 mesh, and the number in the brackets indicates the front end circle radius of the chamfer, in mm.
[0051] By selecting the above parameter range, a chamfered surface with a roughness Ra of 5-10um can be obtained. By using the silicon wafer rotation speed in the "priority" column, a faster processing speed can be achieved while ensuring a better chamfered surface, and the overall performance is the best. The effect of the scheme of this embodiment is further reflected by setting a comparative example. Specifically, for different chamfering types, if a silicon wafer rotation speed greater than 20mm / s is selected, the roughness range of the chamfered surface is 15-25um. If a silicon wafer rotation speed less than 4mm / s is selected, the production capacity is delayed due to the slow rotation speed, resulting in low efficiency, and accompanied by other defects such as chamfer lines.
[0052] Therefore, from the above comparison, it can be seen that a better chamfered surface can be obtained when the silicon wafer rotation speed is limited to 4-20 mm / s.
[0053] In the description of the present application, it should be understood that the terms "up", "down", "front", "back", "left", "right", "vertical", "horizontal", "top", "bottom", "inside", "outside", etc., indicating orientations or positional relationships, are based on the orientations or positional relationships shown in the accompanying drawings, and are only for the convenience of describing the present application and simplifying the description, and do not indicate or imply that the referred device or element must have a specific orientation, be constructed and operated in a specific orientation, and therefore should not be understood as a limitation on the present application.
[0054] The above describes the specific embodiments of the present invention. It should be understood that the present invention is not limited to the above specific embodiments, and those skilled in the art can make various changes or modifications within the scope of the claims, which does not affect the essence of the present invention. In the absence of conflict, the embodiments of the present application and the features in the embodiments can be combined with each other arbitrarily.
Claims
1. A chamfering process for improving the roughness of the chamfered surface of a silicon wafer. It is characterized in that The steps include: Rough chamfering process steps: fix the silicon wafer on the chamfering grinding table, and the grinding table drives the silicon wafer close to the rough grinding wheel groove for rough chamfering. The feed rate of the rough grinding wheel is 100-1000mm / r; Fine chamfering process steps: After the rough chamfering process is completed, the grinding table moves to align with the groove of the fine grinding wheel for fine chamfering. The feed rate of the fine grinding wheel is 50-150um / r, and the silicon wafer speed is 4-20mm / s; During the rough chamfering and fine chamfering processes, the grinding wheel speed is 3000-6000r / min.
2. The chamfering process for improving the roughness of the chamfered surface of a silicon wafer according to claim 1, It is characterized in that The method further includes a preparatory step, which is performed before the rough chamfering step and specifically includes the following steps: Step 1: Load the silicon wafer to be chamfered into a wafer box, and place the wafer box on the loading area of the chamfering machine; Step 2: The robot takes the silicon wafer from the wafer box and places it on the machine orientation calibration table; Step 3: The orientation calibration table rotates and calibrates the silicon wafer to the corresponding position; Step 4: The robot picks up the calibrated silicon wafer from the orientation calibration table and places it on the grinding table.
3. The chamfering process for improving the roughness of the chamfered surface of a silicon wafer according to claim 1, It is characterized in that The cleaning step is performed after the fine chamfering step and specifically includes the following steps: After the fine chamfering process is completed, the robot picks up the silicon wafer and moves it to the cleaning table, where it is rinsed with pure water and blown dry with air.
4. The chamfering process for improving the roughness of the chamfered surface of a silicon wafer according to claim 3, It is characterized in that The step of unloading is also included, and the step of unloading is performed after the step of cleaning, and specifically includes the following steps: After cleaning, the robot picks up the silicon wafer and moves it to the unloading area of the chamfering machine, and puts the chamfered silicon wafer into the receiving box.
5. The chamfering process for improving the roughness of the chamfered surface of a silicon wafer according to claim 1, It is characterized in that During the rough chamfering and fine chamfering processes, cooling water is sprayed on the chamfering area and the grinding wheel groove, with a water flow rate of 2-4L / min.
6. The chamfering process for improving the roughness of the chamfered surface of a silicon wafer according to claim 1, It is characterized in that In the rough chamfering process, the rough grinding wheel has a mesh size of 800.
7. The chamfering process for improving the roughness of the chamfered surface of a silicon wafer according to claim 1, It is characterized in that In the fine chamfering process, the mesh number of the fine grinding wheel is 3000 mesh.
8. The chamfering process for improving the roughness of the chamfered surface of a silicon wafer according to claim 1, It is characterized in that During the rough chamfering and fine chamfering processes, the vibration of each operating axis of the chamfering grinding table is less than 5um, the vibration of the grinding table surface is less than 10um, the vibration of the grinding wheel axis is less than 5um, and the vibration of the grinding wheel surface is less than 10um.
9. The chamfering process for improving the roughness of the chamfered surface of a silicon wafer according to claim 1, It is characterized in that The silicon wafer rotation speed is designed according to the amount of silicon powder removed during the fine chamfering process.
Citation Information
Cited By
Wafer edge chamfer cutting and cleaning method and cutting and cleaning device
CN119601462A
Wafer edge chamfer cutting and cleaning method and cutting and cleaning device
CN119601462B
Silicon wafer containing low-roughness chamfer and processing method thereof
CN121340039A